A sodium-ion battery
By introducing cyclic sulfonyl compounds and sodium fluorosulfinate compounds into the electrolyte of sodium-ion batteries, a uniform and dense SEI film is formed, which solves the problems of slow charge transfer rate at low temperatures and unstable performance at high temperatures in sodium-ion batteries, and improves high-temperature storage and cycle performance.
Patent Information
- Application Number
- CN202510498052.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-21
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-04-21
AI Technical Summary
Sodium-ion batteries exhibit poor electrochemical performance at low temperatures, particularly due to difficulties in cation desolvation at the electrode-electrolyte interface, leading to slow charge transfer rates, Na+ accumulation, and sodium precipitation. Furthermore, their performance is unstable during high-temperature storage and cycling.
Compounds A and B are introduced into the electrolyte of a sodium-ion battery. Compound A contains a cyclic sulfonyl compound, and compound B is a sodium fluorosulfinate compound. They work synergistically to form a uniform and dense SEI film on the electrode surface, improving the battery's high-temperature storage and cycle performance, and suppressing low-temperature sodium precipitation.
Stable storage and cycle performance of sodium-ion batteries at high temperatures were achieved, while sodium ion precipitation was effectively suppressed at low temperatures, thus improving the overall electrochemical performance of the battery.
Smart Images

Figure CN120357013B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of secondary battery technology, and particularly relates to a sodium-ion battery. Background Technology
[0002] Due to the abundance of sodium resources, rechargeable sodium-ion batteries (SIBs) have long been considered ideal candidate materials for large-scale energy storage systems. Although sodium-ion batteries have significant theoretical advantages, their electrochemical performance at low temperatures has been unsatisfactory, especially when the temperature drops below -0°C. This is mainly due to the low ion transport efficiency in the electrolyte, the difficulty of cation desolvation at the electrode-electrolyte interface, and the kinetic barriers to electron and ion transport within the electrode materials.
[0003] One of the biggest challenges faced by sodium-ion batteries under low-temperature conditions is the interfacial Na+ interface. + The desolvation process becomes particularly slow and a key factor limiting the charge transfer rate, which not only increases the dominant charge transfer impedance but also leads to Na... + Accumulation near the SEI layer leads to the deposition of sodium metal. Furthermore, an ideal SEI film formed by additives in the electrolyte should be electronically insulating and ionicly conductive, and should be insoluble and inert relative to the electrolyte to avoid irreversible capacity loss due to side reactions. Compared to lithium-ion batteries, the solubility of alkyl sodium and alkyl carbonate in carbonates in the Na-SEI film of sodium-ion batteries is 70-80 times higher than that of inorganic components such as NaF and Na₂CO₃. Moreover, the solubility of inorganic components NaF and Na₂CO₃ in Na-SEI is 30-40 times higher than that of inorganic components LiF and Li₂CO₃ in Li-SEI. This means that the Na-SEI film is more easily corroded by the electrolyte, leading to increased instability of the Na-SEI, further exacerbating side reactions with the electrolyte, and ultimately affecting the high-temperature storage and cycle performance of sodium-ion batteries.
[0004] Therefore, there is an urgent need for a sodium-ion battery to address the shortcomings of existing technologies. Summary of the Invention
[0005] In view of the above problems, the purpose of this invention is to provide a sodium-ion battery that has good high-temperature storage performance, high-temperature cycle performance and low-temperature performance.
[0006] To achieve the above objectives, the present invention provides a sodium-ion battery, comprising a positive electrode, a negative electrode, and an electrolyte. The electrolyte comprises a non-aqueous organic solvent, a sodium salt, and an additive. The additive comprises compound A and compound B. The structure of compound A is shown in Formula 1, and the structure of compound B is shown in Formula 2.
[0007] Among them, one of X, Y, and Z is a sulfonyl group, and the other two of X, Y, and Z are each independently selected from sulfonyl or carbonyl groups, and the other two of X, Y, and Z are not simultaneously sulfonyl groups; R is a fluorinated alkane containing 1 to 6 carbon atoms.
[0008] Compared with existing technologies, this invention introduces compound A into the electrolyte of a sodium-ion battery. Compound A contains a cyclic sulfonyl compound, which helps to form compounds such as Na₂S and Na₂SO₃ with good thermodynamic stability at the electrode interface, thereby suppressing the reaction between the electrode material and the electrolyte and significantly improving the high-temperature storage and high-temperature cycling performance of the sodium-ion battery. Furthermore, although the cyclic sulfonyl compound in compound A can reduce the electron cloud density of C=O in the carbonate solvent through its strong electronegativity, thus weakening the Na₂S / Na₂SO₃ reaction... + The binding strength with solvent molecules and promotes Na + The desolvation process occurs, but compound A has poor wettability on the hard carbon anode surface, resulting in uneven distribution on the electrode surface. This uneven distribution leads to inconsistent SEI film thickness, with some areas rich in insulating components and insufficient in conductive components, causing increased interfacial impedance. Under high impedance conditions, Na... + The migration rate decreases significantly, leading to charge accumulation at the interface and ultimately causing sodium deposition. Based on this, this application also introduces compound B, a sodium fluorosulfinate compound. Compound B, due to the high electronegativity and electron-withdrawing properties of its fluorine atoms, exhibits high solubility and dissociation in non-aqueous solvents, improving the uniformity of compound A's distribution on the negative electrode surface. Therefore, compounds A and B, through synergistic action, can form a uniform, dense, and thermodynamically stable SEI film on the negative electrode surface. This film also exhibits lower impedance at low temperatures, effectively suppressing further sodium ion deposition and reducing the sodium deposition phenomenon. Therefore, the sodium-ion battery of this invention possesses good high-temperature storage performance, high-temperature cycle performance, and low-temperature performance.
[0009] Furthermore, the fluorinated alkanes containing 1 to 6 carbon atoms in this invention refer to alkane derivatives with a carbon chain length of 1 to 6 carbon atoms and where some or all hydrogen atoms are replaced by fluorine (F). Depending on the degree of fluorination, they can be classified into perfluoroalkanes (all hydrogen atoms are replaced by fluorine) and partially fluorinated alkanes (some hydrogen atoms are replaced by fluorine). Specifically, fluorinated alkanes containing 1 to 6 carbon atoms can be, but are not limited to, tetrafluoromethane (CF4), difluoromethane (CH2F2), octafluoropropane (C3F8), and hexafluoroethane (C2F6).
[0010] Further, the mass percentage of compound A in the electrolyte is 0.1% to 2%. Specifically, the mass percentage of compound A in the electrolyte may be, but is not limited to, 0.1%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, or 2%.
[0011] Furthermore, the mass percentage of compound B in the electrolyte is 0.1% to 1%. Specifically, the mass percentage of compound B in the electrolyte may be, but is not limited to, 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, 0.9%, or 1.0%.
[0012] Furthermore, compound A of the present invention is selected from at least one of compounds A1 to A3: .
[0013] Furthermore, compound B of the present invention is selected from at least one of compound B1, compound B2, and compound B3: .
[0014] Furthermore, the sodium salt of the present invention is selected from NaPF6 (sodium hexafluorophosphate), NaBF4 (sodium tetrafluoroborate), NaClO4 (sodium perchlorate), NaBOB (sodium bis(oxalato)borate), NaODFB (sodium difluorooxalato)borate, NaFAP (sodium tri(pentafluoroethyl)trifluorophosphate), NaAsF6 (sodium hexafluoroarsenate), NaSbF6 (sodium hexafluoroantimonate), NaCF3SO3 (sodium trifluoromethanesulfonate), NaN(SO2CF3)2 (sodium bis(trifluoromethanesulfonyl)imide), N At least one of the following: aN(SO2C2F5)2 (sodium bis(pentafluoroethylsulfonyl)imide), NaN(SO2C4F9)2 (sodium bis(nonafluorobutylsulfonyl)imide), NaC(SO2CF3)3 (sodium tri(trifluoromethylsulfonyl)methyl), NaPF2(C2O4)2 (sodium difluorobis(oxalato)phosphate), NaPF4(C2O4) (sodium tetrafluorooxalato)phosphate, NaB(CF3)4 (sodium tetra(trifluoromethyl)borate), and NaBF3(C2F5) (sodium trifluoroethyltrifluoroborate).
[0015] Furthermore, the concentration of the sodium salt in the electrolyte of the present invention is 0.5~2.5 mol / L. Specifically, the concentration of the sodium salt in the electrolyte may be, but is not limited to, 0.5 mol / L, 0.8 mol / L, 1.2 mol / L, 1.6 mol / L, 1.9 mol / L, 2.2 mol / L, and 2.5 mol / L.
[0016] Furthermore, the non-aqueous organic solvent of the present invention is selected from carbonate compounds and / or carboxylic acid ester compounds.
[0017] Further, the non-aqueous organic solvent of the present invention is selected from at least one of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), γ-butyrolactone (GBL), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), butyl acetate (BA), ethyl propionate (EP), propyl propionate (PP) and butyl propionate (BP).
[0018] Further, the positive electrode active material of the present invention is a layered oxide, and the chemical formula of the layered oxide is Na x M 1-y-z Fe y Mn z O2, wherein M includes at least one of Co, Ni, Cu, Mg, Zn, Al, Sn, Ga, Cr, Sr, V and Ti, 0<x≤1, 0≤y<1, 0≤z<1, y+z≤1. Certainly, the positive electrode active material may also be other materials capable of realizing ion deintercalation with sodium ions.
[0019] Further, the negative electrode active material of the present invention includes a hard carbon material. DETAILED DESCRIPTION
[0020] To better illustrate the purpose, technical solutions and beneficial effects of the present invention, the present invention will be further described below with reference to specific examples. It should be noted that the methods described in the following examples are further illustrative of the present invention and should not be construed as limiting the present invention.
[0021] Example 1 (1) Preparation of electrolyte: The electrolyte is prepared in a vacuum glove box with a water content of <1 ppm under an argon atmosphere. In the glove box under a dry argon atmosphere, propylene carbonate (PC), diethyl carbonate (DEC), propyl acetate (PA) and butyl acetate (BA) are mixed at a weight ratio of PC:DEC:PA:BA=5:4:2:1, then an additive is added. After dissolution and thorough stirring, the electrolyte salt NaPF6 is added, and the mixture is uniformly mixed to obtain the electrolyte.
[0022] (2) Preparation of positive electrode sheet: The positive electrode active material NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3 O2, the binder PVDF and the conductive agent SuperP are uniformly mixed at a mass ratio of 95:1:4 to prepare a sodium-ion battery positive electrode slurry with a certain viscosity. The prepared slurry is coated on both sides of an aluminum foil, and after drying and rolling, the positive electrode sheet is obtained.
[0023] (3) Preparation of negative electrode sheet: Hard carbon (Kuraray Type 1) is mixed with conductive agent SuperP, thickener CMC and binder SBR (styrene-butadiene rubber emulsion) in a mass ratio of 95:1.5:1.0:2.5 to make a slurry. The mixture is evenly mixed and coated on both sides of copper foil. After drying and rolling, the negative electrode sheet is obtained.
[0024] (4) Preparation of sodium-ion battery: The positive electrode, separator and negative electrode are stacked to form a square cell, which is packaged with polymer, filled with the electrolyte prepared above, and then processed through formation, capacity testing and other processes to produce a sodium-ion battery with a capacity of 1000mAh.
[0025] The electrolyte formulations for Examples 1-8 and Comparative Examples 1-3 are shown in Table 1. The preparation steps for the sodium-ion batteries are the same as those for Example 1.
[0026] Table 1 Electrolyte formulations for the examples and comparative examples
[0027] The sodium-ion batteries prepared in Examples 1-8 and Comparative Examples 1-3 were tested using the following test methods. The test results are shown in Table 2.
[0028] First Coulomb efficiency test: Sodium-ion batteries were placed in a high-temperature, high-pressure formation chamber and formed in three steps at 25°C and 0.28 MPa (4 batteries). The first step involved a constant current of 0.05C for 60 minutes, recording the charging capacity C1. The second step involved a constant current of 0.1C for 120 minutes, recording the charging capacity C2. The third step involved a constant current of 0.2C for 240 minutes, recording the charging capacity C3. The upper limit voltage was 3.9V. The batteries were then resealed using a rotary sealing machine. They were then charged at room temperature at a constant current of 0.5C until the voltage reached 4.25V, followed by constant voltage charging at 4.25V until the current reached 0.05C. Finally, they were discharged at a constant current of 1C until the voltage reached 2.5V. The initial discharge capacity C0 was recorded, and the initial coulombic efficiency was calculated as C0 / (C1+C2+C3)×100%.
[0029] High-temperature cycle performance test of sodium-ion batteries: The sodium-ion battery was placed in a 45°C constant temperature chamber and allowed to stand for 30 minutes to reach a constant temperature. It was then charged at a constant current of 1C until the voltage reached 4.25V, followed by constant voltage charging at 4.25V until the current reached 0.05C. Finally, it was discharged at a constant current of 1C until the voltage reached 2.0V. The first discharge capacity was recorded, constituting one charge-discharge cycle. This cycle was repeated 400 times, recording the discharge capacity of the first and last cycles. The capacity retention rate was calculated using the following formula.
[0030] Capacity retention rate = (Discharge capacity in the last cycle / Discharge capacity in the first cycle) × 100% High-temperature storage performance test of sodium-ion batteries: At room temperature (25℃), the sodium-ion battery was charged and discharged once at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.25V. Then, the battery was charged to 4.25V under constant current and constant voltage conditions at 0.5C, and the battery thickness was measured (the thickness was recorded as D0). The battery was placed in a 60℃ oven for 30 days, and then removed and the battery thickness was measured (the thickness was recorded as D1). The thickness expansion rate was calculated.
[0031] Thickness expansion rate = (D1 / D0) × 100% Low-temperature discharge test: At room temperature (25℃), the sodium-ion battery was charged and discharged once at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.25V. The battery was then placed in a low-temperature chamber at -10℃ and discharged at a constant current of 0.1C until the voltage reached 2.0V. The first discharge capacity of the battery was recorded as C1, which constitutes one charge-discharge cycle. The sodium-ion battery was then charged and discharged once at room temperature (25℃) once more at 0.5C / 0.5C (the battery discharge capacity was recorded as C2). After 10 cycles, the battery was disassembled to observe the sodium deposition on the electrodes.
[0032] Capacity recovery rate = (C2 / C0) × 100% Table 2 Performance test results of sodium-ion batteries in the examples and comparative examples
[0033] As shown in Table 2, compared to Comparative Examples 1-3, the sodium-ion batteries of Examples 1-8 exhibit better high-temperature cycle performance, high-temperature storage performance, and low-temperature discharge performance. This is because the sodium-ion batteries of Examples 1-8 contain compounds A and B. Compound A contains cyclic sulfonyl compounds, which helps to form compounds such as Na2S and Na2SO3 with good thermodynamic stability at the electrode interface, thereby suppressing the reaction between the electrode material and the electrolyte and significantly improving the high-temperature storage and high-temperature cycle performance of the sodium-ion battery. Meanwhile, compound B, due to the high electronegativity and electron-withdrawing properties of its fluorine atoms, has high solubility and dissociation in non-aqueous solvents, improving the uniformity of compound A's distribution on the negative electrode surface. Therefore, compounds A and B, through synergistic effects, can form a uniform, dense, and thermodynamically stable SEI film on the negative electrode surface. This film also has lower impedance at low temperatures, effectively suppressing further sodium ion precipitation and reducing the "sodium precipitation" phenomenon. Therefore, the sodium-ion battery of the present invention has better high-temperature storage performance, high-temperature cycle performance, and low-temperature performance.
[0034] Comparing Example 2 with Comparative Examples 1 and 2, it can be seen that Compound A and Compound B can form a uniform, dense, and thermodynamically stable SEI film on the negative electrode surface through synergistic effect. This film also has lower impedance at low temperatures. In short, removing either Compound A or Compound B cannot guarantee that the sodium-ion battery will have good high-temperature storage performance, high-temperature cycle performance, and low-temperature performance at the same time.
[0035] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A sodium-ion battery, comprising a positive electrode, a negative electrode, and an electrolyte, wherein the electrolyte comprises a non-aqueous organic solvent, a sodium salt, and additives, characterized in that, The additive includes compound A and compound B, wherein the structure of compound A is shown in Formula 1 and the structure of compound B is shown in Formula 2. Among them, one of X, Y, and Z is a sulfonyl group, and the other two of X, Y, and Z are each independently selected from sulfonyl or carbonyl groups, and the other two of X, Y, and Z are not simultaneously sulfonyl groups; R is a fluorinated alkane containing 1 to 6 carbon atoms.
2. The sodium-ion battery as described in claim 1, characterized in that, The mass percentage of compound A in the electrolyte is 0.1% to 2%.
3. The sodium-ion battery as described in claim 1, characterized in that, The mass percentage of compound B in the electrolyte is 0.1% to 1%.
4. The sodium-ion battery as described in claim 1, characterized in that, Compound A is selected from at least one of compounds A1 to A3:
5. The sodium-ion battery as described in claim 1, characterized in that, The compound B is selected from at least one of compounds B1, B2, and B3:
6. The sodium-ion battery as described in claim 1, characterized in that, The sodium salt is selected from at least one of NaPF6, NaBF4, NaClO4, NaBOB, NaODFB, NaFAP, NaAsF6, NaSbF6, NaCF3SO3, NaN(SO2CF3)2, NaN(SO2C2F5)2, NaN(SO2C4F9)2, NaC(SO2CF3)3, NaPF2(C2O4)2, NaPF4(C2O4), NaB(CF3)4, and NaBF3(C2F5).
7. The sodium-ion battery as described in claim 1, characterized in that, The concentration of the sodium salt in the electrolyte is 0.5–2.5 mol / L.
8. The sodium-ion battery as described in claim 1, characterized in that, The non-aqueous organic solvent is selected from carbonate compounds and / or carboxylic acid ester compounds.
9. The sodium-ion battery as described in claim 8, characterized in that, The non-aqueous organic solvent is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate, and butyl propionate.
10. The sodium-ion battery as described in claim 1, characterized in that, The active material of the negative electrode includes hard carbon material, and the active material of the positive electrode is a layered oxide with the chemical formula Na. x M 1-y-z Fe y Mn z O2, wherein M includes at least one of Co, Ni, Cu, Mg, Zn, Al, Sn, Ga, Cr, Sr, V, and Ti, 0 <x≤1,0≤y<1,0≤z<1,y+z≤1。
Citation Information
Patent Citations
Sodium ion battery
CN114447333A
Cation conductive membranes comprising polysulfonic acid polymers and metal salts having an f-containing anion
US20110303868A1