Single-component low-temperature rapid thermocuring epoxy adhesive for bonding PA9T plastic
By adding a self-made long-chain tackifying resin and dimer acid-modified epoxy resin to the epoxy adhesive, the problem of low-temperature rapid curing and bonding of PA9T plastic was solved, achieving high-strength bonding performance and weather resistance.
Patent Information
- Application Number
- CN202511342469.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-19
- Publication Date
- 2025-11-28
AI Technical Summary
Existing low-temperature curing epoxy adhesives are difficult to effectively bond PA9T plastics, and high-temperature and long-time curing conditions limit their application scenarios.
By using self-made long-chain tackifying resin and dimer acid modified epoxy resin, combined with other components, a synergistic effect is formed to improve the molecular chain entanglement at the bonding interface and achieve low-temperature rapid curing.
It achieves low-temperature rapid curing of PA9T plastic at 80℃, improves bonding strength, and has good resistance to thermal shock and humid heat aging.
Smart Images

Figure BDA0005604086840000011 
Figure BDA0005604086840000021 
Figure BDA0005604086840000061
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of adhesives, and particularly relates to a single-component low-temperature rapid thermal curing epoxy adhesive for bonding PA9T plastic. BACKGROUND
[0002] PA9T (Polyamide 9T, nylon 9T) is a polyamide engineering plastic developed by Kureha, which has the toughness of aliphatic nylon and the high heat resistance, low water absorption, and chemical resistance of aromatic nylon. It has a large number of applications in the fields of electronics, automobiles, LEDs, etc. Although there are currently low-temperature curing epoxy adhesives on the market for bonding plastics, the current low-temperature curing epoxy adhesives are not ideal for bonding PA9T materials. The main reason is the low surface polarity of this material. Although the low surface polarity brings good wear resistance, it is not easy to form chemical bonds such as hydrogen bonds, thereby causing difficulties in bonding. Although patents such as CN118652664A, CN115236938A, and CN109957366A mention adding a polyamide resin to the adhesive or resin composition to improve the bonding strength, they do not mention whether the PA9T has good bonding strength. CN116836667A discloses a single-component epoxy adhesive. Although it is explicitly mentioned that the tensile shear strength of the adhesive to LCP and PA9T materials can reach more than 5 MPa, the curing conditions of the adhesive are 150℃ / 30min, the curing temperature is too high, and the curing time is too long, which limits its application scenarios. Therefore, it is urgent to develop a single-component low-temperature rapid thermal curing epoxy adhesive for bonding PA9T plastic. SUMMARY
[0003] The technical problem to be solved by the application is to provide a single-component low-temperature rapid thermal curing epoxy adhesive for bonding PA9T plastic. The adhesive of the application can be rapidly cured at a low temperature of 80℃, has good bonding performance to PA9T nylon plastic with low polarity, and also has good cold and hot impact resistance and wet heat aging resistance.
[0004] The technical solution adopted by the application to solve the above problems is as follows:
[0005] A single-component low-temperature rapid thermal curing epoxy adhesive for bonding PA9T plastic, the adhesive comprises the following raw materials by weight:
[0006]
[0007]
[0008] This invention improves the bonding strength of a single-component, low-temperature, rapid thermosetting epoxy adhesive by adding a self-made long-chain tackifying resin and a dimer acid-modified epoxy resin, which work synergistically with other components to increase the molecular chain entanglement between the epoxy resin and the PA9T material surface at the bonding interface.
[0009] Further, the epoxy resin I is one or more of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD type epoxy resin, phenolic epoxy resin, glycidyl amine type epoxy resin, and glycidyl ester type epoxy resin. The epoxy equivalent of the epoxy resin I is 50-600. Epoxy resin I is preferably Shell 828 epoxy resin or Dow Chemical 331 epoxy resin.
[0010] Furthermore, the dimer acid modified epoxy resin contains a dimer acid structure, which includes one or more mixtures of similar products with different structures and viscosities; depending on the molecular weight and structure, these dimer acid modified epoxy resins range in viscosity from 500 mPa·s to semi-solid at 50°C. Specifically, the dimer acid modified epoxy resin is preferably Shell 172 epoxy resin.
[0011] Furthermore, the self-made long-chain tackifying resin is a polyurethane-modified epoxy resin.
[0012] Furthermore, the preparation method of the self-made long-chain tackifying resin includes the following steps:
[0013] S1. First, add the polyol polymer to the reaction vessel, heat to 105-110℃, dehydrate under vacuum for 1-2 hours, then cool down to 60℃, add the isocyanate monomer dropwise to the reaction vessel, stir and heat to 75-90℃, react for 1-3 hours to obtain the prepolymer, and discharge for later use.
[0014] S2. Epoxy resin II and catalyst are added to the reaction vessel. After heating to 60°C, the above prepolymer is added dropwise to the reaction vessel and reacted at 90°C. When the content of -NCO groups is measured to be zero, the material is discharged after cooling to obtain the self-made long-chain segment tackifying resin.
[0015] In step S1, the molar ratio of the -NCO group of the isocyanate monomer to the -OH group of the polyol polymer is 2.1 to 2.5:1; in step S1, the theoretical molar ratio of the epoxy group of epoxy resin II to the remaining -NCO group in step S1 is 2.2 to 2.6:1.
[0016] More preferably, in step S1, the molar ratio of the -NCO group of the isocyanate monomer to the -OH group of the polyol polymer is 2.3:1; in step S2, the theoretical molar ratio of the epoxy group of epoxy resin II to the remaining -NCO group in step S1 is 2.4:1.
[0017] Among the polyol polymers, polyethers are selected from common polyether polyols and polyester polyols because ether bonds are less polar than ester bonds, which is more conducive to bonding to low-polarity, low-surface-energy substrates. More specifically, it includes at least one of polypropylene glycol ether polyols, polytrimethylol ether polyols, and polytetrahydrofuran ether polyols with different molecular weights and 2-3 functional groups. Preferably, the polyether polyol is a polypropylene glycol ether (PPG2000) with a molecular weight of 2000.
[0018] The isocyanate monomers include xylene diisocyanate (TDI, containing 2,4-toluene diisocyanate and 2,6-toluene diisocyanate), naphthalene diisocyanate (NDI), diphenylmethane diisocyanate (MDI), polyphenylmethane polyisocyanate (polyMDI), triphenylmethane triisocyanate (JQ-1), 1,6-hexanediisocyanate (HDI), and isophorone diisocyanate (IPDI); the isocyanate monomers also include hydrogenated compounds of these isocyanates, such as 1-methyl-2,4-diisocyanate cyclohexane, 1-methyl-2,6-diisocyanate cyclohexane, and dicyclohexylmethane diisocyanate; the isocyanate monomers also include at least one of the dimers or trimers of all of the above isocyanates. Preferably, the isocyanate monomer is isophorone diisocyanate (IPDI).
[0019] Among them, epoxy resin II is preferably E44 epoxy resin.
[0020] The catalyst is a combination of organotin and imidazole catalysts, wherein the organotin catalyst is preferably dibutyltin (DBT) structure, and the imidazole catalyst is preferably biimidazolium metal salt structure, which respectively catalyze the reaction of -NCO group with -OH group and the reaction of -NCO group with epoxy group, and work together to extend the molecular chain segment of polymer resin.
[0021] Preferably, in step S1, the molar ratio of the -NCO group of the isocyanate monomer to the -OH group of the polyol polymer is 2.3:1, and in step S2, the molar ratio of the epoxy group of epoxy resin II to the -NCO group is 2.4:1.
[0022] Further, the polythiol is one or more selected from pentaerythritol tetrakis(3-mercaptopropionic acid), trimethylolpropane tris(3-mercaptopropionate), ethylene glycol di(3-mercaptopropionate), trimethylolpropane tris(2-mercaptoacetate), diethanolamine dimercaptoacetate, isooctyl mercaptoacetate, ethoxytrimethylolpropane tris(3-mercaptopropionate), and isooctyl mercaptopropionate. The polythiol is preferably trimethylolpropane tris(2-mercaptoacetate) (i.e., TMPMP).
[0023] Further, the filler is one or more of the following: asbestos, alumina, kaolin, carbon black, graphite, silica powder, microsilica powder, calcium silicate, diatomaceous earth, magnesium oxide, titanium oxide, magnesium hydroxide, aluminum hydroxide, quartz powder, talc, calcium carbonate, magnesium carbonate, barite, mica, and clay. Preferably, the D50 particle size range of the filler is 5–50 micrometers. More preferably, the filler is a combination of calcium carbonate and talc with a D50 particle size of 10 micrometers.
[0024] Furthermore, the accelerator is one or more of modified imidazole and its derivatives, and modified amine compounds. Preferably, the accelerator is PN-23 accelerator.
[0025] Furthermore, the stabilizer is one or more of borate ester complexes and organic acid compounds. Preferably, the stabilizer is barbituric acid.
[0026] Furthermore, the defoamer is one or more of a polysiloxane-based defoamer and a silicone-free defoamer. Preferably, the polysiloxane-based defoamer is BYK-A530, and the silicone-free defoamer is BYK-1794.
[0027] Further, the coupling agent is one or more of 3-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, bis(γ-triethoxysilylpropyl)-tetrasulfide, phenyltrimethoxysilane, phenyltriethoxysilane, methyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloyloxypropyltrimethoxysilane, and γ-glycidoxypropyltrimethoxysilane. Preferably, the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane (WD-60 grade).
[0028] The present invention has the following beneficial effects:
[0029] The present invention relates to a single-component, low-temperature, rapid-curing epoxy adhesive for bonding PA9T plastic. By adding a self-made long-chain tackifying resin and a dimer acid-modified epoxy resin to the epoxy adhesive, and in conjunction with other components, a synergistic effect is achieved, increasing the molecular chain entanglement between the epoxy adhesive and the PA9T material surface at the bonding interface, thereby significantly improving the interfacial bonding strength. The adhesive of the present invention can cure rapidly at a low temperature of 80°C, exhibits good adhesion performance to low-polarity PA9T nylon plastic, and also has good resistance to thermal shock and humid heat aging. Detailed Implementation
[0030] To make the technical problems, solutions, and advantages of this invention clearer, a detailed description will be provided below with reference to specific examples. However, the scope of protection of this invention is not limited to the following specific embodiments. The described embodiments are merely some, not all, of the embodiments of this invention, and are not intended to limit the invention. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0031] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0032] Unless otherwise specified, all raw materials, reagents, instruments, and equipment used in this invention are commercially available or can be prepared using existing methods. Unless otherwise specified, the parts mentioned in this invention are parts by weight.
[0033] 1. Preparation of self-made long-chain tackifying resin:
[0034] Resin Synthesis Example 1:
[0035] S1. Add 200g of polypropylene glycol ether (PPG 2000) to a three-necked flask, heat to 105℃, and dehydrate under vacuum for 1 hour. Then, cool down to 60℃ and add 51.1g of IPDI (molar ratio -NCO:-OH = 2.3:1) to the three-necked flask. Stir and heat to 80℃, react for 3 hours to obtain the prepolymer for later use. S2. Add 141.6g of E44 epoxy resin (calculated based on the theoretical value of 2.4 times the remaining -NCO molar number in step S1) and 0.4g of catalyst (composed of dibutyltin dilaurate and biimidazole copper ion complex in a 1:1 ratio) to a three-necked flask. Heat to 60℃ and add the prepolymer dropwise to the three-necked flask. React at 90℃. When the NCO group content is zero as measured by infrared spectroscopy, cool down and discharge to obtain the self-made long-chain tackifying resin I.
[0036] Resin Synthesis Example 2:
[0037] S1. Add 200g of polypropylene glycol ether (PPG 2000) to a three-necked flask, heat to 105℃, and dehydrate under vacuum for 1 hour. Then, cool down to 60℃ and add 46.7g of IPDI (molar ratio -NCO:-OH = 2.1:1) to the three-necked flask. Stir and heat to 80℃, react for 3 hours to obtain the prepolymer for later use. S2. Add 119.9g of E44 epoxy resin (calculated based on the theoretical value of 2.4 times the remaining -NCO molar number in step S1) and 0.4g of catalyst (composed of dibutyltin dilaurate and biimidazole copper ion complex in a 1:1 ratio) to a three-necked flask. Heat to 60℃ and add the prepolymer dropwise to the three-necked flask. React at 90℃. When the NCO group content is zero as measured by infrared spectroscopy, cool down and discharge to obtain the self-made long-chain tackifying resin II.
[0038] Resin Synthesis Example 3:
[0039] S1. Add 200g of polypropylene glycol ether (PPG 2000) to a three-necked flask, heat to 105℃, and dehydrate under vacuum for 1 hour. Then, cool down to 60℃ and add 55.6g of IPDI (molar ratio -NCO:-OH = 2.5:1) to the three-necked flask. Stir and heat to 80℃, react for 3 hours to obtain the prepolymer for later use. S2. Add 163.4g of E44 epoxy resin (calculated based on the theoretical value of 2.4 times the remaining -NCO molar number in step S1) and 0.4g of catalyst (composed of dibutyltin dilaurate and biimidazole copper ion complex in a 1:1 ratio) to a three-necked flask. Heat to 60℃ and add the prepolymer dropwise to the three-necked flask. React at 90℃. When the NCO group content is zero as measured by infrared spectroscopy, cool down and discharge to obtain the self-made long-chain tackifying resin III.
[0040] Resin Synthesis Example 4:
[0041] S1. Add 200g of polypropylene glycol ether (PPG 2000) to a three-necked flask, heat to 105℃, and dehydrate under vacuum for 1 hour. Then, cool down to 60℃ and add 51.1g of IPDI (molar ratio -NCO:-OH = 2.3:1) to the three-necked flask. Stir and heat to 80℃, react for 3 hours to obtain the prepolymer for later use. S2. Add 129.8g of E44 epoxy resin (calculated based on the theoretical value of 2.2 times the remaining -NCO molar number in step S1) and 0.4g of catalyst (composed of dibutyltin dilaurate and biimidazole copper ion complex in a 1:1 ratio) to a three-necked flask. Heat to 60℃ and add the prepolymer dropwise to the three-necked flask. React at 90℃. When the NCO group content is zero as measured by infrared spectroscopy, cool down and discharge to obtain the self-made long-chain tackifying resin IV.
[0042] Resin Synthesis Example 5:
[0043] S1. Add 200g of polypropylene glycol ether (PPG 2000) to a three-necked flask, heat to 105℃, and dehydrate under vacuum for 1 hour. Then, cool down to 60℃ and add 51.1g of IPDI (molar ratio -NCO:-OH = 2.3:1) to the three-necked flask. Stir and heat to 80℃, react for 3 hours to obtain the prepolymer for later use. S2. Add 153.5g of E44 epoxy resin (calculated based on the theoretical value of 2.6 times the remaining -NCO molar number in step S1) and 0.4g of catalyst (composed of dibutyltin dilaurate and biimidazole copper ion complex in a 1:1 ratio) to a three-necked flask. Heat to 60℃ and add the prepolymer dropwise to the three-necked flask. React at 90℃. When the NCO group content is zero as measured by infrared spectroscopy, cool down and discharge to obtain the self-made long-chain tackifying resin V.
[0044] 2. Examples and Comparative Examples
[0045] This invention provides examples 1-7 for a single-component, low-temperature, rapid thermosetting epoxy adhesive for bonding PA9T plastic, and comparative examples 1-2. The formulations are shown in Table 1, where the contents are parts by weight.
[0046] Table 1 Formulations of the adhesives in the examples and comparative examples
[0047]
[0048]
[0049] In Table 1, I, II, III, IV, and V represent the self-made long-chain tackifying resins prepared in Resin Synthesis Example 1, Resin Synthesis Example 2, Resin Synthesis Example 3, Resin Synthesis Example 4, and Resin Synthesis Example 5, respectively.
[0050] The single-component, low-temperature, rapid-curing epoxy adhesive for bonding PA9T plastic in Example 1 is prepared as follows: Weigh the raw materials according to the formula, and add epoxy resin I, dimer acid-modified epoxy resin, self-made long-chain tackifying resin, polythiol, filler, stabilizer, coupling agent, and defoamer to a reaction vessel. Control the material temperature at 30℃ and the vacuum degree at no less than -0.09MPa, and stir and disperse for 90 minutes. Then add PN-23 accelerator, and stir and disperse under the same conditions for 40 minutes before discharging.
[0051] The methods for preparing adhesives in Examples 2-7 and Comparative Examples 1-2 are similar. If there are components that need to be replaced or not added, they can be replaced or removed in the corresponding preparation steps.
[0052] The adhesive test items for Examples 1-7 and Comparative Examples 1-2 are as follows:
[0053] 1. Stability test:
[0054] a. Stability test at room temperature: 5g of each adhesive from the examples / comparative examples was injected into a circular iron cap with a diameter of 4cm and spread evenly. The cap was then placed in an environment of 25±2℃ and 80±5%RH, and the time for the adhesive surface to form a skin was recorded. Skinning was considered to occur when a toothpick lightly touched the adhesive surface without picking up any adhesive.
[0055] b. 40℃ Storage Stability Test: First, use a Fibre viscometer to test the initial viscosity of the adhesive at a rotor speed of 20 r / min; then, load the adhesives of each example / comparative example into a standard 30 ml dispensing syringe and place it in a 40±2℃ oven. Take it out every day and use a Fibre viscometer to test the viscosity of the adhesive at a rotor speed of 20 r / min (the constant temperature bath is kept constant to 25±2℃). When the viscosity reaches twice or more of the initial viscosity, it is considered that the adhesive has failed and deteriorated.
[0056] 2. Extrusion volume test:
[0057] Using a standard 30ml syringe dispensing tube and an 18# standard dispensing needle, continuously extrude adhesive for 30 seconds under 4kg air pressure, and weigh the mass of the extruded adhesive.
[0058] 3. Tensile shear strength test:
[0059] The adhesive was applied to a 3mm thick PA9T board and cured at 80℃ for 10 minutes. Tensile shear samples were prepared and tested using a tensile testing machine according to GB / T7124-2008. To ensure that the breaking load was within 10%-80% of the maximum load of the tensile testing machine and that the response time of the testing machine was short enough to ensure the accuracy of the fracture time determination, the tensile speed was set to 5mm / min and the test temperature was room temperature.
[0060] 4. Tensile shear strength test after thermal shock cycles:
[0061] According to GB / T2423.22-2012, the same sample as the one used to test the tensile shear strength was subjected to 50 cycles of thermal shock treatment at -40℃ / 30min and 100℃ / 30min, with each cycle lasting 15min. The sample was then removed and tested again under the same conditions to determine its tensile shear strength.
[0062] 5. Tensile shear strength test after high temperature and high humidity:
[0063] According to GB / T 2423.3-2016, the same sample as the sample used to test the tensile shear strength was placed at 85±2℃ and 85±3%RH for 500h, and then the sample was taken out and the tensile shear strength was tested again under the same conditions.
[0064] The test results are shown in Table 2.
[0065] Table 2 Performance test results of the adhesives in the examples and comparative examples
[0066]
[0067] As shown in Table 2, by comparing Examples 1-3 and Examples 4-7, it can be seen that the adhesive using 10-30 parts of the self-made long-chain tackifying resin I has excellent adhesion to the PA9T substrate. Furthermore, when using 20 parts of the self-made long-chain tackifying resin I, the substrate of the sample was completely broken during the initial tensile-shear test. Moreover, the shear strength of the sample was also the highest after 50 cycles of thermal shock at -40℃ to 100℃ and double aging at 85500h, indicating that the adhesive using 20 parts of the self-made long-chain tackifying resin I has the best bonding effect.
[0068] Under the same conditions, adhesives using self-made long-chain tackifying resin II-V either exhibited slightly reduced bonding performance, lower extrusion volume, or insufficient stability and compatibility, and their performance was not as good as adhesives using self-made long-chain tackifying resin I. However, compared to adhesives in Comparative Examples 1 and 2 that did not use long-chain tackifying resin or dimer acid-modified epoxy resin, the samples using self-made long-chain tackifying resin II-V showed significantly better shear strength.
[0069] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
[0070] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0071] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A single-component, low-temperature, rapid-curing thermosetting epoxy adhesive for bonding PA9T plastic, characterized in that, The adhesive comprises the following raw materials in parts by weight:
2. The adhesive according to claim 1, characterized in that, The epoxy resin I is one or more of the following: bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD type epoxy resin, phenolic epoxy resin, glycidylamine type epoxy resin, and glycidyl ester type epoxy resin.
3. The adhesive according to claim 1, characterized in that, The self-made long-chain tackifying resin is a polyurethane-modified epoxy resin.
4. The adhesive according to claim 3, characterized in that, The preparation method of the self-made long-chain tackifying resin includes the following steps: S1. First, add the polyol polymer to the reaction vessel, heat to 105-110℃, dehydrate under vacuum for 1-2 hours, then cool down to 60℃, add the isocyanate monomer dropwise to the reaction vessel, stir and heat to 75-90℃, react for 1-3 hours to obtain the prepolymer, and discharge for later use. S2. Epoxy resin II and catalyst are added to the reaction vessel. After heating to 60°C, the above prepolymer is added dropwise to the reaction vessel and reacted at 90°C. When the content of -NCO groups is measured to be zero, the material is discharged after cooling to obtain the self-made long-chain segment tackifying resin. In step S1, the molar ratio of the -NCO group of the isocyanate monomer to the -OH group of the polyol polymer is 2.1 to 2.5:1; in step S2, the theoretical molar ratio of the epoxy group of epoxy resin II to the remaining -NCO group in step S1 is 2.2 to 2.6:
1.
5. The adhesive according to claim 4, characterized in that, In step S1, the molar ratio of the -NCO group of the isocyanate monomer to the -OH group of the polyol polymer is 2.3:1; in step S2, the theoretical molar ratio of the epoxy group of epoxy resin II to the remaining -NCO group in step S1 is 2.4:
1.
6. The adhesive according to claim 4, characterized in that, The polyol polymer is a polyether polyol, the epoxy resin II is E44 epoxy resin, and the catalyst is a combination catalyst of organotin and imidazole.
7. The adhesive according to claim 1, characterized in that, The polythiol is one or more of pentaerythritol tetrakis(3-mercaptopropionic acid), trimethylolpropane tris(3-mercaptopropionic acid), di(3-mercaptopropionic acid) ethylene glycol ester, trimethylolpropane tris(2-mercaptoacetic acid), diethanol dimercaptoacetic acid, isooctyl mercaptoacetate, ethoxytrimethylolpropane tris(3-mercaptopropionic acid), and isooctyl mercaptopropionic acid.
8. The adhesive according to claim 1, characterized in that, The filler is one or more of the following: asbestos, alumina, kaolin, carbon black, graphite, silica powder, microsilica powder, calcium silicate, diatomaceous earth, magnesium oxide, titanium oxide, magnesium hydroxide, aluminum hydroxide, quartz powder, talc, calcium carbonate, magnesium carbonate, barite, mica, and clay.
9. The adhesive according to claim 1, characterized in that, The accelerator is one or more of modified imidazole and its derivatives, and modified amine compounds; the stabilizer is one or more of borate ester complexes and organic acid compounds; the defoamer is one or more of polysiloxane-based defoaming agents and silicone-free defoamers.
10. The adhesive according to claim 1, characterized in that, The coupling agent is one or more of 3-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, bis(γ-triethoxysilylpropyl)-tetrasulfide, phenyltrimethoxysilane, phenyltriethoxysilane, methyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloyloxypropyltrimethoxysilane, and γ-glycidoxypropyltrimethoxysilane.
Citation Information
Patent Citations
Epoxy resin-polyamide resin adhesive
CN109957366A
Negative photosensitive polyamic acid ester resin composition and application thereof
CN115236938A
Single-component epoxy adhesive and preparation method thereof
CN116836667A
Polyester block bio-based polyamide hot melt adhesive as well as preparation method and application thereof
CN118652664A