Heteroelectrolyte secondary battery and method for manufacturing same
By using a heterogeneous electrolyte type of secondary battery in lithium secondary batteries, employing a separator impregnated with positive and negative electrode electrolytes, and utilizing polymer solid electrolytes to selectively permeate lithium ions, the problem of battery performance degradation caused by solvent or additive decomposition is solved, achieving battery stability and safety over a wide voltage range.
Patent Information
- Application Number
- CN202480034639.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-07-04
- Filing Date
- 2024-06-27
- Publication Date
- 2025-12-23
AI Technical Summary
Existing lithium secondary batteries suffer from performance degradation and limited operating voltage range due to side reactions at high or low potentials that cause solvent or additive decomposition and form undesirable byproducts.
The secondary battery employs a heterogeneous electrolyte and uses a separator impregnated with positive and negative electrode electrolytes. The separator is composed of a polymer solid electrolyte, containing polymer resin, lithium salt and solvent. It selectively permeates lithium ions, inhibits the movement of anions and additives, and forms a gel polymer electrolyte through a polymerization initiator.
Improve battery performance over a wide operating voltage range, suppress side reactions, maintain battery stability and safety, enhance the selective permeability of the electrolyte, and extend the battery's operating voltage range.
Smart Images

Figure CN121195374A_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This application claims the benefit of Korean Patent Application No. 10-2023-0086752, filed on July 4, 2023, with the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] This invention relates to a heterogeneous electrolyte secondary battery and its manufacturing method. Background Technology
[0004] With the technological advancements in electronic devices and the increasing demands they generate, the need for secondary batteries as energy sources is rapidly growing. Among these secondary batteries, lithium-ion batteries, characterized by high energy density and voltage, have been commercialized and are widely used. Typically, liquid electrolytes (especially ion-conducting organic liquid electrolytes obtained by dissolving salts in non-aqueous organic solvents) are primarily used as electrolytes for secondary batteries. However, these liquid electrolytes have drawbacks: not only are the organic solvents prone to evaporation, but rising ambient and battery temperatures can also lead to combustion, resulting in low safety. Therefore, recent research has focused on commercializing polymer electrolytes, such as gel polymer electrolytes, as alternatives to liquid electrolytes.
[0005] The oxidation and reduction stability of electrolyte components is important for battery operation over a wide operating voltage range. All rechargeable batteries used to date employ a single electrolyte. However, battery performance deteriorates when some solvents or additives, expected to significantly improve performance, decompose or form undesirable byproducts due to high- or low-potential side reactions. This makes it impossible to use certain electrolyte components or limits the operating potential, leading to a decrease in cell voltage.
[0006] On the other hand, lithium-ion (Li-Nafion) films are polymer solid electrolytes, possessing not only relatively high Li- content but also... + Ionic conductivity, and can selectively permeate Li + It also inhibits the movement of anions, additives, solvents, etc. between the positive and negative electrodes.
[0007] Therefore, there is a need to develop a heteroelectrolyte-based secondary battery that can selectively allow lithium ions to permeate while suppressing the fluidity of the electrolyte within the cell, and has a wide operating voltage range. Summary of the Invention
[0008] Technical issues
[0009] Therefore, the inventors sought to solve the problem of battery performance degradation caused by solvent or additive decomposition or formation of undesirable byproducts due to side reactions at high or low potentials, thereby providing a heteroelectrolyte secondary battery with a wide operating voltage range.
[0010] Technical solution
[0011] In the following, specific embodiments of the electrolyte composition for lithium metal batteries and the like will be described.
[0012] The terms or words used in this specification and claims should not be construed as limited to their general or dictionary meanings, and based on the principle that inventors can appropriately define the concepts of terms in order to best describe their inventions, this invention should be interpreted as having meanings and concepts consistent with the technical concept of the invention.
[0013] The terminology used herein is provided to describe exemplary embodiments, but is not intended to limit the inventive concept. Singular forms include plural forms unless the context clearly indicates otherwise.
[0014] It should be understood that the terms “comprising,” “including,” “having,” etc., are used herein to specify the presence of the said feature, integer, step, component, or combination thereof, but do not exclude the presence or addition of one or more other features, integers, steps, components, or combinations thereof.
[0015] Heterogeneous electrolyte secondary batteries
[0016] According to one embodiment of the present invention, a heterogeneous electrolyte secondary battery is provided, comprising: a positive electrode impregnated with a positive electrolyte; a negative electrode impregnated with a negative electrolyte; and a separator disposed between the positive electrode and the negative electrode and comprising a polymeric solid electrolyte, wherein the polymeric solid electrolyte comprises a polymer resin and an electrolyte, and the positive electrolyte and the negative electrolyte have different compositions from each other.
[0017] diaphragm
[0018] In an exemplary embodiment, the diaphragm may comprise a polymeric solid electrolyte containing a polymeric resin. Specifically, the polymeric solid electrolyte may be a polymeric electrolyte formed by adding a polymeric resin to a solvated lithium salt.
[0019] Therefore, polymeric solid electrolytes can contain at least one of polymeric resin, lithium salt, polymerization initiator, additives, and solvent, and the electrolyte can contain at least one of lithium salt, polymerization initiator, additives, and solvent. For example, polymeric solid electrolytes can be composed of polymeric resin, lithium salt, and solvent, thus minimizing resistance.
[0020] In an exemplary embodiment, the membrane may have a function for lithium ions (Li... + Selective permeability.
[0021] In an exemplary embodiment, the polymer resin may include a perfluorosulfonic acid resin. For example, the perfluorosulfonic acid resin may be lithium-ion Nafion.
[0022] In an exemplary embodiment, the diaphragm may be a diaphragm impregnated with a polymeric solid electrolyte or a polymeric solid electrolyte membrane. For example, as such a diaphragm, a conventional porous polymer membrane may be used alone, such as a porous polymer membrane produced by using polyolefin polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, ethylene / methacrylate copolymer, etc., or they may be laminated and used together. Alternatively, conventional porous nonwoven fabrics may be used, such as high-melting-point glass fiber, polyethylene terephthalate fiber, etc., but are not limited thereto.
[0023] In an exemplary embodiment, the polymer resin content can be from 10% to 30% by weight relative to the total weight of the separator. For example, the content can be from 10% to 20% by weight, 15% to 25% by weight, or 20% to 30% by weight. Within the above-mentioned polymer resin content range, lithium ions can be selectively permeated into the cell to maintain a state of heteroelectrolyte isolation. Figure 1 A schematic diagram illustrates the mechanism for suppressing the movement of anions and additives between the positive and negative electrodes in a gel polymer secondary battery, wherein the gel polymer matrix is densely formed in the pore space of the coating layer and the separator, thereby physically isolating components larger than Li ions between the positive and negative electrodes.
[0024] In one exemplary embodiment, the lithium salt acts as a lithium-ion source in the battery, enabling the lithium secondary battery to operate substantially, and can promote the migration of lithium ions between the positive and negative electrodes. The lithium salt commonly used in electrolytes for lithium secondary batteries can be used without limitation. For example, the lithium salt may contain Li. + It is a cation, and may contain at least one selected from the group consisting of: F - Cl - ,Br - I - NO3 - N(CN)2 - BF4 - ClO4 - AlO4 - AlCl4 - PF6 - SbF6 - AsF6- BF2C2O4 - BC4O8 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - CF3SO3 - C4F9SO3 - CF3CF2SO3 - (CF3SO2)2N - (F2SO2)2N - CF3CF2(CF3)2CO - (CF3SO2)2CH - CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - and (CF3CF2SO2)2N - .
[0025] Lithium salts can be used alone or, if necessary, in combination of two or more. The lithium salts can be appropriately varied within the generally usable range, but to achieve the best effect of forming a film on the electrode surface to prevent corrosion, lithium salts can be included in the gel polymer electrolyte composition at a concentration of 0.8 M to 2 M, specifically 0.8 M to 1.5 M.
[0026] Furthermore, in exemplary embodiments of the present invention, the solvent contained in the polymeric solid electrolyte is not limited, as long as it can minimize decomposition due to oxidation reactions during the charging and discharging of the secondary battery and exhibit the desired properties together with additives. For example, ether solvents, ester solvents, amide solvents, etc., can be used alone, or a mixture of two or more of them can be used.
[0027] As an organic solvent, an ether solvent can be selected from any one of the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether and ethyl propyl ether, or a mixture of two or more of them, but is not limited thereto.
[0028] In addition, ester solvents may include at least one compound selected from the group consisting of cyclic carbonate compounds, linear carbonate compounds, linear ester compounds, and cyclic ester compounds.
[0029] Specific examples of cyclic carbonate compounds may be any one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentene carbonate, 2,3-pentene carbonate, vinylene carbonate, and fluoroethylene carbonate (FEC), or a mixture of two or more thereof.
[0030] In addition, specific examples of linear carbonate compounds may be selected from any one of the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate and ethyl propyl carbonate, or a mixture of two or more thereof, but are not limited thereto.
[0031] Specific examples of straight-chain ester compounds may be any one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate and butyl propionate, or a mixture of two or more of them, but are not limited thereto.
[0032] Specific examples of cyclic ester compounds may be any one selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone and ε-caprolactone, or a mixture of two or more of them, but are not limited thereto.
[0033] In ester solvents, cyclic carbonate compounds are preferred because they have high dielectric constants as high-viscosity organic solvents, thus effectively dissociating lithium salts in the electrolyte. Cyclic carbonate compounds are even more preferred because they can be used to prepare heteroelectrolytes with high conductivity when mixed in appropriate proportions with low-viscosity, low-dielectric-constant linear carbonate compounds (e.g., dimethyl carbonate and diethyl carbonate) and linear ester compounds.
[0034] In one exemplary embodiment, conventional polymerization initiators known in the art can be used as polymerization initiators. For example, typical examples of polymerization initiators may include organic peroxides or hydrogen peroxide, such as benzoyl peroxide, acetyl peroxide, dilauroyl peroxide, di-tert-butyl peroxide, tert-butyl peroxide-2-ethylhexanoate, isopropylphenyl hydrogen peroxide, and hydrogen peroxide, as well as azo compounds selected from, but not limited to, at least one of the group consisting of 2,2'-azobis(2-cyanobutane), dimethyl 2,2'-azobis(2-methylpropionate), 2,2'-azobis(methylbutyronitrile), 2,2'-azobis(isobutyronitrile) (AIBN), and 2,2'-azobis(dimethylvaleronitrile) (AMVN).
[0035] The polymerization initiator can be decomposed by heat within the battery (as a non-limiting example, heat from 30°C to 100°C, specifically from 60°C to 80°C) or at room temperature (5°C to 30°C) to form free radicals, and can react with polymerizable oligomers through free radical polymerization to form a gel polymer electrolyte.
[0036] Based on 100 parts by weight of oligomer, the content of polymerization initiator can range from 0.1 parts by weight to 5 parts by weight. When the content of polymerization initiator is greater than 5 parts by weight, unreacted polymerization initiator may remain during the manufacturing process of the gel polymer electrolyte, which may adversely affect battery performance. Conversely, when the amount of polymerization initiator is less than 0.1 parts by weight, gelation may not proceed smoothly even under conditions above a certain temperature.
[0037] Optionally, the polymeric solid electrolyte may further comprise additional additives. As additional additives that can be used in this invention, vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, vinyl ethylene carbonate, cyclic sulfite, saturated sulfonyl lactone, unsaturated sulfonyl lactone, and acyclic sulfone may be used alone, or in combination of two or more of these.
[0038] In this context, cyclic sulfites may include ethylene sulfite, methyl ethylene sulfite, ethyl ethylene sulfite, 4,5-dimethyl ethylene sulfite, 4,5-diethyl ethylene sulfite, propylene sulfite, 4,5-dimethyl propylene sulfite, 4,5-diethyl propylene sulfite, 4,6-dimethyl propylene sulfite, 4,6-diethyl propylene sulfite, 1,3-butanediol sulfite, etc.; saturated sulfonyl lactones may include 1,3-propane sulfonyl lactone, 1,4-butane sulfonyl lactone, etc.; unsaturated sulfonyl lactones may include vinyl sulfonyl lactone, 1,3-propene sulfonyl lactone, 1,4-butene sulfonyl lactone, 1-methyl-1,3-propene sulfonyl lactone, etc.; and noncyclic sulfones may include divinyl sulfone, dimethyl sulfone, diethyl sulfone, methyl ethyl sulfone, methyl vinyl sulfone, etc.
[0039] Additional additives can be used in combination of two or more types, and their content can be from 0.01 wt% to 5 wt%, particularly from 0.01 wt% to 3 wt%, and even more particularly from 0.05 wt% to 3 wt%, based on the total weight of the polymeric solid electrolyte. If the amount of additional additive is less than 0.01 wt%, the effect of improving the battery's low-temperature output, high-temperature storage characteristics, and high-temperature life characteristics is not significant. Furthermore, if the amount of additional additive is greater than 5 wt%, excessive side reactions may occur in the electrolyte during battery charging and discharging. In particular, since the additional additives cannot be fully decomposed at high temperatures when excessive amounts of solid electrolyte interphase (SEI) forming additives are added, the additional additives may exist in the electrolyte as unreacted materials or precipitates at room temperature. Therefore, side reactions that reduce the life or resistivity characteristics of the secondary battery may occur.
[0040] positive electrode
[0041] In a heteroelectrolyte secondary battery according to one embodiment of the present invention, the positive electrode can be prepared by forming a positive electrode mixture layer on a positive electrode current collector, and then used by impregnation with a positive electrode electrolyte. The positive electrode mixture layer can be prepared by coating the positive electrode current collector with a positive electrode slurry containing a positive electrode active material, a binder, a conductive material, a solvent, etc., and then drying and rolling the coated positive electrode current collector.
[0042] In an exemplary embodiment, the positive electrode electrolyte may comprise a lithium salt and a solvent, as well as optional additives. In this case, the positive electrode electrolyte may comprise a solvent with poor reduction stability or a positive electrode coating film forming material. The additives and / or solvents applied to the positive electrode electrolyte may be the same as those applied to the polymeric solid electrolytes described above.
[0043] On the other hand, the positive and negative electrode electrolytes can have different compositions; for example, the type and / or concentration of lithium salts can differ. The preferred compositions of the positive and negative electrode electrolytes can depend on the cell design and the desired functionality. For example, in the case of a Si-rich cell, an excess of cyclic carbonate compounds (e.g., FEC) must be added to continuously form a coating film that suppresses side reactions caused by cracking in the active material during charging and discharging. However, this is not functional in the positive electrode and increases the overall resistance of the cell. In this case, an electrolyte composition with an excess of cyclic carbonate compounds (e.g., FEC) can be applied to the negative electrode, and an electrolyte composition with high potential stability and low ionic conductivity can be applied to the positive electrode.
[0044] In an exemplary embodiment, the lithium salt contained in the positive electrode electrolyte may include Li + It is a cation, and may contain at least one selected from the group consisting of: F- Cl - ,Br - I - NO3 - N(CN)2 - BF4 - ClO4 - AlO4 - AlCl4 - PF6 - SbF6 - AsF6 - BF2C2O4 - BC4O8 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - CF3SO3 - C4F9SO3 - CF3CF2SO3 - (CF3SO2)2N - (F2SO2)2N - CF3CF2(CF3)2CO - (CF3SO2)2CH - CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - and (CF3CF2SO2)2N - .
[0045] Lithium salts can be used alone or, if necessary, in combination of two or more. The lithium salts can be appropriately varied within the generally usable range, but to achieve the best effect of forming a coating film on the electrode surface for corrosion prevention, lithium salts can be included in the gel polymer electrolyte composition at a concentration of 0.8 M to 2 M, specifically 0.8 M to 1.5 M.
[0046] There are no particular restrictions on the positive electrode current collector, as long as it is conductive and does not cause chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treated with one of carbon, nickel, titanium, silver, etc. can be used.
[0047] The positive electrode active material is a compound capable of reversibly intercalating and deintercalating lithium. Among them, the positive electrode active material may specifically include lithium composite metal oxides containing lithium and at least one metal (such as cobalt, manganese, nickel or aluminum). More specifically, the lithium composite metal oxides may include lithium manganese oxides (such as LiMnO2, LiMn2O4, etc.), lithium cobalt oxides (such as LiCoO2, etc.), lithium nickel oxides (such as LiNiO2, etc.), lithium nickel manganese oxides (such as LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-Z Ni z O4 (where 0 < Z < 2), etc.), lithium nickel cobalt oxides (such as LiNi 1-Y1 CoY1O2 (where 0 < Y1 < 1)), lithium manganese cobalt oxides (such as LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn2- Z1 Co z1 O4 (where 0 < Z1 < 2), etc.), lithium nickel manganese cobalt oxides (such as Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1 and p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2 and p1 + q1 + r2 = 2), etc.) or lithium nickel cobalt transition metal (M) oxides (such as Li(Ni p2 Co q2 Mn r3 M S2 )O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r3 and s2 are the atomic fractions of the respective independent elements, where 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1 and p2 + q2 + r3 + s2 = 1), etc.), and may include any one of them or two or more of these compounds.
[0048] Among these materials, in terms of improving the capacity characteristics and stability of the battery, the lithium composite metal oxides may include LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxides (such as Li(Ni 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni0.5 Mn 0.3 Co 0.2 O2, Li(Ni) 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 (O2, etc.) or lithium nickel cobalt aluminum oxide (e.g., Li(Ni) 0.8 Co 0.15 Al 0.05 (O2, etc.)
[0049] Based on the total weight of solids in the cathode slurry, the content of the cathode active material can be from 80% to 99.5% by weight, especially from 85% to 95% by weight.
[0050] When the amount of positive electrode active material is below 80% by weight, the energy density decreases, and therefore the capacity may decrease.
[0051] The binder is a component that facilitates adhesion between the active material and the conductive material, as well as adhesion to the current collector. The amount of binder added is typically from 1% to 30% by weight, based on the total weight of solids in the cathode slurry. More specifically, the amount of binder added is from 1 part by weight to 50 parts by weight, and more specifically, from 3 parts by weight to 15 parts by weight, based on the total weight of solids in the cathode slurry. When the amount of binder is less than 1 part by weight, the adhesion between the electrode active material and the current collector may be insufficient. While an amount of binder greater than 50 parts by weight can improve adhesion, the content of the electrode active material may be correspondingly reduced, potentially leading to a decrease in battery capacity.
[0052] In addition, the conductive material is a material that provides conductivity without causing chemical changes in the battery, and its addition amount can be from 1% to 20% by weight, based on the total weight of solids in the positive electrode slurry.
[0053] Typical examples of such conductive materials include, for example, the following conductive materials: carbon powder, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermally cracked carbon black; graphite powder, such as natural graphite, artificial graphite, or graphite with a well-grown crystal structure; conductive fibers, such as carbon fibers or metal fibers; fluorocarbons; metal powders, such as aluminum powder and nickel powder; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives, and materials currently sold under the following names may be used: acetylene black conductive materials (Chevron Chemical Company), Denka black (Denka Singapore Private Limited or GulfOil Company), Ketjen black, EC conductive materials (Armak Company), Vulcan XC-72 (Cabot Company), and Super P (Timcal Graphite & Carbon).
[0054] The solvent may include an organic solvent, such as N-methyl-2-pyrrolidone (NMP), and its amount may be such that the desired viscosity is obtained when a positive electrode active material is included, and optionally a binder and conductive material are included. For example, the solvent content may be such that the concentration of solids in the slurry containing the positive electrode active material and optionally a binder and conductive material is 10% to 60% by weight, preferably 20% to 50% by weight.
[0055] negative electrode
[0056] In a heteroelectrolyte secondary battery according to one embodiment of the present invention, the negative electrode can be prepared by forming a negative electrode mixture layer on a negative electrode current collector, and then used by impregnation with a negative electrode electrolyte. The negative electrode mixture layer can be prepared by coating the negative electrode current collector with a negative electrode slurry containing a negative electrode active material, a binder, a conductive material, a solvent, etc., and then drying and rolling the coated negative electrode current collector.
[0057] In an exemplary embodiment, the negative electrode electrolyte may comprise a lithium salt and a solvent, as well as optional additives. In this case, the negative electrode electrolyte may comprise a solvent with poor oxidative stability or a negative electrode coating film forming material. The additives and / or solvents applied to the negative electrode electrolyte may be the same as those applied to the polymeric solid electrolytes described above.
[0058] In an exemplary embodiment, the lithium salt contained in the negative electrode electrolyte may include Li + It is a cation, and may contain at least one selected from the group consisting of: F - Cl- ,Br - I - NO3 - N(CN)2 - BF4 - ClO4 - AlO4 - AlCl4 - PF6 - SbF6 - AsF6 - BF2C2O4 - BC4O8 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - CF3SO3 - C4F9SO3 - CF3CF2SO3 - (CF3SO2)2N - (F2SO2)2N - CF3CF2(CF3)2CO - (CF3SO2)2CH - CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - and (CF3CF2SO2)2N - .
[0059] Lithium salts can be used alone or, if necessary, in combination of two or more. The lithium salt concentration can be appropriately varied within the generally usable range, but to achieve the best effect of forming a coating film on the electrode surface to prevent corrosion, lithium salts can be included in the negative electrode electrolyte at a concentration of 0.8 M to 2 M, specifically 0.8 M to 1.5 M.
[0060] The thickness of the negative electrode current collector can generally be from 3 μm to 500 μm. The negative electrode current collector is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or copper or stainless steel treated on the surface with one of carbon, nickel, titanium, silver, etc., aluminum cadmium alloy, etc. can be used. In addition, similar to the positive electrode current collector, the negative electrode current collector can have fine concavo-convex structures formed on its surface to enhance the adhesion of the negative electrode active material. For example, the negative electrode current collector can be used in various forms such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabric structures.
[0061] In addition, the negative electrode active material can include lithium metal, carbon materials capable of reversibly intercalating / deintercalating lithium ions, metals or alloys of lithium with these metals, metal composite oxides, materials capable of doping and dedoping lithium, and transition metal oxides.
[0062] As the carbon materials capable of reversibly intercalating / deintercalating lithium ions, any carbon material can be used without particular limitation as long as it is a carbon-based negative electrode active material commonly used in lithium ion secondary batteries. As typical examples thereof, crystalline carbon, amorphous carbon, or both can be used. Examples of crystalline carbon can be graphite, such as natural graphite or artificial graphite in irregular shape, planar shape, sheet shape, spherical shape, or fibrous shape. Examples of amorphous carbon can be soft carbon (low-temperature calcined carbon) or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0063] As the metals or alloys of lithium with these metals, metals selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn or alloys of lithium with these metals can be used.
[0064] As the metal composite oxides, at least one selected from the group consisting of PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1), and Sn x Me 1-x Me' y O z (where Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, elements of Groups I, II, and III of the periodic table, halogens; 0<x≤1; 1≤y≤3; 1≤z≤8) can be used.
[0065] The materials capable of doping and dedoping lithium can include Si, SiOx (0 < x < 2), Si - Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, Sn - Y (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), etc., and at least one of them can be mixed and used with SiO2. The element Y can be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0066] Transition metal oxides can include lithium - containing titanium composite oxides (LTO), vanadium oxides, lithium vanadium oxides, etc.
[0067] Based on the total weight of the solids in the negative electrode slurry, the content of the negative electrode active material can be 80% to 99% by weight.
[0068] The binder is a component that helps the adhesion between the conductive material, the active material, and the current collector, and based on the total weight of the solids in the negative electrode slurry, the addition amount of the binder is 1% to 30% by weight. Examples of the binder can include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene - propylene - diene polymer (EPDM), sulfonated EPDM, styrene - butadiene rubber, nitrile rubber, fluororubber, various copolymers thereof, etc.
[0069] The conductive material can be the same as the conductive material used in the preparation of the positive electrode, and based on the total weight of the solids in the negative electrode slurry, the addition amount of the conductive material can be 1% to 20% by weight.
[0070] The solvent can include water or organic solvents such as NMP (N - methyl - 2 - pyrrolidone), etc., and its amount can be such that the negative electrode active material and optionally the binder, conductive material, etc. contained together with the solvent have the required viscosity. For example, the content of the solvent can be such that the concentration of the solids containing the negative electrode active material and optionally the binder and conductive material is 50% to 95% by weight, preferably 70% to 90% by weight.
[0071] In an exemplary embodiment, the first gel polymer and the second gel polymer can be the same substance or they can be different substances. On the other hand, the content of the first gel polymer in the positive electrode electrolyte and the content of the second gel polymer in the negative electrode electrolyte can be substantially the same as or different from each other. That is, the content of the first gel polymer in the positive electrode electrolyte can be greater than or less than the content of the second gel polymer in the negative electrode electrolyte.
[0072] In an exemplary embodiment, the separator can be in direct contact with the positive and negative electrodes. Specifically, no additional layer may be provided between the separator and the positive electrode or between the separator and the negative electrode, so at least a portion of the separator can be in direct contact with the positive and negative electrodes. Therefore, a heterogeneous electrolyte secondary battery according to one embodiment of the present invention can provide adhesion by curing the positive electrode / separator / negative electrode under compressed conditions, thus eliminating the need for separate adhesion materials or lamination processes.
[0073] Manufacturing method of heteroelectrolyte secondary batteries
[0074] According to another embodiment of the present invention, a method for manufacturing a heterogeneous electrolyte secondary battery is provided, the method comprising the following steps: impregnating a spare positive electrode and a spare negative electrode with a positive electrode electrolyte and a negative electrode electrolyte, respectively, to prepare a positive electrode and a negative electrode; impregnating a separator with a polymeric solid electrolyte, or using a polymeric solid electrolyte membrane, to prepare an electrolyte layer; and sequentially stacking a positive electrode, an electrolyte layer, and a negative electrode.
[0075] The manufacturing method of this invention involves pre-impregnating the electrodes and separator before assembly, thereby reducing the amount of electrolyte by using a minimal amount, thus offering advantages in terms of safety and cost. Furthermore, except for the electrode-electrolyte impregnation and crosslinking processes, current large-scale production processes can be used in the same manner, thus requiring no addition or modification of any special equipment.
[0076] First, a spare positive electrode and a spare negative electrode can be prepared by impregnating them separately with a positive electrode electrolyte and a negative electrode electrolyte. Specifically, a spare positive electrode prepared by forming a positive electrode mixture layer on a positive electrode current collector can be impregnated with a positive electrode electrolyte containing a first gel polymer, and a spare negative electrode prepared by forming a negative electrode mixture layer on a negative electrode current collector can be impregnated with a negative electrode electrolyte containing a second gel polymer. Impregnation can be performed using methods commonly used in this technical field.
[0077] In an exemplary embodiment, the impregnation step can be performed at room temperature for 2 to 48 hours to uniformly impregnate the entire positive and negative electrodes. The content of the first gel polymer can be from 0.1% to 10% by weight relative to the total weight of the impregnated positive electrode, and the content of the second gel polymer can be from 0.1% to 10% by weight relative to the total weight of the impregnated negative electrode.
[0078] Alternatively, the separator can be impregnated with a polymeric solid electrolyte, or a polymeric solid electrolyte membrane can be used to prepare the electrolyte layer. Specifically, the separator and the polymeric solid electrolyte can be the same as described above, and can be impregnated in the same manner as the electrodes. Such a separator can be made by using a separator impregnated with a minimum amount of high-content polymeric solid electrolyte, or by using a high-content gel polymer film, thereby minimizing the increase in resistance.
[0079] Next, the positive electrode, separator, and negative electrode can be sequentially stacked and cured. For example, the positive electrode, electrolyte layer, and negative electrode can be arranged sequentially to form an electrode assembly. Specifically, the electrode assembly can be a stacked structure containing two electrodes (i.e., a positive electrode and a negative electrode) and an electrolyte layer as a separator disposed between the electrodes or above or below one of the electrodes to insulate the electrodes from each other. The stacked structure can have various forms without limitation, such as: stacking a given standard positive and negative electrode with the separator between them, or winding them in the form of a core. Positive and negative tabs can be connected to the electrode assembly. Specifically, the positive and negative tabs are connected to the positive and negative electrodes of the electrode assembly, respectively, and can protrude to the outside of the secondary battery casing to provide a path for electron migration.
[0080] Subsequently, the stacked positive electrode, separator, and negative electrode can be thermosetting. Specifically, the positive electrode electrolyte impregnated in the positive electrode, the negative electrode electrolyte impregnated in the negative electrode, and the polymer-based solid electrolyte of the separator can be thermosetting. This curing step can be performed using a thermosetting process.
[0081] Beneficial effects
[0082] As described above, one embodiment of the gel polymer secondary battery of the present invention applies a high content of polymeric solid electrolyte to the separator, thereby suppressing the movement of substances with larger molecular weights between the positive and negative electrodes, selectively allowing only lithium ions to permeate within the cell, and maintaining the isolation of heterogeneous electrolytes. Furthermore, by utilizing a separator impregnated with a polymeric solid electrolyte such as Li-Nafion, the composition of the positive and negative electrodes can be changed in a battery designed to allow only lithium ion permeation. This allows the use of solvents, salts, additives, etc., with poor oxidation and reduction stability at specific potentials over a wide operating voltage range without side reactions. Attached Figure Description
[0083] Figure 1 A schematic diagram illustrating a mechanism for suppressing the movement of anions and additives between the positive and negative electrodes in a heteroelectrolyte secondary battery according to an embodiment of the present invention is shown; and
[0084] Figure 2 and Figure 3 A comparison of charge-discharge analysis results of heterogeneous electrolyte secondary batteries of Examples 1 to 2 of the present invention is shown. Detailed Implementation
[0085] Embodiments of the present invention will be described in detail below to enable those skilled in the art to readily implement them. However, the present invention can be implemented in various different forms and is not limited to the embodiments provided herein.
[0086] Example 1: Battery using heterogeneous gel electrolyte
[0087] 1 M LiPF6 was dissolved in a solvent (ethylene carbonate (EC):propylene carbonate (PC) volume ratio = 5:5), and 0.06 wt% AIBN as a polymerization initiator was added to prepare the positive electrode electrolyte, and an NCM 811 positive electrode was impregnated therein. Conversely, 2 M LiFSI was dissolved in a solvent (ethylene carbonate (EC):propylene carbonate (PC) volume ratio = 5:5), and 0.06 wt% AIBN as a polymerization initiator was added to prepare the negative electrode electrolyte, and a graphite negative electrode was impregnated therein.
[0088] In addition, 20 wt% Li-Nafion and 0.06 wt% AIBN as a polymerization initiator were added to NMP solvent to prepare a polymer-based solid electrolyte composition, and a PP membrane was impregnated therein. After impregnation, the membrane was vacuum dried at 100°C for 12 hours to remove the NMP solvent.
[0089] The prepared materials are stacked sequentially in the order of positive electrode / separator / negative electrode and then thermosetting under compression to produce a "Group 1" full cell.
[0090] Example 2: Battery using heterogeneous gel electrolyte membrane
[0091] The “Group 2” full cell (Li-Nafion membrane: 13 μm, membrane: approximately 70 μm) was manufactured in the same manner as in Example 1, except that the Li-Nafion membrane (Nafion membrane purchased from Sigma-Aldrich, reacted with 1 M LiOH solution and lithiated) was used as the polymeric solid electrolyte.
[0092] Example 3: Battery using heterogeneous gel electrolyte
[0093] The “Group 3” full cell was manufactured in the same manner as in Example 1, except that a PP separator without impregnation of a polymer-based solid electrolyte composition was used.
[0094] Experimental Example 1: Charge and Discharge Analysis
[0095] The charge / discharge efficiency of the secondary batteries manufactured in Examples 1 to 3 was evaluated, and the results were as follows: Figure 2 As shown in the figure. Specifically, the samples of Examples 1 to 3 were charged to 4.20 V with a constant current of 0.1 C, left to stand for 30 minutes, and then discharged to 2.5 V with a constant current of 0.1 C. The charge-discharge characteristics in the first cycle were observed.
[0096] Furthermore, the samples from Examples 1 to 3 were initially charged and discharged twice at 0.1 C, then charged and discharged three times at 0.33 C. This charging and discharging process was repeated, and the discharge capacity of each cycle was measured. Figure 3 As shown in the image.
[0097] During the initial charging process, the PC interacts with Li + Coordinated Li-(PC)n infiltrates into the graphite lattice structure of the negative electrode, leading to structural disruption and exfoliation, and consequently, a decrease in capacity. Specifically, when 2 M LiFSI is applied, Li... + - The coordination number between PCs is reduced, thus significantly reducing performance degradation caused by stripping.
[0098] Reference Figure 2 and Figure 3 It can be confirmed that in Example 1 (Group 1), the movement of the electrolyte impregnated in the positive electrode via the separator was prevented, and in Example 2 (Group 2), movement via the heterogeneous gel electrolyte membrane was prevented. However, in the case of Example 2 (Group 2), while the movement of electrolytes to each other was prevented, due to the thicker membrane, in Example 3 (Group 3), the electrolyte impregnated in the positive electrode moved and mixed with the electrolyte impregnated in the negative electrode, showing a trend of significantly reduced capacity and lifetime. Thus, it can be confirmed that the Li-Nafion or Li-Nafion membrane impregnated in the separator effectively prevents the movement of matter between the positive and negative electrodes.
[0099] Therefore, the gel polymer secondary battery of the present invention, by applying a separator impregnated with Li-Nafion, can maintain the isolation of heterogeneous electrolytes between the positive and negative electrodes, and can have the effects of a wide operating voltage range and reduced electrolyte amount.
Claims
1. A heterogeneous electrolyte secondary battery, comprising: A positive electrode impregnated with a positive electrolyte; A negative electrode impregnated with a negative electrolyte; and A membrane containing a polymeric solid electrolyte is disposed between the positive electrode and the negative electrode. in, The polymer-based solid electrolyte comprises a polymer resin and an electrolyte, and the positive electrode electrolyte and the negative electrode electrolyte have different compositions from each other.
2. The heterogeneous electrolyte secondary battery as described in claim 1, wherein: The diaphragm is a diaphragm impregnated with the polymer-based solid electrolyte or the polymer-based solid electrolyte membrane.
3. The heterogeneous electrolyte secondary battery as described in claim 1, wherein: The polymer resin includes perfluorosulfonic acid resin.
4. The heterogeneous electrolyte secondary battery as described in claim 3, wherein: The perfluorosulfonic acid resin is lithium-ion Nafion.
5. The heterogeneous electrolyte secondary battery as described in claim 1, wherein: The content of the polymer resin is from 10% to 30% by weight relative to the total weight of the diaphragm.
6. The heterogeneous electrolyte secondary battery as described in claim 1, wherein: The content of the polymer resin is 15% to 25% by weight relative to the total weight of the diaphragm.
7. The heterogeneous electrolyte secondary battery as described in claim 1, wherein: The positive electrode electrolyte and the negative electrode electrolyte comprise at least one lithium salt selected from the group consisting of: LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3 and LiB(C2O4)2.
8. The heterogeneous electrolyte secondary battery as described in claim 7, wherein: The positive electrode electrolyte and the negative electrode electrolyte contain different lithium salts.
9. The heterogeneous electrolyte secondary battery as described in claim 7, wherein: The positive electrode electrolyte contains a lithium salt with a concentration of 0.1 M to 2 M.
10. The heterogeneous electrolyte secondary battery as described in claim 7, wherein: The negative electrode electrolyte contains a lithium salt with a concentration of 1 M to 3 M.
11. The heterogeneous electrolyte secondary battery as described in claim 1, wherein: The membrane facilitates the removal of lithium ions (Li). + It has selective permeability.
12. The heterogeneous electrolyte secondary battery as described in claim 1, wherein: The diaphragm is in direct contact with the positive electrode and the negative electrode.
13. A method for manufacturing a heterogeneous electrolyte secondary battery, the method comprising the following steps: The positive electrode and the negative electrode were respectively impregnated with positive electrolyte and negative electrolyte to prepare the positive electrode and the negative electrode; An electrolyte layer is prepared by impregnating a membrane with a polymer-based solid electrolyte, or by using a polymer-based solid electrolyte membrane; and The positive electrode, the electrolyte layer, and the negative electrode are stacked in sequence.
Citation Information
Patent Citations
Treatment of cervical dystonia
KR1020230086752A