Self-repairing bio-based coating material giving consideration to nutrient controlled release and membrane shell degradation and preparation method of self-repairing bio-based coating material

By reacting easily degradable polyester polyols with crosslinking promoters and functional chain extenders, a triblock structure self-healing bio-based coating material is formed, which solves the problems of poor toughness and slow degradation of bio-based coated controlled-release fertilizers, and achieves stable nutrient release and efficient membrane degradation.

CN121378658AActive Publication Date: 2026-01-23SHANDONG AGRICULTURAL UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202511609537.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-05
Publication Date
2026-01-23
Estimated Expiration
2045-11-05

AI Technical Summary

Technical Problem

Existing bio-based coated controlled-release fertilizers suffer from poor membrane toughness and low strength, making them prone to damage and nutrient leakage. Furthermore, the membrane shell degrades slowly after nutrient release, leading to soil ecology and environmental pollution problems.

Method used

A self-healing bio-based coating material with a triblock structure was constructed by reacting easily degradable polyester polyols with crosslinking promoters and functional chain extenders. This improved the toughness and degradation efficiency of the membrane shell and enabled the membrane shell to self-repair and release stable nutrients through dynamic covalent bonds and hydrogen bonds.

Benefits of technology

It improves the toughness and strength of the membrane shell, ensures the stability of nutrient release, and rapidly degrades after complete nutrient release, resulting in high degradation efficiency and solving the problem of membrane shell accumulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121378658A_ABST
    Figure CN121378658A_ABST
Patent Text Reader

Abstract

The invention discloses a self-repairing bio-based coating material giving consideration to nutrient controlled release and membrane shell degradation and a preparation method of the self-repairing bio-based coating material, and belongs to the technical field of controlled release fertilizer production. The self-repairing bio-based coating material is prepared from the following raw materials in parts by weight: 80 to 100 parts of easily degradable polyester polyol, 30 to 50 parts of cross-linking promoting agent and 10 to 20 parts of functional chain extender. According to the self-repairing bio-based coating material and the preparation method thereof, the easily degradable polyester polyol reacts with the cross-linking promoting agent and the functional chain extender to synthesize the self-repairing bio-based coating material which gives consideration to nutrient controlled release and membrane shell degradation, and the self-repairing bio-based coating material can improve the toughness of a membrane material, promote rapid repairing of a damaged area and improve the service life of the membrane material. The stability of nutrient release is improved; in addition, a chain reaction of structural fracture can be triggered in the membrane material degradation process, and the degradation rate of a membrane shell after nutrients are completely released is increased. The invention effectively solves the problem that the degradation performance of the membrane shell and the controlled release performance of nutrients are difficult to coexist.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of controlled-release fertilizer production, in particular to a self-repairing bio-based coating material considering nutrient controlled release and film shell degradation and a preparation method thereof. BACKGROUND

[0002] Bio-based coated controlled-release fertilizer has the characteristics of slow release of nutrients, which can significantly improve nutrient utilization rate. However, bio-based coated controlled-release fertilizer has the following problems, which restrict the progress and development of the industry: (1) The bio-based film material has poor toughness and low strength, and is easily damaged by external influences, resulting in nutrient leakage and reducing nutrient controlled release efficiency. In the large-scale production process of controlled-release fertilizer, the friction between fertilizer-fertilizer and fertilizer-equipment causes damage.

[0003] (2) It is difficult to achieve stable controlled release performance and excellent degradation performance. After the release of many controlled-release fertilizers, the film shell cannot be effectively degraded in a short time, and microplastics are easily produced in the slow degradation process, which exist in the soil for a long time and harm the soil ecology and human health.

[0004] In order to solve the above problems of coated controlled-release fertilizer, the related patent CN119263918A discloses a yield-increasing functional full-biodegradable controlled-release fertilizer and a preparation method thereof, which obtains a film coating material with yield-increasing and excellent degradation functions by reacting carrier-functional material slow-release complex, full-biodegradable resin and solvent. The principle is to cross-link into easily degradable resin in the reaction system, which promotes the degradation effect in the environment. Although this degradation effect is green and pollution-free, the bio-based film shell prepared by this material has strong hydrophilicity, which will cause the controlled release performance to decrease. The related patent CN118271131A discloses a self-repairing modified lignin-based polyester polyol coating material and a preparation method thereof, which prepares a lignin-based coated fertilizer with self-repairing function by gradually reacting lignin polyester polyol, accelerant and self-repairing adhesive. The principle is to embed dynamic covalent bonds in the polyurethane network, which prolongs the molecular chain and improves the molecular migration. This technology can improve the toughness and strength of the film material, but cannot achieve effective degradation of the film shell after nutrient release. The related patent CN114621415A discloses a two-component polyol degradable polyurethane coated controlled-release fertilizer and a preparation method and application thereof, which synthesizes a degradable bio-based polyurethane film by reacting polyester polyol, biomass polyol and curing agent. The principle is to modify the cross-linking of polyester polyol and liquefied biomass polyol, which optimizes the reaction structure arrangement and promotes the structure batch degradation effect. Although degradation is achieved under the condition of ensuring controlled release performance, the degradation efficiency is realized in three steps, and the actual degradation effect is poor. SUMMARY

[0005] In view of the problems existing in the prior art, the present application aims to provide a self-repairing bio-based coating material with nutrient controlled release and film shell degradation and a preparation method thereof.

[0006] To achieve the above-mentioned object, the present application adopts the following technical solutions: In a first aspect, the present application provides a self-repairing bio-based coating material with nutrient controlled release and film shell degradation, comprising the following raw materials by weight: 80-100 parts of easily degradable polyester polyol, 30-50 parts of cross-linking promoter, and 10-20 parts of functional chain extender; The functional chain extender is obtained by blending the first component and the second component in a molar ratio of 1:(1-3); the first component is one or more of thiamine disulfide, captopril disulfide, and 2-chloro-2-(hydroxyimino) ethyl acetate; and the second component is one or more of polytetrahydrofuran, polycarbonate diol, and polycaprolactone diol.

[0007] Preferably, the easily degradable polyester polyol is obtained by reacting the A component and the B component in a molar ratio of (0.5-1.5):(0.5-1.5); the A component is one or more of aspartic acid, glutamic acid, and lysine; and the B component is one or more of soybean oil polyol and flaxseed oil polyol.

[0008] Preferably, the cross-linking promoter is selected from one or more of m-xylylene diisocyanate, 4-chloro-6-methyl-m-phenylene diisocyanate, and 2,4-difluorophenyl isocyanate.

[0009] In some preferred embodiments of the present application, the reaction conditions of the easily degradable polyester polyol are as follows: After mixing the A component and the B component, p-toluenesulfonic acid and toluene are added, and the temperature is raised to 140-160℃ under nitrogen protection, and the reaction is carried out for 6-8h; and the temperature is cooled to 80℃, and the reaction is carried out for 20-40min.

[0010] In some preferred embodiments of the present application, the blending conditions of the functional chain extender are as follows: The first component is mixed with the vacuum-dried second component, and the reaction is continuously stirred at 40-60℃ for 20-40min.

[0011] In a second aspect, the present application provides a preparation method of the self-repairing bio-based coating material with nutrient controlled release and film shell degradation, comprising the following steps: The easily degradable polyester polyol is added into an organic solvent, and stirred until the solution is uniform, and then the functional chain extender is added, and the reaction is continuously stirred at 40-50℃ under nitrogen protection for 0.5-1.5h to generate an intermediate; The intermediate is added into the cross-linking promoter, and after dropping dibutyltin dilaurate, it is quickly stirred until a large amount of bubbles are generated, an organic solvent is added, then nitrogen is introduced, and the mixed solution is vacuum dried, and the self-repairing bio-based coating material is prepared after the bubbles disappear.

[0012] Preferably, the organic solvent is N,N dimethylformamide or acetone.

[0013] In a third aspect of the present application, the self-repairing bio-based coating material with the functions of nutrient controlled release and film shell degradation is applied to the preparation of controlled release fertilizer.

[0014] In a fourth aspect of the present application, a film-coated controlled release fertilizer is provided, which comprises a fertilizer core and the self-repairing bio-based coating material with the functions of nutrient controlled release and film shell degradation sprayed on the surface of the fertilizer core.

[0015] Preferably, the spraying amount of the self-repairing bio-based coating material with the functions of nutrient controlled release and film shell degradation accounts for 1-5% of the weight of the fertilizer core.

[0016] The present application has the following advantages: (1) The present application improves the toughness and elasticity of the bio-based film shell, solves the problem of fertilizer damage caused by the friction between the fertilizer and the equipment during the production and transportation of the controlled release fertilizer, and ensures the stability of nutrient release.

[0017] (2) The present application coordinates the problems of nutrient release and film shell degradation, the covalent bond is not fully soaked by water in a short time, and the degradation efficiency is low, which ensures the stable nutrient release at this time, and after the complete release of nutrients, the covalent bond is fully soaked by water, starts to hydrolyze, and the film shell starts to degrade; the degradation rate of the bio-based film shell of the present application can reach about 50% in 180 days, and the degradation speed is fast and the degradation efficiency is high.

[0018] In summary, the present application synthesizes a self-repairing bio-based coating material with the functions of nutrient controlled release and film shell degradation by synthesizing easily degradable polyester polyol from easily degradable amino acid and plant oil polyol, and then reacting with cross-linking promoter, degradation-promoting chain extender and curing agent. The film material structure has excellent molecular migration property, and the easily degradable chemical bond and amino acid structure are all on the reaction sites of the components. This structure not only improves the toughness of the film material and promotes the rapid repair of the damaged area, but more importantly, the degradation process triggers a chain reaction of structure rupture, improves the degradation efficiency, improves the stability of nutrient release and the degradation rate of the film shell after complete release of nutrients. BRIEF DESCRIPTION OF DRAWINGS

[0019] Figure 1 The Fourier infrared spectrum detection results of the self-repairing bio-based coating materials prepared in Examples 1-3 of the present application.

[0020] Figure 2 Results of mechanical property detection of the bio-based coating material prepared in Example 1 and Comparative Example 1 of the present application.

[0021] Figure 3 Results of complete release of the bio-based coated controlled-release fertilizer prepared in Example 4 and Comparative Example 1 of the present application, and weight change after absorbing moisture.

[0022] Figure 4 Results of volume change of the bio-based coated controlled-release fertilizer prepared in Example 4 and Comparative Example 1 of the present application after absorbing moisture.

[0023] Figure 5 Surface images of the polyurethane coating layer observed under a scanning electron microscope (SEM) after 180 days of degradation of the film shell of Example 1 and conventional bio-based fertilizer.

[0024] Figure 6 Results of weight loss rate of the film shell of Comparative Examples 1-3 and Example 4 of the present application.

[0025] Figure 7 Nutrient release curves of the coated controlled-release fertilizer prepared in Examples 4-6 and Comparative Examples 1-3 of the present application.

[0026] Figure 8 Nutrient release curves of the coated controlled-release fertilizer prepared in Example 4 and Comparative Example 1 of the present application before and after damage. DETAILED DESCRIPTION

[0027] It should be noted that the following detailed description is exemplary and is intended to provide further explanation of the present application. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present application belongs.

[0028] As described previously, some agricultural wastes can be synthesized into bio-based raw materials through liquefaction, purification, etc., for preparing bio-based controlled-release fertilizers, which have the advantages of low cost and wide sources, etc. However, the film shells prepared from these bio-based materials have poor toughness and low strength, which leads to unstable nutrient release, affecting the matching degree of nutrient release and crop fertilizer requirement and the nutrient utilization rate. Moreover, after complete release of nutrients, the film shell has a slow degradation rate, causing accumulation of the film shell in the soil and affecting the ecological environment.

[0029] In view of this, the present application develops a self-repairing biological coating material which takes into account nutrient controlled release and film shell degradation, the present application constructs a brand new three-block structure, crosslinks the easily degradable molecular structure to the reaction sites of each component through reaction, improves the degradation efficiency, solves the problems of difficult and slow film shell degradation at present, and relieves the soil environmental pressure; crosslinking the functional chain extender into the structure can improve the molecular migration efficiency and exchange capacity, increase the toughness and strength of the film material, and has the function of repairing the damaged area, solves the problem of nutrient release in advance caused by film shell damage, and improves the nutrient utilization rate.

[0030] The self-repairing biological coating material which takes into account nutrient controlled release and film shell degradation of the present application is prepared by reaction of easily degradable polyester polyol, crosslinking agent and functional chain extender. In an embodiment of the present application, the preparation method of the self-repairing biological coating material which takes into account nutrient controlled release and film shell degradation is given, which is as follows: The easily degradable polyester polyol is added to an organic solvent and stirred until the solution is uniform, then it is added to a three-necked flask, then the functional chain extender is added, a magnetic stirrer is connected, nitrogen is introduced to remove air, and stirring is continued at 45 DEG C for 1 h to generate an intermediate; The intermediate is added to the crosslinking agent, then dibutyltin dilaurate is added dropwise, and then rapid stirring is carried out until a large number of bubbles are generated, then an organic solvent is added, then nitrogen is introduced, and then slow stirring is carried out for 3-5 min, then the mixed solution is placed in a vacuum drying box, vacuum drying is carried out at 30 DEG C for 5 min, and then the self-repairing biological coating material which takes into account nutrient controlled release and film shell degradation is prepared after the bubbles disappear.

[0031] The coating material of the present application has high strength, high elasticity, stable nutrient release rate and excellent degradation performance, and the action mechanism of the coating material of the present application is as follows: The first component in the functional chain extender is mainly to provide dynamic covalent bonds. The migration and recombination of the broken dynamic covalent bonds caused by membrane shell damage are important factors to determine the repair effect. The second component belongs to a low molecular weight dihydric alcohol. Compared with the high molecular weight polyester polyol, the crosslinking density is relatively low. The addition of the second component is beneficial to improve the migration rate of the molecular chain (the repair effect is closely related to the molecular migration rate). After the first component and the second component of the functional chain extender are blended in an organic solvent, the functional small molecule substances (dynamic covalent bonds) are uniformly distributed in the solution. After the functional chain extender is added to the easily degradable polyester polyol, the uniformity of the functional small molecule substances is further improved, and a viscous intermediate is generated. During the reaction of the intermediate with the crosslinking promoter, due to electrostatic attraction, the easily degradable amino acid structure, ester group structure and functional small molecule structure on both sides are attracted by the crosslinking promoter, forming a three-block bridge structure. This structure not only effectively ensures the uniform distribution of the functional small molecules in the entire network structure, but also ensures that the easily degradable bonds are located at the reaction sites of the network structure. When the bonds are broken, the overall structure is decomposed, significantly improving the degradation efficiency.

[0032] The membrane shell repair process mainly focuses on the production, transportation and application processes. These three processes are easily affected by the external environment, which can damage the controlled-release membrane. The repair function mainly acts in these three stages. The dynamic covalent bonds and hydrogen bonds in the network structure of the damaged membrane shell will be broken due to the structural damage. However, the dynamic covalent bonds and hydrogen bonds can spontaneously recombine, which gradually restores the broken network structure and promotes the self-repair of the damaged membrane shell.

[0033] After the fertilizer is applied to the soil, the dynamic disulfide bond is very sensitive and is easily attacked by microorganisms and some enzymes in the soil. After being attacked, the dynamic disulfide bond is broken or even decomposed. After the nutrient release is completed, the process gradually becomes faster. The breaking of the dynamic disulfide bond promotes the breaking of the entire network structure, thereby promoting the degradation.

[0034] In summary, in view of the problems of poor membrane shell toughness, low strength, slow degradation, and poor degradation effect of the existing bio-based coated controlled-release fertilizer in large-scale application, the application originally synthesizes an easily degradable polyester polyol and originally adds a functional chain extender to the coating material. The added functional chain extender not only has the ability to repair the damaged area of the membrane shell, but also significantly enhances the strength of the fertilizer. More importantly, the functional small molecules provided by the functional chain extender also have the property of easy degradation. During the degradation process of the bio-based membrane shell, the functional chain extender and the easily degradable polyester polyol have a synergistic effect. The functional chain extender and the easily degradable polyester polyol react with the crosslinking promoter to construct a new three-block bridge structure, which significantly improves the damage resistance, toughness and elasticity of the bio-based membrane shell while ensuring excellent degradation ability.

[0035] In order for those skilled in the art to more clearly understand the technical solutions of the present application, the technical solutions of the present application will be described in detail below in conjunction with specific examples.

[0036] The test materials used in the examples and comparative examples of the present application are all conventional test materials in the art and can be purchased through commercial channels. Among them: Soybean oil polyol is purchased from Guangzhou Hailuoma Vegetable Oil and Fat Co., Ltd., and flaxseed oil polyol is purchased from Jiangxi Xinsen Natural Plant Oil Co., Ltd.

[0037] Thiamine disulfide: 67-16-3; Captopril disulfide: 64806-05-9; Ethyl 2-chloro-2-(hydroxyimino)acetate: 14337-43-0; Polytetrahydrofuran: 25190-06-1; Polycarbonate diol: 24937-06-2; Polycaprolactone diol: 36890-68-3.

[0038] Example 1: Preparation of self-repairing bio-based coating material considering nutrient controlled release and shell degradation (1) Preparation of easily degradable polyester polyol: Take aspartic acid as component A; soybean oil polyol as component B; Put 6.65 g of component A and 50 g of component B into a three-necked flask in turn, add 0.57 g of p-toluenesulfonic acid, connect a mechanical stirrer, a nitrogen protection system and a water separator, then add 50 ml of toluene for azeotropy, start the mechanical stirring, heat to 140℃, the nitrogen flow rate is 20 ml / min, maintain reflux reaction for 8 hours, after stopping heating, cool to 80℃, transfer the mixed solution to a rotary evaporator, react at 80℃ for 30 min, and obtain the easily degradable polyester polyol, which is stored in a sealed manner.

[0039] (2) Preparation of functional chain extender: Take thiamine disulfide as the first component; polytetrahydrofuran as the second component; Put 5.62 g of the first component into a beaker, add 10 ml of N,N dimethylformamide; put 20 g of the second component into a beaker, then place it in a vacuum drying oven, dry at 80℃ for half an hour, then add it into the first component, continuously stir at 50℃ for 30 min, stop stirring until the mixed solution is uniform, and obtain the functional chain extender.

[0040] (3) Preparation of coating material: Take 8 g of the easily degradable polyester polyol synthesized in step (1) into a beaker, add 3 ml of acetone, stir until the solution is uniform, transfer it into a three-necked flask, then add 1 g of the functional chain extender synthesized in step (2), connect a magnetic stirrer, introduce nitrogen to remove air, and continuously stir at 45℃ for 1 h to generate an intermediate; To the intermediate, 3 g of crosslinking promoter (m-xylylene diisocyanate) was added, 1 drop of dibutyltin dilaurate was added, and rapid stirring was performed until a large number of bubbles were generated. Then, 3 ml of acetone was added, followed by nitrogen gas blowing. The mixed solution was placed in a vacuum drying box and dried at 30°C for 5 min. After the bubbles disappeared, the self-repairing bio-based coating material with nutrient controlled release and shell degradation was prepared.

[0041] Example 2: Preparation of self-repairing bio-based coating material with nutrient controlled release and shell degradation (1) Preparation of easily degradable polyester polyol: Glutamic acid was used as component A, and soybean oil polyol was used as component B. 7.35 g of component A and 50 g of component B were sequentially placed in a three-necked flask, 0.57 g of p-toluenesulfonic acid was added, a mechanical stirrer, a nitrogen protection system and a water separator were connected, 50 ml of toluene was added for azeotropy, the mechanical stirring was started, the temperature was raised to 150°C, the nitrogen flow rate was 20 ml / min, and the reflux reaction was maintained for 7 hours. After stopping heating, the mixed solution was transferred to a rotary evaporator and reacted at 80°C for 30 min to obtain the easily degradable polyester polyol, which was sealed and stored.

[0042] (2) Preparation of functional chain extender: Captopril disulfide was used as the first component, and polycarbonate diol was used as the second component. 8.64 g of the first component was placed in a beaker, 10 ml of N,N-dimethylformamide was added, 20 g of the second component was placed in a beaker, and then placed in a vacuum drying box and dried at 80°C for half an hour. Then, it was added to the first component, and stirring was continued at 50°C for 30 min until the mixed solution became uniform. Then, the stirring was stopped to obtain the functional chain extender.

[0043] (3) Preparation of coating material: 9 g of the easily degradable polyester polyol synthesized in step (1) was taken in a beaker, 3 ml of acetone was added, and stirring was performed until the solution was uniform. Then, it was transferred into a three-necked flask, 1.5 g of the functional chain extender synthesized in step (2) was added, a magnetic stirrer was connected, nitrogen was blown to remove air, and stirring was continued at 45°C for 1 h to generate an intermediate. To the intermediate, 4 g of crosslinking promoter (4-chloro-6-methyl-m-phenylene diisocyanate) was added, 1 drop of dibutyltin dilaurate was added, and rapid stirring was performed until a large number of bubbles were generated. Then, 4 ml of acetone was added, followed by nitrogen gas blowing. The mixed solution was placed in a vacuum drying box and dried at 30°C for 5 min. After the bubbles disappeared, the self-repairing bio-based coating material with nutrient controlled release and shell degradation was prepared.

[0044] Example 3: Preparation of a self-healing bio-based coating material that combines nutrient controlled release and membrane degradation (1) Preparation of easily degradable polyester polyols: Lysine is used as component A; soybean oil polyols are used as component B. 7.3g of component A and 50g of component B were placed in a three-necked flask, and 0.57g of p-toluenesulfonic acid was added. A mechanical stirrer, a nitrogen protection system, and a water separator were connected, and then 50ml of toluene was added for azeotroping. The mechanical stirrer was started, and the temperature was raised to 160℃. The nitrogen flow rate was 20ml / min, and the reaction was maintained under reflux for 6 hours. After heating was stopped, the mixture was cooled to 80℃, and the mixture was transferred to a rotary evaporator and reacted at 80℃ for 30 minutes to obtain a biodegradable polyester polyol, which was then sealed and stored.

[0045] (2) Preparation of functional chain extenders: Ethyl 2-chloro-2-(oxime)ethyl acetate was used as the first component; polycaprolactone diol was used as the second component. Place 4.5g of the first component in a beaker, add 10ml of N,N-dimethylformamide, place 20g of the second component in a beaker, and then place the beaker in a vacuum drying oven. After drying at 80℃ for half an hour, add the second component to the first component and stir continuously at 50℃ for 30 minutes until the mixture becomes homogeneous. Stop stirring to obtain the functional chain extender.

[0046] (3) Preparation of coating materials: Take 10g of the biodegradable polyester polyol synthesized in step (1) into a beaker, add 3ml of acetone, stir until the solution is uniform, transfer it into a three-necked flask, add 2g of the functional chain extender synthesized in step (2), connect a magnetic stirrer, purge with nitrogen to remove air, and stir continuously at 45℃ for 1h to generate an intermediate. Add 5g of crosslinking agent (2,4-difluorophenyl isocyanate) to the intermediate, add 1 drop of dibutyltin dilaurate, stir rapidly until a large number of bubbles are generated, add 5ml of acetone, then purge with nitrogen gas, stir slowly for 5min, place the mixed solution in a vacuum drying oven, and vacuum dry at 30℃ for 5min. After the bubbles disappear, a self-healing bio-based coating material that combines nutrient controlled release and membrane degradation is obtained.

[0047] Example 4: Preparation of Coated Controlled-Release Fertilizer Take 2000g of polished urea granules and put them into a coating pan at 45℃. Keep the coating pan rotating at 10 rpm. Use a spray gun to spray the self-healing bio-based coating material prepared in Example 1, which combines nutrient control and membrane degradation, onto the surface of the rolling urea granules. Let it cure for 5 minutes. Each spraying amount is 0.5% of the fertilizer mass. Repeat the above spraying operation until the weight of the coating liquid accounts for 2.5% of the total weight of the urea granules, and the coated controlled-release fertilizer is obtained.

[0048] Example 5: Preparation of Coated Controlled-Release Fertilizer Take 2000g of polished urea granules and put them into a coating pan at 45℃. Keep the coating pan rotating at 12 rpm. Use a spray gun to spray the self-healing bio-based coating material prepared in Example 2, which combines nutrient control and membrane degradation, onto the surface of the rolling urea granules. Let it cure for 5 minutes. Each spraying amount is 0.5% of the fertilizer mass. Repeat the above spraying operation until the weight of the coating liquid accounts for 3% of the total weight of the urea granules, and the coated controlled-release fertilizer is obtained.

[0049] Example 6: Preparation of Coated Controlled-Release Fertilizer Take 2000g of polished urea granules and put them into a coating pan at 45℃. Keep the coating pan rotating at 15 rpm. Use a spray gun to spray the self-healing bio-based coating material prepared in Example 3, which combines nutrient control and membrane degradation, onto the surface of the rolling urea granules. Let it cure for 5 minutes. Each spraying amount is 0.5% of the fertilizer mass. Repeat the above spraying operation until the weight of the coating liquid accounts for 3.5% of the total weight of the urea granules, and the coated controlled-release fertilizer is obtained.

[0050] Comparative Example 1: Preparation of Conventional Bio-based Fertilizers (1) Take 8g of soybean oil polyol and 3g of m-phenylenedimethyl diisocyanate and mix them evenly at room temperature. Continue stirring until the solution turns white and then stop stirring to obtain a bio-based coating solution.

[0051] (2) Take 2000g of polished urea granules and put them into a coating pan at 65℃. Keep the coating pan speed at 20rps. After preheating, use a spray gun to spray the bio-based coating liquid prepared in step (1) onto the surface of the rolling urea granules. Let it solidify for 12min. Each spraying amount is 0.5% of the fertilizer mass. Repeat the above spraying operation until the weight of the coating liquid accounts for 2.5% of the total weight of the urea granules, and then the conventional bio-based fertilizer is obtained.

[0052] Comparative Example 2: The preparation method of the biodegradable polyester polyol is the same as that in Example 1, except that only thiamine disulfide is used as a functional chain extender; the coating material is prepared according to the method in Example 1.

[0053] Following the coating treatment conditions of Example 4, coated controlled-release fertilizer A was prepared.

[0054] Comparative Example 2: The preparation method of the biodegradable polyester polyol is the same as that in Example 1, except that only polytetrahydrofuran is used as a functional chain extender; the coating material is prepared according to the method in Example 1.

[0055] Following the coating treatment conditions of Example 4, coated controlled-release fertilizer B was prepared.

[0056] Experimental Example 1: The self-healing bio-based coating materials prepared in Examples 1-3 were cured to form a membrane shell. Fourier transform infrared spectroscopy was used to detect changes in characteristic functional groups within the membrane shell, and the results are as follows: Figure 1 As shown, the two characteristic peaks of polyurethane, NH group and C=O group, appear, while -NCO group completely disappears, indicating that the polyurethane coating has been formed.

[0057] Tensile tests were conducted on the membrane shell formed by the curing of the self-healing bio-based coating material prepared in Example 1 using a universal testing machine, with a tensile rate of 200 mm / s; the membrane shell formed by the curing of the bio-based coating solution in Comparative Example 1 was used as a control. The results are as follows: Figure 2 As shown, the tensile strength of the coating material prepared by the present invention can be above 700% without breaking, indicating that the self-healing bio-based coating material prepared by the present invention has good tensile properties and elasticity.

[0058] Experimental Example 2: 1. Flexibility Assessment: The absorbed weight and expansion volume of the coating are measured to assess its integrity and resilience. Specifically: The coated controlled-release fertilizers prepared in Example 4 and Comparative Example 1 were labeled, and the initial weight and volume of the coated controlled-release fertilizers were measured. Then, the labeled coated controlled-release fertilizers were immersed in water, and the weight and volume of the coated controlled-release fertilizers were measured again after 45 days. The weight increment and volume increment of the coated controlled-release fertilizers were calculated.

[0059] The results are as follows Figure 3 and Figure 4 As shown, the results indicated that, after 45 days of nitrogen release, the conventional bio-based fertilizer in Comparative Example 1 increased in weight by 8.9 mg and in volume by 19.24 mm. 3 During the same release period, the weight of the coated controlled-release fertilizer in Example 4 increased by 46.67 mg, and its volume increased by 41.66 mm. 3 The increase in weight and volume of Comparative Example 1 after absorbing water and swelling was greater than that of conventional bio-based coated fertilizers. This indicates that the coating material of the controlled-release fertilizer in Example 4 has better elasticity.

[0060] 2. Degradation performance evaluation The membrane shells of the coated controlled-release fertilizers prepared in Comparative Examples 1-3 and Example 4 were separated from the fertilizer granules, thoroughly washed, and air-dried. The dried membrane shells were then placed in mesh bags and buried 10 cm deep in farmland soil (Linyi, China; November 2024). Samples were taken at 30, 60, 90, 120, and 180 days after each treatment.

[0061] The membrane morphology of the conventional bio-based fertilizer in Comparative Example 1 and the coated controlled-release fertilizer in Example 4 after 180 days of degradation was captured using SEM. The results are as follows: Figure 5 As shown in the figure. The results show that the membrane shell of the coated controlled-release fertilizer in Example 4 has a more significant degradation effect.

[0062] The degradation rate of the membrane shell was calculated using weight loss, and the results are as follows: Figure 6 As shown in the figure. The results show that the membrane shell of Example 4 achieved a degradation rate of nearly 50% after 180 days, which is more than three times that of conventional bio-based fertilizers.

[0063] 3. Nutrient release assay: The nitrogen release rates of conventional bio-based fertilizers, as well as the coated controlled-release fertilizers prepared in Examples 4, 5, and 6 and Comparative Examples 1-3, were determined according to the National Standard for Slow-Release Fertilizers of the People's Republic of China GB / T 23348-2009.

[0064] The results are as follows Figure 7 As shown, the release period of conventional bio-based fertilizer is 37 days; the release period of bio-based coated fertilizer in Example 4 is 55 days; the release period of bio-based coated fertilizer in Example 5 is 64 days; the release period of bio-based coated fertilizer in Example 6 is 88 days; the release period of bio-based coated fertilizer in Comparative Example 2 is 42 days; and the release period of bio-based coated fertilizer in Comparative Example 3 is 44 days.

[0065] 4. Self-healing performance test: The coated controlled-release fertilizer granules prepared in Example 4 and Comparative Example 1 were completely punctured with a needle and left at room temperature for 24 hours. Then, 10g of the damaged fertilizer was placed in 200ml of water to test its nitrogen release rate. The coated controlled-release fertilizers prepared in Example 4 and Comparative Example 1 without puncture damage treatment were used as controls.

[0066] The results are as follows Figure 8 As shown in the figure. The results show that: after being punctured, the nutrient release of the coated controlled-release fertilizer in Comparative Example 1 was accelerated, indicating that it does not have self-repairing properties; while the nutrient release of the coated controlled-release fertilizer prepared in Example 4 was basically the same as that of the unpunctured fertilizer after being punctured, proving that the coated controlled-release fertilizer of the present invention has self-repairing properties.

[0067] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A self-healing bio-based coating material that combines controlled nutrient release and membrane degradation, characterized in that, Including the following parts by weight of raw materials: 80-100 parts of easily degradable polyester polyol, 30-50 parts of crosslinking accelerator, and 10-20 parts of functional chain extender; The functional chain extender is obtained by blending a first component and a second component in a molar ratio of 1:(1-3); the first component is one or more of thiamine disulfide, captopril disulfide, and ethyl 2-chloro-2-(oxime)acetate; the second component is one or more of polytetrahydrofuran, polycarbonate diol, and polycaprolactone diol.

2. The self-healing bio-based coating material according to claim 1, characterized in that, The readily degradable polyester polyol is obtained by reacting component A and component B in a molar ratio of (0.5-1.5):(0.5-1.5); component A is one or more of aspartic acid, glutamic acid, and lysine; and component B is one or more of soybean oil polyol and flaxseed oil polyol.

3. The self-healing bio-based coating material according to claim 1, characterized in that, The crosslinking agent is selected from one or more of isophthalic diisocyanate, 4-chloro-6-methyl-m-phenylene diisocyanate, and 2,4-difluorophenyl isocyanate.

4. The self-healing bio-based coating material according to claim 1 or 2, characterized in that, The reaction conditions for the readily degradable polyester polyol are as follows: After mixing components A and B, p-toluenesulfonic acid and toluene are added, and the mixture is heated to 140-160℃ under nitrogen protection and reacted for 6-8 hours; then cooled to 80℃ and reacted for 20-40 minutes.

5. The self-healing bio-based coating material according to claim 1, characterized in that, The blending conditions for the functional chain extender are as follows: Mix the first component with the vacuum-dried second component and stir continuously at 40-60℃ for 20-40 minutes.

6. The method for preparing the self-healing bio-based coating material according to any one of claims 1-5, characterized in that, Includes the following steps: Easily degradable polyester polyols are added to organic solvents and stirred until the solution is homogeneous. Then, functional chain extenders are added, and the mixture is stirred continuously at 40-50°C for 0.5-1.5 hours under nitrogen protection to generate an intermediate. The intermediate was added to the crosslinking agent, and dibutyltin dilaurate was added dropwise. The mixture was stirred rapidly until a large number of bubbles were generated. An organic solvent was added, followed by nitrogen gas. The mixture was stirred slowly for 3-5 minutes. The mixed solution was then vacuum dried. After the bubbles disappeared, the self-healing bio-based coating material was obtained.

7. The preparation method according to claim 6, characterized in that, The organic solvent is N,N-dimethylformamide or acetone.

8. The application of the self-healing bio-based coating material according to any one of claims 1-5 in the preparation of controlled-release fertilizers.

9. A coated controlled-release fertilizer, characterized in that, The fertilizer core includes a self-healing bio-based coating material as described in any one of claims 1-5, which combines nutrient controlled release and membrane degradation, and is sprayed onto the surface of the fertilizer core.

10. The coated controlled-release fertilizer according to claim 9, characterized in that, The amount of self-healing bio-based coating material that balances nutrient control and membrane degradation accounts for 1-5% of the fertilizer core weight.

Citation Information

Patent Citations

  • Yield-increasing functional full-biodegradable controlled-release fertilizer and preparation method thereof

    CN119263918A

  • Biodegradation sustained-release fertilizer coating material containing soybean oil polyhydric alcohol and preparation process thereof

    CN103772646A

  • Recyclable self-repairing elastic bio-based coating material and preparation method thereof

    CN113336604A

  • Bio-based membrane with self-repairing function, coated controlled-release fertilizer and preparation method

    CN113788711A

  • Captopril sustained-release microcapsule and preparation method thereof

    CN113925843A