Production method of flat-bulb titanium profile for marine equipment

By using segmented electromagnetic induction heating and semi-continuous rolling processes, the problems of low surface quality and yield in the production of spherical flat titanium have been solved, enabling efficient and low-cost production of high-precision spherical flat titanium profiles to meet the high-end needs of marine equipment.

CN121315065APending Publication Date: 2026-01-13CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202511529843.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-24
Publication Date
2026-01-13

AI Technical Summary

Technical Problem

Existing methods for producing flattened spherical titanium have problems such as easy surface cracking, pitting and pitting, difficulty in controlling shape and size, low yield, and poor uniformity of mechanical properties, which cannot meet the high-precision quality control requirements of high-end marine equipment.

Method used

A segmented electromagnetic induction heating method is used to heat titanium alloy billets, including low-temperature, medium-temperature, high-temperature and heat-holding sections. Combined with a semi-continuous rolling process, high-quality spherical flat titanium profiles are prepared by controlling the frequency and current of electromagnetic induction heating, along with rolling, cooling, straightening, shot peening and passivation treatments.

Benefits of technology

This has improved the surface quality of titanium alloys, avoiding pitting and roughness, ensuring temperature uniformity, increasing production efficiency and yield, meeting the high precision requirements of marine equipment, and reducing energy consumption and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121315065A_ABST
    Figure CN121315065A_ABST
Patent Text Reader

Abstract

The invention relates to a production method of a flat-bulb titanium profile for marine equipment, belongs to the technical field of non-ferrous metals, and is used for solving at least one of the problems that the surface of flat-bulb titanium prepared by the existing method is easy to crack, pitted surfaces and pitted spots exist, the shape and size are difficult to control, the yield is low, and the uniformity of mechanical properties is poor. By adopting segmented heating and controlling the frequency and the current of each segment of heating, electromagnetic induction heating of the non-magnetic metal titanium can be realized, pits and pitted surfaces on the surface of the titanium alloy can be effectively prevented, and the flat-bulb titanium profile for the marine equipment with high surface quality is obtained; in addition, rapid and efficient heating of the non-magnetic metal titanium alloy is achieved through the electromagnetic induction heating mode, cost is reduced, and energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metals technology, and in particular to a method for producing spherical flat titanium profiles for marine equipment. Background Technology

[0002] Titanium alloys, characterized by high specific strength, excellent corrosion resistance, non-magnetic properties, and weldability, are hailed as natural "marine metals." In recent years, with the rapid development of lightweight ships and deep-sea submersibles, the demand for titanium alloy materials has been increasing. Flattened spherical titanium, as a specialized profile for titanium alloy hull structures, is used in the keel and reinforcing ribs of ships, playing a role in strengthening and preventing deflection. However, the production and application of flattened spherical titanium are still in their early stages, and the corresponding products suffer from problems such as large performance fluctuations, poor surface quality, and difficulty in controlling shape and dimensions.

[0003] Currently, the production methods for spherical flat titanium include extrusion molding and rolling molding processes. Patent CN116689534A discloses an extrusion process for pure titanium spherical flat profiles. The main invention aims to improve upon the problems of surface cracking, large dimensional deviations, and poor overall performance inherent in the extrusion process. While this invention improves the shape and performance control of extruded spherical flat titanium, it cannot meet the high-precision quality control requirements of high-end marine equipment. Furthermore, the extrusion method suffers from low production efficiency, product shape distortion, and uneven mechanical properties. Patent CN 117324370A discloses a production method for spherical flat titanium profiles, primarily employing a rolling process to address the low production efficiency, product shape distortion, and substandard end performance issues of the extrusion process. However, this process uses a resistance furnace for heating, resulting in high energy consumption, severe oxide scaling, and poor material surface quality and coarse grains. Summary of the Invention

[0004] In view of the above analysis, the present invention aims to provide a method for producing spherical flat titanium profiles for marine equipment, so as to solve at least one of the problems of spherical flat titanium profiles prepared by existing methods, such as easy cracking of the surface, presence of pitting and pinholes, difficulty in controlling shape and size, low yield, and poor uniformity of mechanical properties.

[0005] In a first aspect, the present invention provides a method for producing spherical flat titanium profiles for marine equipment, the method comprising heating a titanium alloy billet using electromagnetic induction heating;

[0006] The electromagnetic induction heating includes sequentially performing low-temperature heating, medium-temperature heating, high-temperature heating, and heat preservation heating. The frequency of the electromagnetic induction heating is 20-28Hz. The current for the low-temperature heating is 1000-2000A, the current for the medium-temperature heating is 2000-3000A, the current for the high-temperature heating is 1500-2500A, and the current for the heat preservation heating is 1200-2400A.

[0007] Furthermore, the heating time for the low-temperature section is 3-5 minutes, the heating time for the medium-temperature section is 7.5-10 minutes, the heating time for the high-temperature section is 7.5-10 minutes, and the heating time for the heat preservation section is 2-3 minutes.

[0008] Furthermore, the titanium alloy blank is a round blank with dimensions of 70-90mm × 2500-3500mm.

[0009] Furthermore, the electromagnetic induction heating is carried out to a surface temperature of 800–1200°C for the billet.

[0010] Furthermore, the method also includes sequentially rolling, cooling, straightening, heat treatment, shot peening, and passivation of the billet after electromagnetic induction heating treatment to obtain the spherical flat titanium profile.

[0011] Furthermore, the rolling process involves 10 passes, including roughing and finishing rolling.

[0012] Furthermore, the roughing speed is 2.0 to 2.5 m / s, and the finishing speed is 0.75 to 1.5 m / s.

[0013] Furthermore, the passivation treatment is acid washing.

[0014] Furthermore, the passivation treatment involves immersing the sample in an acid pickling tank for 15–60 minutes.

[0015] Secondly, the present invention provides a spherical flat titanium profile for marine equipment obtained by the above-described production method.

[0016] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0017] (1) By using the segmented heating of the present invention and controlling the frequency and the current of each segment heating, electromagnetic induction heating of non-magnetic titanium can be realized, which can effectively prevent the formation of pits and rough surfaces on the titanium alloy surface and obtain high surface quality spherical flat titanium profiles for marine equipment. In addition, the electromagnetic induction heating method realizes rapid and efficient heating of non-magnetic titanium alloys, reduces costs and saves energy consumption.

[0018] (2) In the segmented heating of this invention, a frequency of 20-28Hz can achieve a greater penetration depth and avoid excessive temperature difference between the surface and core of the billet; if the frequency is too high, it will be difficult to achieve heating, and if the frequency is too low, it will lead to severe surface oxidation. The segmented current of this invention can realize the preheating, heating, high temperature and heat preservation heating processes, and achieve temperature uniformity at the beginning and end as well as on the surface and in the core.

[0019] (3) In this invention, a semi-continuous rolling mill is used to form spherical flat titanium. Pre-deformation of the spherical flat titanium is achieved through rough rolling, and then precise control of the dimensional shape of the spherical flat titanium is ensured by a high-precision continuous rolling mill. This invention achieves efficient heating, high-precision rolling, and low-cost production through the synergistic effect of electromagnetic induction heating and the semi-continuous rolling process. The resulting spherical flat titanium exhibits excellent mechanical properties, with a finished product yield exceeding 95%, meeting the design and construction requirements of ships and marine equipment.

[0020] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0021] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0022] Figure 1 This is a diagram of the K1-K10 pass profiles in the semi-continuous rolling process for spherical flat titanium in this invention;

[0023] Figure 2 This is a macroscopic morphology diagram of the rolled TA3 spherical flat titanium in Example 1 of the present invention;

[0024] Figure 3 This is a 200x magnification microstructure image of a TA3 spherical flattened titanium prepared in Example 1 of the present invention;

[0025] Figure 4 This is a 500x magnification microstructure of a TA3 spherical flattened titanium prepared in Example 1 of the present invention. Detailed Implementation

[0026] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0027] While existing technologies include methods for producing bulb flat steel using electromagnetic induction heating, these methods cannot be directly applied to bulb flat titanium. This is primarily due to two major technical obstacles: First, regarding magnetism, bulb flat steel, as a ferromagnetic material, exhibits high permeability and a significant eddy current effect, resulting in extremely high induction heating efficiency. In contrast, titanium alloys are non-magnetic materials with extremely low permeability, leading to poor energy coupling efficiency when relying on eddy current heating. Therefore, parameters such as frequency and current need to be redesigned to avoid insufficient heating or uneven temperature distribution. Second, structurally, bulb flat titanium, as a high-precision profile used in ship keels, has extremely stringent requirements for temperature uniformity and microstructure consistency during rolling due to its unique bulb-web structure. Directly applying the crude heating process used for bulb flat steel can easily lead to localized overheating, coarse grains, or excessively thick oxide layers in the titanium alloy, resulting in problems such as cracks, pitting, substandard performance, and a sharp drop in yield. Therefore, it is essential to develop a dedicated induction heating process adapted to the characteristics of non-magnetic titanium alloys and the structural features of the profiles.

[0028] A specific embodiment of the present invention discloses a method for producing spherical flat titanium profiles for marine equipment, the method comprising heating a titanium alloy billet using electromagnetic induction heating;

[0029] The electromagnetic induction heating includes sequential heating in a low-temperature section, heating in a medium-temperature section, heating in a high-temperature section, and heating in a heat-preserving section. The frequency of the electromagnetic induction heating is 20–28 Hz, for example, 20 Hz, 21 Hz, 22 Hz, 23 Hz, 24 Hz, 25 Hz, 26 Hz, 27 Hz, and 28 Hz. The current for the low-temperature section heating is 1000–2000 A, for example, 1000 A, 1100 A, 1200 A, 1300 A, 1400 A, 1500 A, 1600 A, 1700 A, 1800 A, 1900 A, and 2000 A. The current for the medium-temperature section heating is 2000–3000 A, for example, 2000 A, 2100 A, and 2200 A. The heating current of the high-temperature section is 1500-2500A, for example, 1500A, 1600A, 1700A, 1800A, 1900A, 2000A, 2100A, 2200A, 2300A, 2400A, 2500A. The heating current of the heat preservation section is 1200-2400A, for example, 1200A, 1300A, 1400A, 1500A, 1600A, 1700A, 1800A, 1900A, 2000A, 2100A, 2200A, 2300A, 2400A, 2400A.

[0030] Compared with existing technologies, the segmented heating of this invention, with control over the frequency and current of each segment, enables electromagnetic induction heating of non-magnetic titanium. This effectively prevents pitting and roughness on the surface of titanium alloys, resulting in high-quality spherical flat titanium profiles for marine equipment. Furthermore, the electromagnetic induction heating method enables rapid and efficient heating of non-magnetic titanium alloys, reducing costs and saving energy consumption.

[0031] It should be noted that the segmented heating in this invention uses a heating current obtained through extensive experimentation. A frequency of 20-28Hz achieves greater penetration depth, preventing excessive temperature differences between the surface and core of the billet. Too high a frequency makes heating difficult, while too low a frequency leads to severe surface oxidation. The segmented current of this invention enables preheating, heating, high-temperature heating, and heat preservation processes, ensuring temperature uniformity at the beginning and end, as well as between the surface and core.

[0032] Specifically, the heating time in the low-temperature section is 3-5 minutes, for example, 3 minutes, 3.2 minutes, 3.4 minutes, 3.6 minutes, 3.8 minutes, 4.0 minutes, 4.2 minutes, 4.4 minutes, 4.6 minutes, 4.8 minutes, or 5 minutes; and the heating time in the medium-temperature section is 7.5-10 minutes, for example, 7.5 minutes, 7.7 minutes, 7.9 minutes, 8.1 minutes, 8.3 minutes, 8.5 minutes, 8.7 minutes, 8.9 minutes, 9.1 minutes, 9.3 minutes, 9.5 minutes, 9.7 minutes, 9.9 minutes, or 10 minutes. The heating time of the high-temperature section is 7.5 to 10 minutes, for example, 7.5 minutes, 7.7 minutes, 7.9 minutes, 8.1 minutes, 8.3 minutes, 8.5 minutes, 8.7 minutes, 8.9 minutes, 9.1 minutes, 9.3 minutes, 9.5 minutes, 9.7 minutes, 9.9 minutes, or 10 minutes. The heating time of the heat preservation section is 2 to 3 minutes, for example, 2 minutes, 2.1 minutes, 2.2 minutes, 2.3 minutes, 2.4 minutes, 2.5 minutes, 2.6 minutes, 2.7 minutes, 2.8 minutes, 2.9 minutes, or 3 minutes.

[0033] Specifically, the titanium alloy billet is a round billet with dimensions of 70-90mm × 2500-3500mm. For example, the diameter of the round billet is 70mm, 80mm, or 90mm.

[0034] It should be noted that the titanium alloy of the present invention also includes a process to remove the surface oxide layer and impurities before heating.

[0035] Specifically, the electromagnetic induction heating to the surface temperature of the billet is 800–1200℃, for example, 800℃, 820℃, 840℃, 860℃, 880℃, 900℃, 920℃, 940℃, 960℃, 980℃, 1000℃, 1020℃, 1040℃, 1060℃, 1080℃, 1100℃, 1120℃, 1140℃, 1160℃, 1180℃, and 1200℃. For example, the heating temperature of TA3 titanium alloy is approximately 850–870℃; the heating temperature of TA17 titanium alloy is approximately 890–920℃.

[0036] Specifically, the method further includes sequentially rolling, cooling, straightening, heat treatment, shot peening, and passivation of the billet after electromagnetic induction heating treatment to obtain the spherical flat titanium profile.

[0037] Specifically, the rolling process involves using a semi-continuous rolling mill to roll the titanium alloy billet into shape.

[0038] Specifically, the rolling process involves 10 passes, including roughing and finishing rolling.

[0039] Preferably, the rolling pass is divided into Φ400mm roughing and Φ320mm finishing, and the pass names are K10-K9-K8-K7-K6-K5-K4-K3-K2-K1, with K10-K6 being roughing passes and K5-K1 being finishing passes.

[0040] Preferably, the roughing speed is 2.0–2.5 m / s, for example, 2 m / s, 2.1 m / s, 2.2 m / s, 2.3 m / s, 2.4 m / s, or 2.5 m / s, and the finishing speed is 0.75–1.5 m / s, for example, 0.75 m / s, 0.80 m / s, 0.85 m / s, 0.90 m / s, 0.95 m / s, 1.00 m / s, 1.05 m / s, 1.10 m / s, 1.15 m / s, 1.20 m / s, 1.25 m / s, 1.30 m / s, 1.35 m / s, 1.40 m / s, 1.45 m / s, or 1.5 m / s.

[0041] This invention employs a semi-continuous rolling mill to form spherical flattened titanium. Pre-deformation of the titanium is achieved through rough rolling, followed by precise control of its dimensions using a high-precision continuous rolling mill. This invention, through the synergistic effect of electromagnetic induction heating and the semi-continuous rolling process, achieves efficient heating, high-precision rolling, and low-cost production. The resulting spherical flattened titanium exhibits excellent mechanical properties, with a finished product yield exceeding 95%, meeting the design and construction requirements of ships and marine equipment.

[0042] It should be noted that the blanks used in this invention are all existing titanium alloy grades, such as TA3, TA17, etc.

[0043] The heat treatment process of this invention is set according to the technical requirements of the titanium alloy grade; for example...

[0044] For titanium alloy of grade TA3, the heat treatment process involves annealing at 550–650℃ for 2–4 hours followed by air cooling in the furnace. The heat treatment process for other grades will be adjusted according to specific technical requirements.

[0045] In this invention, cooling is achieved by transporting the rolled billet to a cooling bed via roller conveyors; a straightening machine is used for straightening; and an automatic shot peening machine is used to clean the surface oxide scale of the spherical flat titanium to remove the surface oxide scale.

[0046] Specifically, the passivation treatment is acid washing, and preferably, the acid is Kroll reagent (volume fraction 1-3% HF + 2-6% HNO3 aqueous solution).

[0047] Preferably, the passivation treatment involves immersing the sample in an acid pickling tank for 15 to 60 minutes, for example, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, or 60 minutes, until the surface turns silvery-gray. After rinsing the acid solution with clean water, the sample is dried using a blower.

[0048] Another specific embodiment of the present invention discloses a spherical flat titanium profile for marine equipment prepared by the above method.

[0049] The technical solution of the present invention will be further explained below with reference to specific embodiments.

[0050] Example 1

[0051] The spherical flattened titanium prepared in this embodiment is grade TA3, and the dimensions of the spherical flattened titanium meet the requirements of type 8 in Table 4 of standard GJB8398-2015.

[0052] This embodiment describes a method for producing spherical flat titanium profiles for marine equipment, comprising the following steps:

[0053] Step 1: Select a round billet with a titanium alloy grade of TA3 as the billet material. The billet material has a size of Φ80×3000mm. Remove the surface oxide layer and impurities.

[0054] Step 2: The billet is subjected to electromagnetic induction heating, which includes sequential heating in a low-temperature section, a medium-temperature section, a high-temperature section, and a holding section. The roller frequency for electromagnetic induction heating is 25Hz. The current for the low-temperature section is 1500A, and the heating time is 4 minutes. The current for the medium-temperature section is 2300A, and the heating time is 8 minutes. The current for the high-temperature section is 2000A, and the heating time is 8 minutes. The current for the holding section is 1800A, and the heating time is 2.5 minutes. At this point, the surface temperature of the billet is 850–870℃. The heated billet is then rolled using a semi-continuous rolling mill, specifically a Φ400mm roughing mill and a Φ320mm finishing mill, with the following pass shapes: Figure 1 As shown, the billet passes through K10-K9-K8-K7-K6-K5-K4-K3-K2-K1 sequentially, with K10-K6 being rough rolling and K5-K1 being finish rolling. The rough rolling speed is approximately 2.2 m / s, and the finish rolling speed ranges from 1 m / s. After rolling, the spherical flat titanium is transported to a cooling bed via roller conveyors for cooling. A straightener is used to straighten the cooled spherical flat titanium. The macroscopic morphology of the rolled TA3 spherical flat titanium is shown in the attached figure. Figure 2 As shown;

[0055] Step 3: Anneal the straightened TA3 spherical flat titanium at a temperature of 580℃ for 3 hours, followed by air cooling in the furnace.

[0056] Step 4: Use a fully automatic shot peening machine to remove the oxide scale from the surface of the straightened TA3 spherical flat titanium to obtain a smooth surface;

[0057] Step 5: After shot peening, the spherical flat titanium is pickled and passivated. The solution is an aqueous solution of 3% HF + 6% HNO3 by volume. The material is immersed in the pickling tank for 40 minutes to obtain a silver-gray surface. After rinsing the pickling solution with clean water, it is dried with a blower to obtain the spherical flat titanium profile.

[0058] The microstructure of the spherical flattened titanium prepared in this embodiment is as follows: Figure 3-4 As shown, the microstructure is fine and equiaxed, which meets the requirements of TA3 microstructure control. The spherical flattened titanium prepared in this embodiment has a smooth surface, no cracks or inclusions, and meets the AA grade standard in ultrasonic testing.

[0059] Example 2

[0060] The production method of the spherical flat titanium profile for marine equipment in this embodiment is similar to that in embodiment 1, except that in step 2, the frequency of the electromagnetic induction heating roller is 20Hz, the current of the low-temperature section heating is 1000A and the heating time is 5min, the current of the medium-temperature section heating is 2000A and the heating time is 10min, the current of the high-temperature section heating is 1500A and the heating time is 10min, and the current of the heat preservation section heating is 1200A and the heating time is 3min.

[0061] Example 3

[0062] The production method of the spherical flat titanium profile for marine equipment in this embodiment is similar to that in embodiment 1, except that in step 2, the frequency of the electromagnetic induction heating roller is 28Hz, the current of the low-temperature section heating is 2000A and the heating time is 3min, the current of the medium-temperature section heating is 3000A and the heating time is 7.5min, the current of the high-temperature section heating is 2500A and the heating time is 7.5min, and the current of the heat preservation section heating is 2400A and the heating time is 2min.

[0063] Example 4

[0064] The spherical flattened titanium prepared in this embodiment is grade TA17, and the dimensions of the spherical flattened titanium meet the requirements of type 6 in Table 4 of standard GJB 8398-2015.

[0065] This embodiment describes a method for producing spherical flat titanium profiles for marine equipment, comprising the following steps:

[0066] Step 1: Select a round billet with a titanium alloy grade of TA17 as the billet material. The billet material has a size of Φ70×2500mm. Remove the surface oxide layer and impurities.

[0067] Step 2: The billet is subjected to electromagnetic induction heating, which includes sequential heating in a low-temperature section, a medium-temperature section, a high-temperature section, and a holding section. The roller frequency for electromagnetic induction heating is 20Hz. The current for the low-temperature section is 1800A, and the heating time is 4 minutes. The current for the medium-temperature section is 2500A, and the heating time is 8 minutes. The current for the high-temperature section is 2100A, and the heating time is 8 minutes. The current for the holding section is 2000A, and the heating time is 2.5 minutes. At this point, the surface temperature of the billet is 890–920℃. The heated billet is then rolled using a semi-continuous rolling mill, specifically a Φ400mm roughing mill and a Φ320mm finishing mill, with the following pass shapes: Figure 1As shown, the billet passes through K10-K9-K8-K7-K6-K5-K4-K3-K2-K1 sequentially, with K10-K6 being rough rolling and K5-K1 being finish rolling. The rough rolling speed is approximately 2.0 m / s, and the finish rolling speed ranges from 1.5 m / s. After rolling, the flattened titanium spherical is transported to a cooling bed via roller conveyors for cooling, and then straightened using a straightener.

[0068] Step 3: Anneal the straightened TA17 spherical flat titanium at a temperature of 820℃ for 2 hours, followed by air cooling in the furnace.

[0069] Step 4: Use a fully automatic shot peening machine to remove the oxide scale from the surface of the straightened TA17 spherical flat titanium to obtain a smooth surface;

[0070] Step 5: After shot peening, the spherical flat titanium is pickled and passivated. The solution is an aqueous solution of 2% HF + 4% HNO3 by volume. The titanium is immersed in the pickling tank for 60 minutes to obtain a silver-gray surface. After rinsing the pickling solution with clean water, the titanium is dried with a blower to obtain the spherical flat titanium profile.

[0071] The spherical flattened titanium prepared in this embodiment has a smooth surface, is free of cracks and inclusions, and meets the AA-level standard in ultrasonic testing.

[0072] Example 5

[0073] The production method of the spherical flat titanium profile for marine equipment in this embodiment is similar to that in embodiment 4, except that in step 1, the rough rolling speed is 2.5 m / s and the finish rolling speed is 0.75 m / s.

[0074] Comparative Example 1

[0075] The production method of the spherical flat titanium profile for marine equipment in this comparative example is similar to that in Example 1, except that the electromagnetic induction heating in step (2) is replaced by box furnace heating, and the billet surface temperature is heated to 850-870°C.

[0076] Comparative Example 2

[0077] The production method of the spherical flat titanium profile for marine equipment in this comparative example is similar to that in Example 1, except that in step (2), electromagnetic induction heating is only used at medium temperature, that is, segmented heating is not used, and the billet surface temperature is heated to 850-870℃.

[0078] Comparative Example 3

[0079] The production method of the spherical flat titanium profile for marine equipment in this comparative example is similar to that in Example 4, except that the heating current in the low-temperature section in step (2) is 800A.

[0080] Comparative Example 4

[0081] The production method of the spherical flat titanium profile for marine equipment in this comparative example is similar to that in Example 4, except that the heating current in the high-temperature section in step (2) is 3000A.

[0082] Comparative Example 5

[0083] The production method of the spherical flat titanium profile for marine equipment in this comparative example is similar to that in Example 1, except that the frequency of electromagnetic induction heating in step (1) is 15Hz.

[0084] Experimental Example 1

[0085] Ultrasonic flaw detection and mechanical property testing were performed on the spherical flattened titanium for marine equipment prepared in the examples and comparative examples, respectively. The results are shown in Table 1.

[0086] Table 1

[0087]

[0088]

[0089] As shown in Table 1, the TA3 spherical flat titanium profiles produced by the method of this invention have the following tensile strengths: head: 572–607 MPa; yield strength: 452–495 MPa; elongation after fracture: 23.0–25.5%; reduction of area: 44–47%; room temperature impact resistance: 41–52 J. Tail: tensile strength: 577–612 MPa; yield strength: 457–497 MPa; elongation after fracture: 23.5–26.5%; reduction of area: 41–50%; room temperature impact resistance: 42–55 J. The yield of the TA3 spherical flat titanium profiles is ≥98%, the ultrasonic flaw detection grade is AA, and the surface is free of pits and roughness.

[0090] The TA17 spherical flat titanium profiles produced by the method of this invention have a tensile strength of 724–759 MPa, a yield strength of 651–676 MPa, an elongation after fracture of 15.0–17.0%, a reduction of area of ​​41–45%, and a room temperature impact resistance of 70–77 J. The tail section has a tensile strength of 726–765 MPa, a yield strength of 648–689 MPa, an elongation after fracture of 15.5–18.5%, a reduction of area of ​​40–45%, and a room temperature impact resistance of 63–92 J. The finished product yield of the TA17 spherical flat titanium profiles is ≥99%, the ultrasonic flaw detection grade is AA, and the surface is free of pits and roughness.

[0091] In summary, the method of this invention yields spherical flat titanium products that meet the technical requirements of the corresponding grades, exhibiting good matching of strength, plasticity, and toughness, a finished product yield exceeding 98%, an ultrasonic flaw detection rating of AA, and a surface free of pits and roughness. Overall, the production method of this invention offers advantages such as high-precision rolling, low-cost production, excellent comprehensive performance, and high yield.

[0092] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for producing spherical flat titanium profiles for marine equipment, characterized in that, The method includes heating the titanium alloy billet using electromagnetic induction heating; The electromagnetic induction heating includes sequentially performing low-temperature heating, medium-temperature heating, high-temperature heating, and heat preservation heating. The frequency of the electromagnetic induction heating is 20-28Hz. The current for the low-temperature heating is 1000-2000A, the current for the medium-temperature heating is 2000-3000A, the current for the high-temperature heating is 1500-2500A, and the current for the heat preservation heating is 1200-2400A.

2. The production method according to claim 1, characterized in that, The heating time for the low-temperature section is 3-5 minutes, the heating time for the medium-temperature section is 7.5-10 minutes, the heating time for the high-temperature section is 7.5-10 minutes, and the heating time for the heat preservation section is 2-3 minutes.

3. The production method according to claim 1, characterized in that, The titanium alloy billet is a round billet with dimensions of 70-90mm × 2500-3500mm.

4. The production method according to any one of claims 1-3, characterized in that, The electromagnetic induction heating is carried out to a surface temperature of 800-1200℃ for the billet.

5. The production method according to any one of claims 1-3, characterized in that, The method further includes sequentially rolling, cooling, straightening, heat treatment, shot peening, and passivation of the billet after electromagnetic induction heating treatment to obtain the spherical flat titanium profile.

6. The production method according to claim 5, characterized in that, The rolling process involves 10 passes, including roughing and finishing rolling.

7. The production method according to claim 6, characterized in that, The roughing speed is 2.0 to 2.5 m / s, and the finishing speed is 0.75 to 1.5 m / s.

8. The production method according to claim 6, characterized in that, The passivation treatment is acid washing.

9. The production method according to claim 6, characterized in that, The passivation treatment involves immersing the food in an acid pickling tank for 15–60 minutes.

10. A spherical flat titanium profile for marine equipment obtained by the production method according to any one of claims 1-9.

Citation Information

Patent Citations

  • Extrusion preparation process of pure titanium flat-bulb profile

    CN116689534A

  • Method for improving uniformity of radial tissue of heat-resisting alloy thick-walled extrusion pipe

    CN103938134A

  • Titanium and titanium alloy flat blank machining method

    CN115672973A

  • Production method of flat-bulb titanium alloy profile

    CN117324370A

  • Plate shape control method for TC4ELI titanium alloy medium-thickness plate with thickness larger than 50 mm