Irregular spherical porous carbon and preparation method and application thereof, and silicon-carbon composite material and preparation method and application thereof

By preparing irregular spherical porous carbon, the contact area between carbon particles and binder is increased, which solves the problem of easy detachment of spherical carbon particles and improves the cycle stability and withstand voltage of lithium-ion batteries.

CN121449066AActive Publication Date: 2026-02-03BEIJING IAMETAL NEW ENERGY TECH CO LTD +1

Patent Information

Application Number
CN202511639499.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-10
Publication Date
2026-02-03
Estimated Expiration
2045-11-10

AI Technical Summary

Technical Problem

The contact between spherical carbon particles is point-to-point, which can easily lead to the spherical particles detaching from the binder and reduce the cycle stability of lithium-ion batteries.

Method used

An irregular spherical porous carbon preparation method is adopted. This method involves emulsification and compounding with a mixture of oil-soluble and water-soluble surfactants as emulsifiers, and changing the shape of the resin under ultrasonic assistance. Combined with pyrolysis and gas activation, irregular spherical porous carbon is prepared to increase the contact area between carbon particles and binder.

Benefits of technology

It improves the cycle stability of lithium-ion batteries and the withstand voltage of carbon particles, thus solving the problem of capacity decay.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121449066A_ABST
    Figure CN121449066A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery negative electrode materials, in particular to irregular spherical porous carbon and a preparation method and application thereof, and a silicon-carbon composite material and a preparation method and application thereof. The liquid phenolic resin is emulsified, compounded, cross-linked and cured under the condition of an oil-soluble and water-soluble compound emulsifier, meanwhile, the shape of the obtained resin is changed in an ultrasonic-assisted mode under the combined action of ultrasonic disturbance and different interfacial tensions, spherical resin is adjusted into irregular spherical resin, and the spherical resin is prepared into the irregular spherical resin. And performing pyrolysis and gas activation to obtain the irregular porous spherical carbon. Compared with spherical carbon, the irregular spherical carbon prepared by the invention has the advantages that on the premise of keeping the strength of the spherical carbon, the irregular spherical carbon can increase the contact area between carbon particles and a binder, and the carbon particles and the binder are not easy to separate, so that the cycling stability of a battery (especially a lithium ion battery) is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] This invention relates to the field of battery anode material technology, specifically to an irregular spherical porous carbon and its preparation method and application, and silicon-carbon composite materials and their preparation method and application. Background Technology

[0003] In the field of lithium-ion battery research, silicon-carbon anode materials have been extensively studied. As a carbon substrate, spherical carbon has attracted attention due to its unique structural characteristics. As an anode material, the spherical structure has high withstand voltage strength. However, the contact between spherical carbon particles is point-to-point, which can easily lead to detachment between the spherical particles and the binder, thereby reducing the cycle stability of lithium-ion batteries. Summary of the Invention

[0004] In view of this, the purpose of this invention is to provide an irregular spherical porous carbon, its preparation method and application, and a silicon-carbon composite material, its preparation method and application. The irregular spherical porous carbon prepared by this invention has high strength, and the irregular spherical structure can increase the contact area between carbon particles and binders, thereby improving the cycle stability of lithium-ion batteries.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing irregularly shaped spherical porous carbon, comprising the following steps: Under ultrasonic conditions, liquid phenolic resin, water, and a compound emulsifier are emulsified, and then crosslinked and cured in the presence of a curing agent to obtain irregular spherical phenolic resin; the compound emulsifier includes oil-soluble surfactants and water-soluble surfactants. The irregular spherical phenolic resin was subjected to pyrolysis and gas activation in sequence to obtain irregular spherical porous carbon; the pyrolysis was carried out under a protective atmosphere.

[0006] Preferably, the power of the ultrasound is 150~1000W and the frequency is 20~40kHz; The compound emulsifier includes a mixture of Span-80 and Tween-80, or a mixture of AEO-3 and AEO-9; The mass ratio of the oil-soluble surfactant to the water-soluble surfactant is 5~10:90~95; The mass of the compound emulsifier is 1-5% of the total mass of phenol and formaldehyde used in the preparation of liquid phenolic resin; The emulsification temperature is 40~50℃ and the time is 2~8h.

[0007] Preferably, the curing agent comprises hexamethylenetetramine; The mass of the curing agent is 1-5% of the total mass of phenol and formaldehyde used in the preparation of the liquid phenolic resin; The cross-linking curing temperature is 85~95℃, and the time is 10~20h.

[0008] Preferably, the pyrolysis temperature is 700~900℃ and the time is 2~4h; The conditions for gas activation include: the activation atmosphere includes CO2 and / or H2O, the temperature is 800~1000℃, and the time is 12~48h.

[0009] Preferably, the preparation method of the liquid phenolic resin includes the following steps: mixing phenol, formaldehyde, alkaline catalyst and water, and carrying out a condensation reaction to obtain liquid phenolic resin.

[0010] Preferably, the molar ratio of phenol to formaldehyde is 1:1.2~1.5; The mass ratio of phenol to alkaline catalyst is 1:0.05~0.5; The alkaline catalyst includes ammonia water; The polycondensation reaction is carried out at a temperature of 65-75°C for 8-12 hours. The solid content of the liquid phenolic resin is 40-45%.

[0011] The present invention also provides irregular spherical porous carbon prepared by the preparation method described in the above technical solution.

[0012] The present invention also provides a silicon-carbon composite material, comprising the irregular spherical porous carbon described in the above technical solution and silicon supported on the irregular spherical porous carbon; The silicon content in the silicon-carbon composite material is 30-50% by mass.

[0013] The present invention also provides a method for preparing the silicon-carbon composite material described in the above technical solution, comprising the following steps: depositing silane on the surface of the silicon-carbon composite material to obtain the silicon-carbon composite material.

[0014] The present invention also provides the application of the silicon-carbon composite material described in the above technical solution or the silicon-carbon composite material prepared by the above technical solution as an electrode in a battery.

[0015] To maintain high pressure resistance of carbon while addressing capacity decay, this invention designs carbon particles into irregular spherical morphology. Emulsification and compounding are performed using oil-soluble and water-soluble surfactants (compound emulsifiers), with ultrasonic assistance. Under the combined effects of ultrasonic disturbance and different interfacial tensions, the shape of the obtained resin is altered, transforming spherical resin into irregular spherical resin. After pyrolysis and gas activation, irregular porous spherical carbon is obtained. Compared to spherical carbon, the irregular spherical carbon prepared by this invention, while maintaining the strength of spherical carbon, increases the contact area between carbon particles and the binder, making them less prone to detachment and thus improving the cycle stability of batteries (especially lithium-ion batteries). Furthermore, phenolic resin exhibits a carbon residue rate greater than 40% at 800°C, while other resins only reach 10-20%. This invention, using phenolic resin as a raw material for porous carbon preparation, can improve the yield of porous carbon. Attached Figure Description

[0016] Figure 1 Here is a SEM image of the irregular spherical resin from Example 1; Figure 2 This is a SEM image of the irregularly shaped spherical porous carbon in Example 1. Detailed Implementation

[0017] This invention provides a method for preparing irregularly shaped spherical porous carbon, comprising the following steps: Under ultrasonic conditions, liquid phenolic resin, water, and a compound emulsifier are emulsified, and then crosslinked and cured in the presence of a curing agent to obtain irregular spherical phenolic resin; the compound emulsifier includes oil-soluble surfactants and water-soluble surfactants. The irregular spherical phenolic resin was subjected to pyrolysis and gas activation in sequence to obtain irregular spherical porous carbon; the pyrolysis was carried out under a protective atmosphere.

[0018] Unless otherwise specified, the materials and equipment used in this invention are all commercially available products in the field.

[0019] This invention involves emulsifying liquid phenolic resin, water, and a compound emulsifier under ultrasonic conditions, followed by crosslinking and curing in the presence of a curing agent to obtain irregularly shaped spherical phenolic resin; the compound emulsifier includes oil-soluble surfactants and water-soluble surfactants.

[0020] In this invention, the preferred method for preparing the liquid phenolic resin includes the following steps: mixing phenol, formaldehyde, an alkaline catalyst and water, and carrying out a condensation reaction to obtain the liquid phenolic resin.

[0021] In this invention, the molar ratio of phenol to formaldehyde is preferably 1:1.2 to 1.5, and may specifically be 1:1.2, 1:1.3, 1:1.4, or 1:1.5. In this invention, the formaldehyde is preferably used in the form of an aqueous solution, and the concentration of the aqueous solution is preferably 30 to 40 wt%, and may specifically be 30 wt%, 32 wt%, 35 wt%, 37 wt%, or 40 wt%.

[0022] In this invention, the mass ratio of phenol to alkaline catalyst is preferably 1:0.05 to 0.5, specifically 1:0.05, 1:0.08, 1:0.1, 1:0.13, 1:0.15, 1:0.2, 1:0.3, 1:0.4, or 1:0.5. In this invention, the alkaline catalyst preferably comprises ammonia water, and the concentration of the ammonia water is preferably 20-30 wt%, specifically 20 wt%, 2 wt%, 25 wt%, 28 wt%, or 30 wt%.

[0023] In this invention, the temperature of the polycondensation reaction is preferably 65~75℃, specifically 65℃, 68℃, 70℃, 72℃ or 75℃; the time of the polycondensation reaction is preferably 8~12h, specifically 8h, 9h, 10h, 11h or 12h.

[0024] In this invention, the total amount of water in the raw materials for preparing the liquid phenolic resin is based on the solid content of the obtained liquid phenolic resin being 40-45%, and the solid content of the liquid phenolic resin can be specifically 40%, 41%, 42%, 43%, 44% or 45%.

[0025] In this invention, the emulsification and cross-linking curing are performed under ultrasonic conditions. The power of the ultrasound is preferably 150-1000W, specifically 150W, 200W, 300W, 400W, 500W, 600W, 700W, 800W, 900W, or 1000W. The frequency of the ultrasound is preferably 20-40kHz, specifically 20kHz, 25kHz, 30kHz, 35kHz, or 40kHz. The emulsification and cross-linking curing are preferably performed in a reaction device equipped with an ultrasonic module.

[0026] In this invention, the compound emulsifier includes oil-soluble surfactants and water-soluble surfactants, preferably including a mixture of Span-80 and Tween-80, or a mixture of AEO-3 and AEO-9. In this invention, the preferred mass ratio of the oil-soluble surfactant to the water-soluble surfactant is 5-10:90-95, specifically 5:90, 5:91, 5:92, 5:93, 5:94, 5:95, 6:90, 6:91, 6:92, 6:93, 6:94, 6:95, 7:90, 7:91, 7:92, 7:93, 7:94, 7:95, 8:90, 8:91, 8:92, 8:93, 8:94, 8:95, 9:90, 9:91, 9:92, 9:93, 9:94, 9:95, 10:90, 10:91, 10:92, 10:93, 10:94, or 10:95. This invention uses oil-soluble and water-soluble surfactants (compound emulsifiers) for emulsification and compounding, and employs an ultrasonic-assisted method to change the shape of the obtained resin under the combined action of ultrasonic disturbance and different interfacial tensions, adjusting the spherical resin into irregular spherical resin.

[0027] In this invention, the mass of the compound emulsifier is preferably 1 to 5% of the total mass of phenol and formaldehyde used in the preparation of liquid phenolic resin, specifically 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 4.9% or 5%.

[0028] In this invention, the emulsification temperature is preferably 40~50℃, specifically 40℃, 42℃, 44℃, 46℃, 48℃ or 50℃; the emulsification time is preferably 2~8h, specifically 2h, 3h, 4h, 5h, 6h, 7h or 8h; the emulsification is preferably carried out under stirring conditions; the stirring speed is preferably 80~120r / min, specifically 80r / min, 90r / min, 100r / min, 110r / min or 120r / min.

[0029] In this invention, the curing agent preferably comprises hexamethylenetetramine. In this invention, the mass of the curing agent is preferably 1-5% of the total mass of phenol and formaldehyde used in the preparation of the liquid phenolic resin, specifically 1%, 1.2%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.

[0030] In this invention, the cross-linking curing temperature is preferably 85~95℃, specifically 85℃, 88℃, 90℃, 93℃ or 95℃; the cross-linking curing time is preferably 10~20h, specifically 10h, 12h, 14h, 16h, 18h or 20h.

[0031] After the crosslinking and curing is completed, the present invention preferably further includes: centrifuging and washing the crosslinked and cured system and then drying it to obtain irregular spherical phenolic resin. In the present invention, the solvent used for centrifugation and washing preferably includes at least one of water, alcohol solvents, and lipid solvents, wherein the alcohol solvent preferably includes methanol and / or ethanol; and the lipid solvent preferably includes ethyl acetate and / or butyl acetate. In the present invention, the drying temperature is preferably 80~150℃, specifically 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, 140℃, or 150℃; and the drying time is preferably 12~48h, specifically 12h, 15h, 18h, 20h, 22h, 24h, 28h, 30h, 32h, 35h, 38h, 40h, 42h, 45h, or 48h.

[0032] After obtaining irregular spherical phenolic resin, the present invention sequentially pyrolyzes and gas-activates the irregular spherical phenolic resin to obtain irregular spherical porous carbon; the pyrolysis is carried out under a protective atmosphere.

[0033] In this invention, the pyrolysis temperature is preferably 700~900℃, specifically 700℃, 750℃, 800℃, 850℃, or 900℃; the pyrolysis time is preferably 2~4 hours, specifically 2 hours, 2.5 hours, 3 hours, 3.5 hours, or 4 hours; the pyrolysis is carried out under a protective atmosphere, preferably including nitrogen, argon, or helium. In this invention, during the pyrolysis process, irregular spherical phenolic resin is transformed into irregular spherical pyrolytic carbon.

[0034] In this invention, the gas activation conditions preferably include: the activation atmosphere comprising CO2 and / or H2O (water vapor); the temperature being 800~1000℃, specifically 800℃, 850℃, 900℃, 950℃ or 1000℃; and the time being 12~48h, specifically 12h, 15h, 18h, 20h, 22h, 25h, 28h, 30h, 32h, 35h, 38h, 40h, 42h, 45h or 48h.

[0035] This invention involves emulsifying and compounding liquid phenolic resin under a mixture of oil-soluble and water-soluble emulsifiers. Simultaneously, an ultrasonic-assisted process is employed to alter the shape of the cross-linked and cured resin under the combined effects of ultrasonic disturbance and varying interfacial tensions, transforming spherical resin into irregularly shaped spherical resin. Following pyrolysis and gas activation, irregularly porous spherical carbon is obtained. Compared to spherical carbon, the irregularly shaped spherical carbon prepared in this invention, while maintaining the strength of spherical carbon, increases the contact area between carbon particles and the binder, making it less prone to detachment and thus improving the cycle stability of batteries (especially lithium-ion batteries).

[0036] This invention also provides irregular spherical porous carbon prepared by the preparation method described in the above technical solution. In this invention, the porous structure of the irregular spherical porous carbon preferably includes micropores (<2nm), pores of 2~10nm, and pores >10nm; the proportion of micropores (<2nm) is preferably 90~97%, specifically 90%, 90.12%, 91%, 92%, 92.31%, 93%, 93.64%, 93.65%, 94%, 95%, 95.63%, 96%, or 97%; the proportion of pores of 2~10nm is preferably 2~10%, specifically 2%, 3%, 3.42%, 4%, 5%, 5.09%, 5.39%, 6%, 6.59%, 6.93%, 7%, 8%, 9%, or 10%. In this invention, the specific surface area of ​​the irregular spherical porous carbon is preferably 2000~2500 μm. 2 / g, which can be specifically 2000m 2 / g、2009.62m 2 / g、2036.26m 2 / g、2063.21m 2 / g、2100m 2 / g、2150m 2 / g、2196.36m 2 / g、2200m 2 / g、2235.61m 2 / g、2300m 2 / g、2400m 2 / g or 2500m 2 / g; the pore volume of the irregularly shaped spherical porous carbon is preferably 0.7~1.0 cm³. 3 / g, which can be specifically 0.7cm 3 / g, 0.8cm 3 / g, 0.89cm 3 / g, 0.90cm 3 / g, 0.91cm 3 / g, 0.92cm 3 / g, 0.96cm 3 / g or 1cm 3 / g.

[0037] The irregular spherical porous carbon provided by this invention has high mechanical strength (e.g., pressure resistance). Silane can be deposited on the irregular spherical porous carbon to obtain silicon-carbon composite materials. When used as a negative electrode in lithium-ion batteries, it exhibits high cycle stability and pressure resistance, while solving the problem of capacity decay.

[0038] The present invention also provides a silicon-carbon composite material, comprising the irregular spherical porous carbon described in the above technical solution and silicon supported on the irregular spherical porous carbon. In the present invention, the mass content of silicon in the silicon-carbon composite material is preferably 30-50%, specifically 30%, 35%, 40%, 45% or 50%.

[0039] This invention also provides a method for preparing the silicon-carbon composite material described in the above technical solution, comprising the following steps: depositing silane on the surface of the silicon-carbon composite material to obtain the silicon-carbon composite material. The silicon-carbon composite material provided by this invention has high mechanical strength and exhibits high cycle stability when applied in the field of lithium-ion batteries.

[0040] In this invention, the preferred conditions for silane deposition include: the reaction gas is silane, specifically including at least one of silane, disilane, trichlorosilane, dichlorosilane, and trichlorosilane; the flow rate of the reaction gas is preferably 5-15 L / min, specifically 5 L / min, 8 L / min, 10 L / min, 12 L / min, or 15 L / min; the carrier gas includes nitrogen and / or argon; the volume ratio of the reaction gas to the carrier gas is 1:1-20, more preferably 1:1-10, specifically 1:1, 1:5, 1:10, 1:15, or 1:20; the deposition temperature is 500-600℃, specifically 500℃, 50℃, 540℃, 560℃, 580℃, or 600℃; and the deposition time is 4-9 h, specifically 4 h, 5 h, 6 h, 7 h, 8 h, or 9 h.

[0041] This invention also provides the application of the silicon-carbon composite material described in the above-described technical solutions, or the silicon-carbon composite material prepared by the above-described technical solutions, as an electrode in a battery. In this invention, the electrode is preferably a negative electrode. In this invention, the battery preferably includes a lithium-ion battery or a sodium-ion battery. The silicon-carbon composite material provided by this invention, while maintaining material strength, can increase the contact area between irregular spherical silicon-carbon particles and the binder, thereby improving the cycle stability of the battery (especially a lithium-ion battery).

[0042] To further illustrate the present invention, the irregular spherical porous carbon and its preparation method and application, as well as the silicon-carbon composite material and its preparation method and application, provided by the present invention are described in detail below with reference to the embodiments. However, these descriptions should not be construed as limiting the scope of protection of the present invention.

[0043] Example 1 S1: Weigh 94.11g of phenol and 121.62g of formaldehyde solution (37wt%), add them to 115.48g of water, then add 9g of ammonia water (25wt%) and stir until homogeneous. React at 70℃ for 12h to obtain liquid phenolic resin.

[0044] S2: Under ultrasonic conditions of 200W and 20Hz, 0.1g of Span-80 and 1.9g of Tween-80 compound emulsifier were added to 100g of liquid phenolic resin. The mixture was dispersed at 45℃ and 90r / min for 4h. After dispersion, 0.42g of hexamethylenetetramine curing agent was added, the temperature was raised to 90℃, and the reaction was carried out for 12h. After the reaction, the mixture was centrifuged and washed, and dried at 100℃ for 24h to obtain irregular spherical phenolic resin.

[0045] S3: Irregular spherical phenolic resin is pyrolyzed at 700℃ for 2 hours under argon atmosphere to obtain irregular spherical pyrolytic carbon.

[0046] S4: Irregular spherical pyrolytic carbon is activated in a CO2 atmosphere at 900℃ for 15 h to obtain irregular spherical porous carbon.

[0047] Figure 1 The image shows an SEM image of the irregular spherical resin prepared in this embodiment. It can be seen that irregular spherical resin can be obtained by the above method, and the morphology presents an irregular polyhedral structure.

[0048] Figure 2 The SEM image of the irregular spherical porous carbon prepared in this embodiment shows that after the pyrolysis and activation process, the resin did not undergo obvious damage such as melting or cracking, and maintained the morphological characteristics of the irregular polyhedral structure consistent with the irregular resin. In addition to the porous structure, the porous carbon material also has micron-level morphological characteristics, and exhibits the advantages brought by its structure in the electrical performance test.

[0049] Example 2 Irregular spherical porous carbon was prepared according to the method of Example 1, the only difference from Example 1 being that the emulsifier in step S2 was a mixture of 0.1g AEO-3 and 1.9g AEO-9.

[0050] Example 3 Irregular spherical porous carbon was prepared according to the method of Example 1, the only difference from Example 1 being that the ultrasonic power in step S2 was 500W.

[0051] Example 4 Irregular spherical porous carbon was prepared according to the method of Example 1, the only difference from Example 1 being that the ultrasonic power in step S2 was 800W.

[0052] Example 5 Irregular spherical porous carbon was prepared according to the method of Example 1, the only difference from Example 1 being that the ultrasonic power in step S2 was 1000W.

[0053] Comparative Example 1 The only difference from Example 1 is that in step S2, the emulsifier is 2.0 g Tween-80, and porous carbon is obtained.

[0054] Comparative Example 2 The only difference from Example 1 is that in step S2, the emulsifier is 2.0g AEO-9, and porous carbon is obtained.

[0055] Comparative Example 3 The only difference from Example 1 is that the ultrasonic power in step S2 is 2000W, resulting in porous carbon.

[0056] Comparative Example 4 The only difference from Example 1 is that in step S2, the emulsifier is a mixture of 1.9g Span-80 and 0.1g Tween-80 to obtain porous carbon.

[0057] Test Example 1 The porous carbon prepared in the examples and comparative examples was subjected to pore structure and compressive strength tests, and the results are shown in Table 1. The compressive strength test method involved ultrasonically dispersing the porous carbon in ethanol solvent. After dispersion, the carbon was placed under an optical system to locate individual particles. A dedicated indenter was used to perform a crush test on the porous carbon, and the strength data was recorded.

[0058] Table 1. Pore structure parameters and compressive strength of porous carbon

[0059] As can be seen from the data in Table 1, compared with the comparative example, the irregular spherical porous carbon obtained in the example also exhibits high microporosity; the compressive strength of the irregular spherical porous carbon obtained in the example is above 590 MPa, specifically 595.89~623.17 MPa, which is high.

[0060] Application Example 1 The porous carbon prepared in the examples and comparative examples was subjected to silane deposition to obtain silicon-carbon composite materials. The silane deposition temperature was 500°C, the deposition time was 5 hours, and the silicon content in the silicon-carbon composite material was 40 wt%.

[0061] The electrochemical performance of various silicon-carbon composite materials was evaluated using them as negative electrodes. The electrochemical performance testing conditions were as follows: assembled button batteries were tested in a Blue Electric testing system at a voltage of 0.005–1.5 V. The positive electrode was a lithium sheet, and the negative electrode was the prepared silicon-carbon composite material. The conductive agent was carbon nanotubes, and the binder was polyacrylic acid. The mass ratio of silicon-carbon negative electrode material to conductive agent to binder was 94:2:4. The electrolyte was a 1 mol / L LiPF6 solution (solvent: diethyl carbonate: dimethyl carbonate: ethylene carbonate volume ratio = 1:1:1). The test results are shown in Table 2.

[0062] Table 2 Electrochemical Performance Tests

[0063] As shown in Table 2, compared with the comparative examples, the carbon-silicon composite materials prepared from the irregular spherical porous carbon in Examples 1-5 exhibited higher capacity retention when used as the negative electrode. The porous carbon prepared in Comparative Examples 1-2, being spherical materials, showed faster capacity decay. In Comparative Example 3, the ultrasonic power used in the porous carbon preparation process was high, resulting in greater spherical deformation and poorer performance. In Comparative Example 4, the excessive amount of water-soluble surfactant in the compound emulsifier led to extremely poor porous carbon morphology and electrical performance.

[0064] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing irregularly shaped spherical porous carbon, characterized in that, Includes the following steps: Under ultrasonic conditions, liquid phenolic resin, water, and a compound emulsifier are emulsified, and then crosslinked and cured in the presence of a curing agent to obtain irregular spherical phenolic resin; the compound emulsifier includes oil-soluble surfactants and water-soluble surfactants. The irregular spherical phenolic resin was subjected to pyrolysis and gas activation in sequence to obtain irregular spherical porous carbon; the pyrolysis was carried out under a protective atmosphere.

2. The preparation method according to claim 1, characterized in that, The power of the ultrasound is 150~1000W, and the frequency is 20~40kHz; The compound emulsifier includes a mixture of Span-80 and Tween-80, or a mixture of AEO-3 and AEO-9; The mass ratio of the oil-soluble surfactant to the water-soluble surfactant is 5~10:90~95; The mass of the compound emulsifier is 1-5% of the total mass of phenol and formaldehyde used in the preparation of liquid phenolic resin; The emulsification temperature is 40~50℃ and the time is 2~8h.

3. The preparation method according to claim 1, characterized in that, The curing agent includes hexamethylenetetramine; The mass of the curing agent is 1-5% of the total mass of phenol and formaldehyde used in the preparation of the liquid phenolic resin; The cross-linking curing temperature is 85~95℃, and the time is 10~20h.

4. The preparation method according to claim 1, characterized in that, The pyrolysis temperature is 700~900℃, and the time is 2~4h; The conditions for gas activation include: the activation atmosphere includes CO2 and / or H2O, the temperature is 800~1000℃, and the time is 12~48h.

5. The preparation method according to claim 1, characterized in that, The preparation method of the liquid phenolic resin includes the following steps: mixing phenol, formaldehyde, alkaline catalyst and water, and carrying out a condensation reaction to obtain liquid phenolic resin.

6. The preparation method according to claim 5, characterized in that, The molar ratio of phenol to formaldehyde is 1:1.2~1.5; The mass ratio of phenol to alkaline catalyst is 1:0.05~0.5; The alkaline catalyst includes ammonia water; The polycondensation reaction is carried out at a temperature of 65-75°C for 8-12 hours. The solid content of the liquid phenolic resin is 40-45%.

7. Irregular spherical porous carbon prepared by the preparation method according to any one of claims 1 to 6.

8. A silicon-carbon composite material, characterized in that, Includes the irregular spherical porous carbon as described in claim 6 and silicon supported on the irregular spherical porous carbon; The silicon content in the silicon-carbon composite material is 30-50% by mass.

9. The method for preparing the silicon-carbon composite material according to claim 8, characterized in that, Includes the following steps: The silicon-carbon composite material is obtained by depositing silane on its surface.

10. The application of the silicon-carbon composite material of claim 8 or the silicon-carbon composite material prepared by the preparation method of claim 9 as an electrode in a battery.

Citation Information

Patent Citations

  • Phenolic resin emulsion, and preparation method and application thereof

    CN109721745A

  • Preparation method of blow-off prevention porous carbon material for silicon-carbon negative electrode

    CN119263273A

  • Phenolic resin-based spherical activated carbon as well as preparation method and application thereof

    CN119683620A

  • Carbon material, silicon-carbon composite material and application thereof

    CN120057919A

  • Resin material as well as preparation method and application thereof

    CN120059398A

Cited By

  • Phenolic resin-based multi-shape silicon-carbon negative electrode material and preparation method thereof

    CN121885604A

  • Anisometric spherical phenol-formaldehyde resin microparticles, and a method for preparing and using the same

    CN122325795A