Electrolyte for aqueous zinc ion battery as well as preparation method and application of electrolyte
By using the synergistic effect of tetrafluoroborate and zwitterionic additives in aqueous zinc-ion batteries, the problems of electrolyte freezing and interface pH fluctuation in low-temperature environments were solved, and the low-temperature cycling performance and electrochemical performance of zinc-ion batteries were improved.
Patent Information
- Application Number
- CN202510598060.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2025-09-12
AI Technical Summary
The viscosity of the electrolyte in aqueous zinc-ion batteries increases and freezes in low-temperature environments, resulting in a decrease in the migration rate of zinc ions and obstruction of electrolyte transmission. At the same time, fluctuations in the pH value at the zinc negative electrode interface lead to corrosion and dendrite formation.
An electrolyte containing tetrafluoroborate and zwitterionic additives is used. Tetrafluoroborate reduces the freezing point of the electrolyte, and the zwitterionic additive buffers the interface pH value, destroys the hydrogen bond network through O—H…F bonds, and regulates the zinc ion deposition behavior.
Improve the cycle life and electrochemical performance of zinc-ion batteries under low temperature environment, inhibit dendrite formation, and maintain the fluidity and interface stability of the electrolyte.
Smart Images

Figure BDA0005395157120000071 
Figure BDA0005395157120000081
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of zinc ion batteries, and in particular to an electrolyte for aqueous zinc ion batteries, a preparation method thereof, and an application thereof. Background Art
[0002] Aqueous zinc-ion batteries are a new type of electrochemical energy storage device using zinc ions as charge carriers and an aqueous electrolyte as a medium. Their operating principle is based on the reversible intercalation and deintercalation of zinc ions between the positive and negative electrode materials, enabling the storage and release of electrical energy. During discharge, zinc ions are released from the negative electrode, migrate through the electrolyte to the positive electrode, and then intercalate into the positive electrode material. During charging, the reverse occurs, with zinc ions returning to the negative electrode from the positive electrode.
[0003] Aqueous zinc-ion batteries offer numerous advantages, including high safety, low cost, and environmental friendliness. Their positive electrode materials typically include manganese oxides and Prussian blue analogs, which efficiently absorb and release zinc ions. The negative electrode is often made of metallic zinc or its alloys. The deposition and dissolution of zinc ions directly impact the battery's performance and lifespan. Furthermore, the composition and concentration of the electrolyte also significantly influence battery performance. For example, aqueous ZnSO₄ electrolytes are widely used due to their high Coulombic efficiency and cycling stability.
[0004] pH fluctuation at the zinc anode interface is a common phenomenon in the operation of zinc ion batteries and is also a serious challenge faced by zinc metal anodes. On the one hand, zinc ions undergo hydrolysis in aqueous solution to generate hydrogen ions H + , resulting in a decrease in local pH. The specific reaction equation is: Zn 2+ +2H2O→Zn(OH)2+2H + , this local acidic environment will further aggravate the corrosion reaction of zinc. On the other hand, during the zinc deposition process, hydrated zinc ions Zn(H2O) n 2+ The desolvation process is incomplete, and the unremoved water molecules will preferentially capture the outer electrons, causing the OH bond to break and generate H2 and OH - , resulting in a local increase in pH. When the pH exceeds 5.47, electrochemically inert Zn4SO4(OH)6 is generated at the interface.
[0005] Another key issue facing zinc-ion batteries is the increased viscosity and freezing of the electrolyte at low temperatures. At low temperatures, the viscosity of aqueous electrolytes increases significantly, which reduces the migration rate of zinc ions. Furthermore, water molecules in the electrolyte are more likely to form ice crystals at low temperatures, causing the electrolyte to freeze, thereby hindering the effective transport of ions. Summary of the Invention
[0006] The technical problem to be solved by the present invention is how to further improve the low-temperature resistance of aqueous zinc ion battery electrolyte.
[0007] The present invention solves the above technical problems through the following technical means:
[0008] An electrolyte for an aqueous zinc ion battery comprises a soluble zinc salt, water, tetrafluoroborate and a zwitterion additive, wherein the mass concentration of the tetrafluoroborate in the electrolyte is 300-800 g / L.
[0009] Preferably, the mass concentration of the zwitterionic additive in the electrolyte is 5-60 g / L.
[0010] Preferably, the mass concentration of the tetrafluoroborate can be 300g / L, 400g / L, 440g / L, 500g / L, 550g / L, 600g / L, 700g / L, 800g / L. If too little tetrafluoroborate is added, the antifreeze effect of the electrolyte is not significant; if too much tetrafluoroborate is added, BF4 - Hydrolysis intensifies and deteriorates the interface microenvironment.
[0011] Preferably, the mass concentration of the zwitterionic additive can be 5 g / L, 10 g / L, 20 g / L, 25 g / L, 30 g / L, 40 g / L, 50 g / L, 55 g / L, or 60 g / L. If too little zwitterionic additive is added, the interfacial pH cannot be effectively maintained; if too much zwitterionic additive is added, an excessively thick interfacial double layer hinders the rapid electroreduction of zinc ions.
[0012] Preferably, the soluble zinc salt includes one or more of zinc sulfate, zinc trifluoromethanesulfonate, and zinc acetate; preferably, the soluble zinc salt is zinc sulfate.
[0013] Preferably, the molar concentration of the soluble zinc salt in the electrolyte is 0.5-5 mol / L.
[0014] Preferably, the molar concentration of the soluble zinc salt can be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 4 mol / L, 4.2 mol / L, or 5 mol / L. Suitable Zn 2+ concentration is beneficial to improving battery performance.
[0015] Preferably, the tetrafluoroborate includes one or more of lithium tetrafluoroborate, sodium tetrafluoroborate, potassium tetrafluoroborate, ammonium tetrafluoroborate, and tetraethylammonium tetrafluoroborate; preferably, the tetrafluoroborate is sodium tetrafluoroborate.
[0016] Preferably, the zwitterionic additive includes one or more of tris(hydroxymethyl)methylglycine, triglycine and N-acetyl-L-proline.
[0017] Preferably, the zwitterionic additive is tris(hydroxymethyl)methylglycine.
[0018] Preferably, the mass concentration of the tetrafluoroborate is 500-700 g / L; and / or the mass concentration of the zwitterionic additive is 25-50 g / L.
[0019] Preferably, the concentration of the tetrafluoroborate is 500 g / L, the concentration of the zwitterionic additive is 25 g / L, and the concentration of the soluble zinc salt is 2 mol / L.
[0020] The present invention also provides a method for preparing the electrolyte for aqueous zinc ion batteries, comprising the following steps: uniformly mixing a soluble zinc salt, tetrafluoroborate, water and a zwitterion additive to obtain the electrolyte for aqueous zinc ion batteries.
[0021] The present invention also proposes an application of the electrolyte for aqueous zinc ion batteries in zinc ion batteries.
[0022] Preferably, the zinc ion battery is an aqueous zinc ion battery.
[0023] The present invention also provides a zinc ion battery containing the electrolyte for aqueous zinc ion batteries.
[0024] Preferably, the zinc ion battery further comprises a positive electrode, a negative electrode and a separator.
[0025] Preferably, the negative electrode is commercial zinc foil or zinc alloy foil.
[0026] Preferably, the negative electrode has a diameter of 16 mm and a thickness of 0.08 mm.
[0027] Preferably, the positive electrode is commercial vanadium pentoxide.
[0028] Preferably, the positive electrode specification is 12 mm in diameter and the surface density of the V2O5 active material is 4-6 mg / cm 2 .
[0029] Preferably, the separator is a glass fiber separator (GF / D).
[0030] Preferably, the housing model used for the zinc ion battery is CR2032.
[0031] The present invention specifically uses tetrafluoroborate and zwitterion additives as electrolyte additives for aqueous zinc ion batteries, thereby improving their electrochemical performance at low temperatures; tetrafluoroborate BF4- The F atoms in BF4 have strong electronegativity, which can attract free H2O in the electrolyte and form O—H…F bonds, which is conducive to breaking the original hydrogen bond network, lowering the freezing point of the electrolyte and preventing the electrolyte from freezing. - It will hydrolyze to produce ZnF2 and form a SEI film on the surface of the negative electrode. The specific reaction equation is: 2BF4 - +2H2O+Zn 2+ →ZnF2+2H + +2BF3(OH) - BF4 - The hydrolysis of BF4 is a spontaneous and uncontrollable process, so the uniformity of the SEI film is poor, especially at the zinc negative electrode interface, where the hydrogen evolution reaction leads to the formation of extremely alkaline micro-regions and a rapid increase in pH, which will promote the formation of BF4 near the region. - The hydrolysis forms ZnF2 insoluble matter covering the negative electrode surface. The surface roughness and increased polarization caused by the byproduct layer will in turn stimulate dendrite growth and hydrogen evolution reaction, forming a vicious cycle inside the battery. To this end, zwitterionic additives are introduced. Zwitterionic additives contain both positively charged amino groups (-NH2) and negatively charged carboxyl groups (-COOH). This structure enables it to buffer the pH of the solution through protonation or deprotonation processes under different pH environments. Specifically, in an acidic environment, the amino group (-NH2) can accept protons (H + ), thus carrying a positive charge and neutralizing acidic substances; in an alkaline environment, the carboxyl group (-COOH) can release protons (H + ), with negative charge, neutralizes alkaline substances. Therefore, the introduction of zwitterionic additives can effectively alleviate the local pH increase caused by hydrogen evolution reaction, which is beneficial to reduce BF4 - The zwitterionic additive reduces the hydrolysis of zinc ions and inhibits the formation of byproducts such as ZnF2, Zn(OH)2, and Zn4SO4(OH)6. Furthermore, the carboxyl groups in the zwitterionic additive chelate with zinc ions, regulating their deposition behavior, promoting uniform zinc deposition, and reducing the formation of zinc dendrites. Therefore, the synergistic effect of the zwitterionic additive and tetrafluoroborate significantly improves the low-temperature cycle life of zinc-ion batteries.
[0032] The present invention addresses the problems of electrolyte freezing and interface pH fluctuation faced by zinc ion batteries in low-temperature environments, and provides an aqueous electrolyte for zinc ion batteries. The aqueous electrolyte for zinc ion batteries is based on the synergistic effect of tetrafluoroborate and a zwitterionic additive. Zinc ion batteries containing the electrolyte additive have good cycle performance in low-temperature environments. The electrolyte additive is inexpensive and has a high cost-effectiveness ratio. The electrolyte preparation operation is simple, and the electrolyte is easy to promote. DETAILED DESCRIPTION
[0033] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts shall fall within the scope of protection of the present invention.
[0034] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0035] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the field or according to the product instructions.
[0036] Example 1
[0037] Preparation of 2mol / L zinc sulfate (ZnSO4) + 500g / L sodium tetrafluoroborate (NaBF4) + 25g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0038] In this embodiment, sodium tetrafluoroborate and tris(hydroxymethyl)methylglycine are used as electrolyte additives to configure an electrolyte and applied to an aqueous zinc ion battery. The raw materials of the electrolyte include zinc sulfate heptahydrate, sodium tetrafluoroborate, tris(hydroxymethyl)methylglycine and deionized water; and the molar concentration of zinc sulfate heptahydrate in the electrolyte is 2mol / L, the mass concentration of sodium tetrafluoroborate is 500g / L, and the mass concentration of tris(hydroxymethyl)methylglycine is 25g / L. The configuration method of the composite electrolyte is as follows: under an air atmosphere, 57.512g zinc sulfate heptahydrate, 50g sodium tetrafluoroborate, and 2.5g tris(hydroxymethyl)methylglycine are weighed, and deionized water is used as a solvent. Zinc sulfate heptahydrate, sodium tetrafluoroborate, and tris(hydroxymethyl)methylglycine are stirred until completely dissolved, and then the volume is adjusted to 100mL using a volumetric flask to obtain the electrolyte described in Example 1.
[0039] Example 2
[0040] Preparation of 2mol / L zinc sulfate (ZnSO4) + 800g / L sodium tetrafluoroborate (NaBF4) + 25g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0041] Except for using 80 g of sodium tetrafluoroborate as the raw material and adjusting the concentration of sodium tetrafluoroborate to 800 g / L, the other operations were the same as those in Example 1.
[0042] Example 3
[0043] Preparation of 2mol / L zinc sulfate (ZnSO4) + 700g / L sodium tetrafluoroborate (NaBF4) + 25g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0044] Except for using 70 g of sodium tetrafluoroborate as the raw material and adjusting the concentration of sodium tetrafluoroborate to 700 g / L, the other operations were the same as those in Example 1.
[0045] Example 4
[0046] Preparation of 2mol / L zinc sulfate (ZnSO4) + 500g / L sodium tetrafluoroborate (NaBF4) + 5g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0047] Except for using 0.5 g of tris(hydroxymethyl)methylglycine powder as the raw material and adjusting the concentration of tris(hydroxymethyl)methylglycine to 5 g / L, the other operations were the same as those in Example 1.
[0048] Example 5
[0049] Preparation of 2mol / L zinc sulfate (ZnSO4) + 500g / L sodium tetrafluoroborate (NaBF4) + 50g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0050] Except for using 5 g of tris(hydroxymethyl)methylglycine powder as the raw material and adjusting the concentration of tris(hydroxymethyl)methylglycine to 50 g / L, the other operations were the same as those in Example 1.
[0051] Example 6
[0052] Preparation of 5mol / L zinc sulfate (ZnSO4) + 500g / L sodium tetrafluoroborate (NaBF4) + 25g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0053] Except for using 143.78 g of zinc sulfate heptahydrate as the raw material and adjusting the concentration of zinc sulfate to 5 mol / L, the other operations were the same as those in Example 1.
[0054] Example 7
[0055] Preparation of 2mol / L zinc sulfate (ZnSO4) + 500g / L lithium tetrafluoroborate (LiBF4) + 25g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0056] Except that the sodium tetrafluoroborate in Example 1 was replaced by lithium tetrafluoroborate of equal mass concentration, the other operations were the same as those in Example 1.
[0057] Example 8
[0058] Preparation of 2mol / L zinc sulfate (ZnSO4) + 500g / L lithium tetrafluoroborate (LiBF4) + 25g / L triglycine composite electrolyte
[0059] Except that tris(hydroxymethyl)methylglycine in Example 7 was replaced by triglycine of equal mass concentration, the other operations were consistent with Example 7.
[0060] Comparative Example 1
[0061] Preparation of 2mol / L zinc sulfate (ZnSO4) + 0g / L sodium tetrafluoroborate (NaBF4) + 25g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0062] Except that the mass concentration of sodium tetrafluoroborate in Example 1 was adjusted to 0, the other operations were the same as those in Example 1.
[0063] Comparative Example 2
[0064] Preparation of 2mol / L zinc sulfate (ZnSO4) + 500g / L sodium tetrafluoroborate (NaBF4) + 0g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0065] Except that the mass concentration of tris(hydroxymethyl)methylglycine in Example 1 was adjusted to 0, the other operations were consistent with Example 1.
[0066] Comparative Example 3
[0067] Preparation of 2mol / L zinc sulfate (ZnSO4) + 0g / L sodium tetrafluoroborate (NaBF4) + 0g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0068] Except that the mass concentrations of sodium tetrafluoroborate and tris(hydroxymethyl)methylglycine were adjusted to 0, the other operations were consistent with those in Example 1.
[0069] Comparative Example 4
[0070] Preparation of 2mol / L zinc sulfate (ZnSO4) + 200g / L sodium tetrafluoroborate (NaBF4) + 25g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0071] Except for using 20 g of sodium tetrafluoroborate as the raw material and adjusting the concentration of sodium tetrafluoroborate to 200 g / L, the other operations were the same as those in Example 1.
[0072] Example 9
[0073] Preparation of 2mol / L zinc sulfate (ZnSO4) + 500g / L sodium tetrafluoroborate (NaBF4) + 60g / L tris(hydroxymethyl)methylglycine (Tricine) composite electrolyte
[0074] Except for using 6 g of tris(hydroxymethyl)methylglycine powder as the raw material and adjusting the concentration of tris(hydroxymethyl)methylglycine to 60 g / L, the other operations were the same as those in Example 1.
[0075] Example 10
[0076] A method for preparing an electrolyte is the same as that of Example 1, except that 14.378 g of zinc sulfate heptahydrate is used as a raw material and the concentration of zinc sulfate is adjusted to 0.5 mol / L.
[0077] Example 11
[0078] A method for preparing an electrolyte, which differs from Example 1 only in that an equimolar amount of zinc acetate is used instead of the zinc sulfate in Example 1, and the other operations are the same as those in Example 1.
[0079] Example 12
[0080] A method for preparing an electrolyte differs from Example 1 only in that an equimolar amount of zinc trifluoromethanesulfonate is used instead of the zinc sulfate in Example 1, and the remaining operations are the same as those in Example 1.
[0081] Example 13
[0082] A method for preparing an electrolyte is consistent with Example 1 except that 30 g of sodium tetrafluoroborate is used as a raw material and the concentration of sodium tetrafluoroborate is adjusted to 300 g / L.
[0083] Comparative Example 5
[0084] A method for preparing an electrolyte is consistent with Example 1 except that 10 g of sodium tetrafluoroborate is used as a raw material and the concentration of sodium tetrafluoroborate is adjusted to 100 g / L.
[0085] Applying the electrolyte to an aqueous zinc ion battery comprises the following steps:
[0086] Electrode preparation: Using NMP as solvent, commercial V2O5 powder, conductive carbon black powder, and PVDF powder were uniformly mixed in a mass ratio of 7:2:1. The positive electrode slurry with appropriate viscosity was evenly coated on the Ti foil current collector, dried at 60°C, and then punched into a circular electrode with a diameter of 12 mm. This was used as the positive electrode for the zinc ion battery. The surface density of the V2O5 active material was 5 mg / cm 2Commercial zinc foil was sanded to remove the oxide layer, then cleaned with anhydrous ethanol and punched into a circular electrode with a diameter of 16 mm and a thickness of 0.08 mm to serve as the negative electrode of the zinc ion battery.
[0087] Battery Assembly: Zinc-ion batteries were assembled in the order of negative electrode, separator, electrolyte, positive electrode, gasket, and spring. (The separator was a glass fiber separator (GF / D), and the battery casing was a CR2032.) Cycling performance of the zinc-ion battery was tested at a low temperature of -35°C, a scan rate of 1 A / g, and a voltage window of 0.2-1.6 V.
[0088] The zinc ion batteries corresponding to the electrolytes prepared in the examples and comparative examples were subjected to -35°C low-temperature cycle performance tests. The test results are shown in Table 1, where failure refers to the freezing of the electrolyte and the inability of the battery to operate normally.
[0089] Table 1 Performance test results of zinc ion batteries corresponding to different electrolytes
[0090]
[0091]
[0092] In conjunction with Table 1, by comparing Example 1 with Comparative Examples 1, 2, and 3, it can be seen that, compared with a battery without tetrafluoroborate and zwitterion additives, the addition of tetrafluoroborate and zwitterion additives enables the zinc ion battery to operate at low temperatures and significantly improves the cycle capacity retention rate of the zinc ion battery.
[0093] By comparing Example 1, Example 9 and Example 2, it can be seen that the increase in the concentration of tetrafluoroborate and zwitterionic additives will aggravate the pH fluctuation at the interface and increase the Zn 2+ Electrochemical reduction resistance leads to decreased battery performance.
[0094] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the various embodiments of the present invention.
Claims
1. An electrolyte for an aqueous zinc ion battery, characterized in that: The electrolyte comprises soluble zinc salt, water, tetrafluoroborate and zwitterion additives, and the mass concentration of the tetrafluoroborate in the electrolyte is 300-800 g / L.
2. The electrolyte for aqueous zinc ion batteries according to claim 1, wherein: The mass concentration of the zwitterion additive in the electrolyte is 5-60 g / L.
3. The electrolyte for aqueous zinc ion batteries according to claim 1, wherein: The soluble zinc salt includes one or more of zinc sulfate, zinc trifluoromethanesulfonate, and zinc acetate.
4. The electrolyte for aqueous zinc ion batteries according to claim 1, wherein: The molar concentration of the soluble zinc salt in the electrolyte is 0.5-5 mol / L.
5. The electrolyte for aqueous zinc ion batteries according to claim 1, wherein: The tetrafluoroborate includes one or more of lithium tetrafluoroborate, sodium tetrafluoroborate, potassium tetrafluoroborate, ammonium tetrafluoroborate, and tetraethylammonium tetrafluoroborate.
6. The electrolyte for aqueous zinc ion batteries according to claim 1, wherein: The zwitterion additive includes one or more of tris(hydroxymethyl)methylglycine, triglycine and N-acetyl-L-proline.
7. The electrolyte for aqueous zinc ion batteries according to claim 1, wherein: The mass concentration of the tetrafluoroborate is 500-700 g / L; and / or the mass concentration of the zwitterionic additive is 25-50 g / L.
8. A method for preparing an electrolyte for an aqueous zinc ion battery according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: uniformly mixing a soluble zinc salt, tetrafluoroborate, water and a zwitterion additive to obtain the electrolyte for an aqueous zinc ion battery.
9. Use of the electrolyte for aqueous zinc ion battery according to any one of claims 1 to 7 in a zinc ion battery.
10. A zinc ion battery, characterized in that: Contains the electrolyte for aqueous zinc ion battery according to any one of claims 1 to 7.