Method for recovering rare earth elements from fluorgypsum
By roasting and leaching fluorgypsum, combined with precipitation reaction and water treatment, the problem of rare earth elements in fluorgypsum not being recycled is solved, efficient recovery and resource recycling are achieved, and environmental pollution and extraction costs are reduced.
Patent Information
- Application Number
- CN202510859759.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-25
- Publication Date
- 2025-09-26
AI Technical Summary
Existing technologies fail to effectively recycle rare earth elements in fluorspar, resulting in waste of resources and environmental pollution. In addition, the stockpiling of fluorspar increases the difficulty and cost of rare earth extraction.
The efficient recovery of rare earth elements is achieved by mixing fluorgypsum with a sulfuric acid aqueous solution and roasting it, then leaching it with water and adjusting the pH value to carry out a precipitation reaction, and finally treating the leachate and filtrate with a precipitant and a water treatment agent.
The recovery rate of rare earth elements in fluorgypsum reaches more than 90wt%, which reduces resource waste and environmental pollution and realizes the recycling of wastewater.
Smart Images

Figure CN120700304A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for recovering rare earth elements from fluorgypsum. Background Art
[0002] Fluorogypsum is a product of hydrofluoric acid produced by the reaction of fluorspar concentrate with concentrated sulfuric acid. Its primary component is calcium sulfate (Type II), which contains no water of crystallization. Every ton of hydrofluoric acid produced generates approximately 3.4 tons of anhydrous fluorogypsum. Currently, fluorogypsum is managed as a Class II general industrial solid waste and is transferred to solid waste dumps for storage. Large-scale stockpiles of fluorogypsum can damage the surrounding environment. Long-term storage and weathering can easily generate secondary dust, contaminating the surrounding soil and impacting the health of nearby residents. Fluorogypsum contains a large amount of calcium sulfate, which remains unused, resulting in a waste of resources.
[0003] The Bayan Obo mine is rich in fluorite resources. The fluorite concentrate produced contains 85-92% CaF2 by weight and 1-4% rare earth oxides (REO). During the production of anhydrous hydrogen fluoride from fluorite concentrate, the rare earth oxides in the fluorite concentrate enter fluorgypsum, turning it into a secondary rare earth resource. Fluorgypsum can only be reused after rare earth resources are recovered. Furthermore, direct storage of fluorgypsum wastes rare earth resources and reduces the economic benefits of the enterprise. Long-term storage and weathering of fluorgypsum cause phase changes in the rare earths, increasing the difficulty and cost of extraction. Therefore, developing technologies to extract and utilize rare earths, calcium sulfate, and other resources from fluorgypsum is of great significance and will bring significant economic and social benefits. Those skilled in the art have been researching how to reuse fluorgypsum.
[0004] CN118324481A discloses a highly water-resistant gypsum-based cementitious material. This material comprises the following raw materials, by weight: 60-70 wt% fluorgypsum, 15-25 wt% fly ash, 9-15 wt% cement, 3-6 wt% slag powder, 0.04-0.1% modified silica, and 0.1-0.5% CSH seed crystals. It also contains a pH regulator and an activator, wherein the pH regulator accounts for 1-5 wt% of the total weight of the fluorgypsum and fly ash, and the activator accounts for 0.5-3 wt% of the total weight of the fluorgypsum and fly ash. The fluorgypsum in this highly water-resistant gypsum-based cementitious material serves only as a component of the cementitious material, and the resource-based elements contained in the fluorgypsum are not recycled.
[0005] CN116460952A discloses a method for producing unfired hollow bricks by combining fluorgypsum with fly ash. This method comprises the following steps: fluorgypsum, carbon fiber, lignin sulfonate, fly ash, cement, and graded sand and gravel are mixed and stirred in a mixer for 20-25 minutes for the first mixing. The mixture is then fed evenly into a spiral mixer via a feeder for a second mixing. Water and a high-efficiency water reducer are added during the mixing process and stirred for 15-20 minutes. A foaming agent is then added and stirred for 10 minutes while cooling air is introduced. The mixture is then uniformly mixed to obtain a uniform mixture. A release agent is applied to the hollow brick mold, and the resulting mixture is evenly poured into multiple sets of hollow brick molds. The mixture is compacted by vibration and then cured in a curing chamber for 7-14 days. Finally, the hollow bricks are released from the molds. This method only uses fluorgypsum as a component of the hollow bricks and does not recycle the resource-based elements contained in the fluorgypsum.
[0006] CN116835626A discloses a method for the comprehensive utilization of fluorinated gypsum and aluminum electrolyte. The method comprises the following steps: (1) calcining a mixture mainly composed of aluminum electrolyte waste slag powder, fluorinated gypsum, and a calcining agent, wherein the calcining agent is ammonium carbonate; (2) alkali leaching the solid calcined product obtained in step (1) with alkali solution, solid-liquid separation, and then adsorbing the lithium ions in the liquid obtained by solid-liquid separation with an adsorbent, then eluting the adsorbent to obtain a lithium ion solution, and simultaneously mixing the adsorbed liquid with hydrogen peroxide to react to prepare an aluminate solution. This method mainly utilizes fluorinated gypsum to extract the lithium neutralized in the aluminum electrolyte waste slag powder, and does not extract or process the resource-based elements in the fluorinated gypsum. Summary of the Invention
[0007] In view of this, the present invention aims to provide a method for recovering rare earth elements from fluorgypsum. The method can achieve a recovery rate of REO in fluorgypsum of more than 90 wt%, thus realizing efficient recovery of rare earth elements in fluorgypsum.
[0008] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.
[0009] The method for recovering rare earth elements from fluorgypsum provided by the present invention comprises the following steps:
[0010] 1) crushing fluorgypsum and mixing it with a sulfuric acid aqueous solution in a weight ratio of 1:0.05-0.5 to obtain a mixed slurry I; roasting the mixed slurry I at 150-400° C. to obtain a roasted ore; wherein the mass concentration of the sulfuric acid aqueous solution is 80-98 wt%;
[0011] 2) mixing the roasted ore with water in a weight ratio of 1:1 to 5 to obtain a mixed slurry II; leaching the mixed slurry II at 20 to 60° C. and a pH of 1 to 3 to obtain a leached product; and separating the leached product into a solid and liquid to obtain a leachate and a water-leached residue;
[0012] 3) adding a precipitant to the leachate and stirring to carry out a precipitation reaction to obtain a mixed slurry III; separating the mixed slurry III into a solid-liquid phase to obtain a precipitate containing rare earth elements and a filtrate I; wherein the precipitant is selected from at least one of oxalic acid and hydroxycarboxylic acid; and the amount of the precipitant added is 1 to 6 wt% of the weight of the fluorgypsum;
[0013] 4) adding a water treatment agent to the filtrate I and stirring to react to obtain a mixed slurry IV; separating the mixed slurry IV into a solid-liquid state to obtain a mixed residue and a filtrate II; wherein the water treatment agent is a calcium oxide slurry with a mass fraction of 5 to 20 wt%; and the amount of the water treatment agent added is 5 to 12 wt% of the weight of the fluorgypsum.
[0014] In the present invention, the fluorgypsum can be any fluorgypsum product containing rare earth elements. Preferably, the fluorgypsum is produced during the production of anhydrous hydrogen fluoride using fluorspar concentrate from Bayan Obo. The fluorine content in the fluorgypsum can be 1 to 5% by weight, preferably 1.1 to 3% by weight. The REO content can be 1 to 4% by weight, preferably 1.5 to 3.5% by weight.
[0015] According to the method of the present invention, preferably, in step 1), the calcination temperature may be 150-400° C., preferably 200-300° C. The calcination time may be 1-5 hours, preferably 1.2-3 hours.
[0016] In the present invention, the mass concentration of the sulfuric acid aqueous solution may be 80 to 98 wt %, preferably 90 to 98 wt %.The weight ratio of fluorgypsum to the sulfuric acid aqueous solution may be 1:0.05 to 0.5, preferably 1:0.08 to 0.3.
[0017] Limiting the roasting conditions to the above range can ensure that rare earth elements are enriched in the roasted ore, which is beneficial to improving the recovery rate of rare earth elements.
[0018] In the present invention, pulverization can be achieved using any type of pulverization equipment known in the art, without particular limitation. For example, an impact crusher, a double-roll crusher, etc. can be used. In the present invention, the maximum particle size of the fluorgypsum after pulverization can be 0.5 to 1 mm, preferably 0.8 to 1 mm.
[0019] The roasting of the present invention can be carried out using any type of roasting equipment known in the art, which will not be described in detail herein, for example, a rotary kiln, a tubular furnace, a muffle furnace, etc.
[0020] According to the method of the present invention, preferably, in step 2), the leaching temperature can be 20-60° C., preferably 22-40° C. The leaching time can be 0.1-1 h, preferably 0.2-0.5 h.
[0021] In the present invention, the weight ratio of roasted ore to water can be 1:1-5, preferably 1:1-3.
[0022] According to the method of the present invention, preferably, in step 2), the pH value of the leaching can be 1 to 3, preferably 1.5 to 2. In the present invention, a neutralizer can be used to adjust the pH value, and the neutralizer can be selected from at least one of magnesium oxide and magnesium hydroxide, preferably at least one of magnesium oxide and magnesium hydroxide.
[0023] In step 2) of the present invention, leaching may also be performed under stirring conditions, and the stirring speed may be 2000-4000 rpm, preferably 2500-3500 rpm.
[0024] Reasonable leaching conditions can ensure that rare earth elements are effectively leached and enriched in the leachate, which is beneficial to improving the recovery rate of rare earth elements; at the same time, it is beneficial to the enrichment of calcium sulfate in the water leaching residue.
[0025] According to the method of the present invention, preferably, in step 2), the water-leached residue is washed with water to obtain washing water. The weight ratio of the water-leached residue to water can be 1:1 to 5, preferably 1:1 to 3. The washing water can replace new water and be mixed with the roasted ore for leaching, thereby achieving the recycling of wastewater. In the present invention, the first leaching is carried out with new water. When the cyclic leaching is carried out for the second time or more, the washing water obtained in the previous leaching can be used for leaching. If the amount of washing water is insufficient, new water is added.
[0026] The water used in the present invention can be any type of water known in the art that can be used for rare earth element leaching and separation, and is not particularly limited herein. For example, it can be tap water, recycled water from sewage regeneration treatment, etc.
[0027] The leaching of the present invention can be carried out in any type of leaching equipment known in the art, without particular limitation herein, such as a colloid mill, a stirred mill, and the like.
[0028] The solid-liquid separation of the present invention can be achieved using any filtration method or filtration equipment known in the art, without particular limitation herein. For example, a plate and frame filter, a vacuum filter, etc. can be used.
[0029] According to the method of the present invention, preferably, in step 3), the amount of the precipitant added can be 1 to 6 wt%, preferably 2 to 5 wt%, based on the weight of the fluorgypsum. The stirring speed can be 200 to 400 rpm, preferably 250 to 350 rpm. The stirring time can be 10 to 60 minutes, preferably 20 to 50 minutes.
[0030] According to the method of the present invention, preferably, in step 3), the precipitant can be selected from at least one of oxalic acid and hydroxycarboxylic acid, preferably at least one of oxalic acid, tartaric acid, citric acid and lactic acid.
[0031] Reasonable precipitation reaction conditions can ensure that rare earth elements are effectively precipitated, which is beneficial to improving the recovery rate of rare earth elements.
[0032] According to the method of the present invention, preferably, in step 4), the water treatment agent can be a calcium oxide slurry with a mass fraction of 5 to 20 wt%, preferably a calcium oxide slurry with a mass fraction of 8 to 15 wt%. The amount of the water treatment agent added can be 5 to 12 wt%, preferably 8 to 11.5 wt%, of the weight of the fluorgypsum.
[0033] In step 4) of the present invention, the stirring speed may be 200 to 400 rpm, preferably 250 to 350 rpm, and the stirring time may be 10 to 60 minutes, preferably 20 to 50 minutes.
[0034] In the present invention, stirring can use any type of stirring equipment known in the art, which will not be described in detail here.
[0035] According to the method of the present invention, preferably, the filtrate II obtained in step 4) can be used to wash the water-leached residue obtained in step 2), thereby achieving wastewater recycling. Fresh water is used for the initial washing of the water-leached residue. For the second or subsequent leaching cycles, the filtrate II obtained in the previous washing cycle can be used for further washing. If the amount of filtrate II is insufficient, fresh water is added.
[0036] Reasonable reaction conditions can ensure that impurity elements are effectively enriched and precipitated in the mixed slag, which is conducive to the filtrate meeting the reuse conditions.
[0037] In the present invention, the REO content in the rare earth element-containing precipitate can be 45.6 wt% or greater, preferably 45.8 wt% or greater. The REO content in the water-leached residue can be 0.5 wt% or less, preferably 0.3 wt% or less. The REO recovery rate in the fluorgypsum can be 90 wt% or greater, preferably 93 wt% or greater.
[0038] The present invention achieves a REO content of over 45.6 wt% in the rare earth element-containing precipitate, less than 0.5 wt% in the water-leached residue, and a REO recovery rate of over 90 wt% in the fluorgypsum, achieving efficient recovery of rare earth elements from the fluorgypsum. Furthermore, the present invention achieves wastewater recycling. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The present invention is a process flow chart. DETAILED DESCRIPTION
[0040] The present invention will be further described below with reference to specific embodiments, but the protection scope of the present invention is not limited thereto.
[0041] The "REO" mentioned in the present invention refers to rare earth oxides.
[0042] <Test method>
[0043] Determination of REO content: refer to GB / T 18114.1-2010.
[0044] Calculation of REO recovery rate: REO recovery rate = product yield × product REO content ÷ raw material REO content.
[0045] <Ingredients>
[0046] Unless otherwise specified, the raw materials used in the following examples are all commercially available products.
[0047] Fluorogypsum was purchased from Inner Mongolia Jin'ebo Fluorine Chemical Co., Ltd.
[0048] Example 1
[0049] The fluorine content in the fluorgypsum used in this embodiment is 1.20 wt % and the REO content is 1.62 wt %.
[0050] This embodiment recovers rare earth elements from 3 kg of fluorgypsum, and the steps are as follows:
[0051] (1) Fluorogypsum was crushed to a particle size of -1 mm using an impact crusher and then mixed with a 95 wt% concentrated sulfuric acid aqueous solution in a weight ratio of 1:0.1 to obtain a mixed slurry I. The mixed slurry I was placed in a rotary kiln and roasted at 250° C. for 1.5 h to obtain a roasted ore.
[0052] (2) The roasted ore is mixed with water in a mass ratio of 1:2 to obtain a mixed slurry II. The mixed slurry II is placed on a colloid mill and leached for 0.3 h at 25°C and a rotation speed of 3000 rpm. While stirring and leaching, magnesium oxide is added and the pH value of the mixed slurry II is adjusted to 1.6 to obtain a leaching product. Then, the leaching product is filtered using a plate and frame filter to obtain a leachate and a water-leached residue. The water-leached residue is washed with water twice the weight of the water-leached residue to obtain washing water. The washing water is used to replace new water for mixed leaching with the roasted ore during the next leaching. When the amount of washing water is insufficient, new water is added.
[0053] (3) Adding 3.5 wt% oxalic acid to the leachate at a weight of 300 rpm to the leachate for precipitation, the mixture was stirred at 300 rpm for 30 minutes to obtain a mixed slurry III. The mixed slurry III was filtered using a plate and frame filter to obtain a rare earth element oxalate precipitate and a filtrate I.
[0054] (4) Adding a calcium oxide slurry (calcium oxide mass fraction: 10 wt%) at 9 wt% of the weight of fluorgypsum to filtrate I, stirring at 300 rpm for 30 min to react, yielding mixed slurry IV. Filtering mixed slurry IV using a plate-and-frame filter yields mixed residue and filtrate II. Filtrate II is used to replace fresh water for washing the leached residue during the next leaching operation. If the amount of filtrate II is insufficient, fresh water is added.
[0055] In this embodiment, the REO content in the rare earth element oxalate precipitate is 45.88 wt %, the REO content in the water-leached residue is 0.15 wt %, and the recovery rate of REO in the fluorgypsum reaches 95.2 wt %; at the same time, no new wastewater is generated.
[0056] Example 2
[0057] The fluorine content in the fluorgypsum used in this embodiment is 1.81 wt % and the REO content is 2.52 wt %.
[0058] This embodiment recovers rare earth elements from 3 kg of fluorgypsum, and the steps are as follows:
[0059] (1) Fluorogypsum was crushed to a particle size of -1 mm using an impact crusher and then mixed with a concentrated sulfuric acid aqueous solution having a mass concentration of 98 wt% in a weight ratio of 1:0.2 to obtain a mixed slurry I. The mixed slurry I was placed in a rotary kiln and roasted at 250° C. for 2 h to obtain a roasted ore.
[0060] (2) The roasted ore and water are mixed in a mass ratio of 1:2 to obtain a mixed slurry II. The mixed slurry II is placed on a colloid mill and leached for 0.25 h at 25°C and a rotation speed of 3000 rpm. While stirring and leaching, magnesium oxide is added and the pH value of the mixed slurry II is adjusted to 1.7 to obtain a leaching product. Then, the leaching product is filtered using a plate and frame filter to obtain a leachate and a water-leached residue. The water-leached residue is washed with water twice the weight of the water-leached residue to obtain washing water. The washing water is used to replace new water for mixed leaching with the roasted ore in the next leaching. When the amount of washing water is insufficient, new water is added.
[0061] (3) Adding oxalic acid at a weight percentage of 4 wt% based on the weight of fluorgypsum to the leachate, stirring at 300 rpm for 30 minutes to effect a precipitation reaction, thereby obtaining a mixed slurry III. The mixed slurry III is filtered using a plate and frame filter to obtain a rare earth element oxalate precipitate and a filtrate I.
[0062] (4) Adding a calcium oxide slurry (calcium oxide mass fraction is 10 wt%) at a weight equivalent to 10 wt% of the weight of fluorgypsum to filtrate I, stirring at 300 rpm for 30 min to react, yielding a mixed slurry IV. Filtering the mixed slurry IV using a plate-and-frame filter yields a mixed residue and a filtrate II. Filtrate II is used to replace fresh water for washing the leached residue during the next leaching operation. If the amount of filtrate II is insufficient, fresh water is added.
[0063] In this embodiment, the REO content in the rare earth element oxalate precipitate is 46.05 wt%, the REO content in the water-leached residue is 0.22 wt%, and the recovery rate of REO in fluorgypsum reaches 94.35 wt%; at the same time, no new wastewater is generated.
[0064] Comparative Example 1
[0065] The only difference from Example 1 is that step (1) is omitted, i.e., the fluorgypsum is not subjected to pulverization and sulfuric acid roasting, but directly to water leaching. The REO content in the resulting rare earth element oxalate precipitate was 45.03 wt%, the REO content in the water leaching residue was 1.92 wt%, and the REO recovery rate in the fluorgypsum was 22.57 wt%.
[0066] Comparative Example 2
[0067] The only difference from Example 2 is that in step (2), calcium oxide is used instead of magnesium oxide to adjust the pH of the mixed slurry II. The REO content in the resulting rare earth element oxalate precipitate was 41.32 wt%, the REO content in the water-leached residue was 0.59 wt%, and the REO recovery rate in the fluorgypsum was 82.62 wt%.
[0068] The present invention is not limited to the above-mentioned embodiments. Any modification, improvement, or substitution that can be conceived by those skilled in the art without departing from the essential content of the present invention shall fall within the scope of the present invention.
Claims
1. A method for recovering rare earth elements from fluorgypsum, characterized in that: The following steps are involved: 1) crushing fluorgypsum and mixing it with a sulfuric acid aqueous solution in a weight ratio of 1:0.05-0.5 to obtain a mixed slurry I; roasting the mixed slurry I at 150-400° C. to obtain a roasted ore; wherein the mass concentration of the sulfuric acid aqueous solution is 80-98 wt%; 2) mixing the roasted ore with water in a weight ratio of 1:1 to 5 to obtain a mixed slurry II; leaching the mixed slurry II at 20 to 60° C. and a pH of 1 to 3 to obtain a leached product; and separating the leached product into a solid and liquid to obtain a leachate and a water-leached residue; 3) adding a precipitant to the leachate and stirring to carry out a precipitation reaction to obtain a mixed slurry III; separating the mixed slurry III into a solid-liquid phase to obtain a precipitate containing rare earth elements and a filtrate I; wherein the precipitant is selected from at least one of oxalic acid and hydroxycarboxylic acid; and the amount of the precipitant added is 1 to 6 wt% of the weight of the fluorgypsum; 4) adding a water treatment agent to the filtrate I and stirring to react to obtain a mixed slurry IV; separating the mixed slurry IV into a solid-liquid state to obtain a mixed residue and a filtrate II; wherein the water treatment agent is a calcium oxide slurry with a mass fraction of 5 to 20 wt%; and the amount of the water treatment agent added is 5 to 12 wt% of the weight of the fluorgypsum.
2. The method according to claim 1, characterized in that In step 1), the calcination time is 1 to 5 hours.
3. The method according to claim 1, characterized in that In step 2), the leaching time is 0.1 to 1 hour.
4. The method according to claim 1, wherein In step 2), a neutralizing agent is used to adjust the pH value to 1-3; the neutralizing agent is selected from at least one of magnesium oxide and magnesium hydroxide.
5. The method according to claim 1, wherein In step 2), the water-soaked residue is washed with water to obtain washing water.
6. The method according to claim 5, characterized in that The washing water is returned to step 2) and mixed with the roasted ore for leaching.
7. The method according to claim 1, characterized in that In step 3), the stirring time is 10 to 60 minutes.
8. The method according to claim 1, characterized in that In step 3), the hydroxycarboxylic acid is selected from at least one of tartaric acid, citric acid, and lactic acid.
9. The method according to claim 1, characterized in that In step 4), the stirring time is 10 to 60 minutes.
10. The method according to claim 1, characterized in that The filtrate II obtained in step 4) is used to wash the water-soaked residue obtained in step 2).
Citation Information
Patent Citations
Method for extracting rare earth, fluorine and thorium from fluorine-contained rare earth minerals by concentrated sulfuric acid
CN106978532A
Treatment method for fluorine-contained rare-earth mineral grains
CN109022838A
Mixture rare earth ore treatment method
CN115029546A
Method for removing fluorine from rare earth ore leachate
CN117904436A
Cited By
Method for recovering rare earth from industrial solid waste fluorgypsum
CN122303642A