A method for preparing a carbon-based ammonia cracking catalyst for hydrogen production and its application

By acid washing and potassium activation of nano-onion carbon, and synergistic effect with cobalt and magnesium oxide additives, a CoMgO4 structure is formed, which solves the problem of insufficient activity and stability of nano-onion carbon catalyst in the medium and low temperature range, and realizes efficient ammonia decomposition to hydrogen production.

CN121513879BActive Publication Date: 2026-11-10CHINA-SINGAPORE INT JOINT RES INST
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202511926048.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-18
Publication Date
2026-11-10
Estimated Expiration
2045-12-18

AI Technical Summary

Technical Problem

Existing non-precious metal catalysts have insufficient catalytic activity and stability in the medium and low temperature range. In particular, nano-onion carbon has fewer functional groups on its surface, resulting in weak interaction with metal ions and insufficient basic sites, leading to low ammonia decomposition efficiency.

Method used

By acid washing and potassium activation pretreatment of nano-onion carbon, oxygen-containing functional groups and strongly electropositive K elements are introduced. Combined with cobalt and magnesium oxide additives, a CoMgO4 spinel structure is formed, which enhances the metal-support interaction and the alkaline sites on the catalyst surface.

Benefits of technology

It significantly improves the low-temperature activity and stability of the catalyst, achieving an ammonia conversion rate of 99.6%. It shows no significant deactivation under harsh conditions and has the potential for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121513879B_ABST
    Figure CN121513879B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a carbon-based ammonia cracking catalyst for hydrogen production and its application. The steps are as follows: A nano-onion carbon support is subjected to a two-stage pretreatment process of acid washing and potassium salt solution impregnation activation to obtain an activated support K-CNO'; Cobalt salt, magnesium salt, and urea are reacted with the activated support under hydrothermal conditions using a uniform deposition precipitation method; after precipitation, filtration, washing, drying, and calcination, the final catalyst Co is obtained. x Mg / K-CNO'. This invention introduces oxygen-containing functional groups onto the surface of CNOs through acid washing, enhances the basicity and specific surface area of ​​the support through potassium activation, and generates a strong synergistic effect with the active component Co and the auxiliary agent MgO, achieving high dispersion, strong stability, and abundant surface basic sites for the Co-based active centers. This catalyst exhibits excellent low-temperature catalytic activity and stability in the ammonia decomposition to hydrogen production reaction, achieving an ammonia conversion rate as high as 99.6% under specific conditions, and can operate stably at 500℃ for extended periods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst technology, specifically relating to a method for preparing a carbon-based ammonia cracking catalyst for hydrogen production and its application. Background Technology

[0002] Hydrogen, as a clean energy carrier, is an important component of the future energy system. Ammonia (NH3) is considered an ideal hydrogen storage medium due to its high hydrogen storage density, easy liquefaction, and mature infrastructure. High-purity hydrogen can be obtained efficiently and conveniently through the ammonia decomposition reaction (2NH3→N2+ 3H2). The key to this technology lies in developing low-temperature, highly active, highly stable, and low-cost catalysts.

[0003] Currently, Ru-based catalysts exhibit the best performance, but their high cost limits their widespread application. Non-precious metals such as Co, Fe, and Ni have become research hotspots, but their catalytic activity, especially in the medium- and low-temperature range, still needs improvement. The performance of a catalyst largely depends on the dispersion and particle size of the active metal, its interaction with the support, and the acidity or basicity of the catalyst surface.

[0004] Nano-onion carbon (CNOs) are a novel carbon material with a multi-layered concentric shell structure. They possess a large specific surface area and abundant surface defects, which facilitates the dispersion and anchoring of metal nanoparticles and effectively inhibits sintering. However, pristine CNOs have few surface functional groups, resulting in weak interactions with metal ions, and their surface basic sites are insufficient for efficient activation of ammonia molecules. Therefore, modifying CNOs and synergistically optimizing the active components is a key challenge in improving their ammonia decomposition catalytic performance. Summary of the Invention

[0005] The main objective of this invention is to overcome the shortcomings and deficiencies of existing technologies and provide a method for preparing a low-temperature, highly active, stable, and low-cost carbon-based ammonia cracking catalyst for hydrogen production, as well as its application. This method significantly improves the overall performance of the catalyst through precise acid washing and potassium activation pretreatment of the CNOs support, combined with the synergistic effect of cobalt and magnesium oxide promoters.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a method for preparing a carbon-based ammonia cracking catalyst for hydrogen production, characterized in that the preparation method includes the following steps:

[0008] S1. Carrier Pretreatment: Nano-onion carbon (CNOs) is sequentially subjected to acid washing and potassium salt solution immersion activation treatment to obtain activated carrier K-CNO'. This step aims to remove metallic impurities from the surface of CNOs and introduce oxygen-containing functional groups (such as -COOH, -OH) as active sites for subsequent anchoring of metal ions. Then, the specific surface area of ​​the carrier is further increased by alkaline etching, and the strongly electropositive potassium element is introduced, significantly enhancing the alkalinity of the carrier surface.

[0009] S2. Catalyst Preparation: Using a uniform deposition precipitation method, cobalt salt, magnesium salt, urea, and the activated support K-CNO' are mixed in an aqueous solution and reacted under heating and stirring conditions, causing cobalt and magnesium hydroxides or carbonates to be uniformly deposited on the activated support K-CNO'. After the reaction is complete, the mixture is filtered, washed, dried, and calcined to obtain the final catalyst Co. x Mg y / K-CNO'.

[0010] Further, the method is characterized in that, in step S1, the acid washing process is as follows: CNOs are dispersed in a 1M hydrochloric acid solution, stirred for 12-36 hours, filtered, washed until neutral, and dried at 100-150 °C to obtain CNO'.

[0011] The purpose of this step is to remove the exposed catalyst and amorphous carbon from the surface of CNOs, thereby obtaining CNO'.

[0012] Further, in step S1, the potassium salt solution impregnation and activation process is as follows: the CNO' obtained after acid washing and drying is added to a 1M potassium carbonate K2CO3 solution, stirred at 90-100 ℃ for 12-36 hours, then filtered, dried, and calcined at 300-400 ℃ for 1-3 hours to obtain K-CNO'.

[0013] In this step, a large number of carboxyl and hydroxyl functional groups are introduced into the CNO' surface, and the K element is added.

[0014] Further, in step S2, the cobalt salt is cobalt nitrate Co(NO3)2·6H2O, the magnesium salt is magnesium nitrate Mg(NO3)2·6H2O, and the molar ratio of urea to the total of cobalt and magnesium salts is (3-5):1.

[0015] In this step, an appropriate ratio of urea to active metal is given, so that the active metal slowly and uniformly precipitates on the K-CNO' surface.

[0016] Furthermore, in step S2, the molar ratio of cobalt to magnesium is 1-4:1, and the total loading of cobalt and magnesium accounts for 25%-35% of the total mass of the catalyst by metal mass.

[0017] In this step, an appropriate active metal loading is provided to form a strong interaction between the metal and the support, resulting in higher catalyst activity.

[0018] Furthermore, in step S2, the temperature for heating and stirring the reaction is 90-100℃, and the time is 20-28 hours.

[0019] In this step, a temperature of 90-100℃ is proposed, as this temperature mainly enhances the hydrolysis of urea.

[0020] Furthermore, in step S2, the calcination conditions are as follows: in air or an inert atmosphere, the temperature is increased to 450-550°C at a rate of 1-5°C / min, and held at that temperature for 3-5 hours.

[0021] The combustion scheme presented in this step converts the hydroxide of the active metal into the oxide of the active metal, thereby better utilizing the performance of the catalyst.

[0022] Secondly, this invention provides an application of a carbon-based ammonia cracking hydrogen production catalyst prepared by the above-mentioned method. Before being used in the ammonia decomposition reaction, the catalyst is pretreated in a hydrogen atmosphere at 450-550°C for 1-3 hours. The ammonia decomposition reaction conditions are: reaction temperature 450-600°C, space velocity 6000-15000 mL·g. cat -1 ·h -1 .

[0023] The application of this carbon-based ammonia cracking hydrogen production catalyst involves the synthesis of Co2MgO4 and Co2Mg / CNO catalysts via homogeneous deposition-precipitation (HDP) for ammonia decomposition to produce CO-free hydrogen. x Hydrogen. Specific improvements are as follows:

[0024] 1. The active metal Co and the promoter MgO form a cobalt-magnesium spinel structure. The activity test results show that the interaction between the support CNOs and the promoter MgO improves the catalyst activity.

[0025] 2. CNOs improve electronic conductivity, resulting in uniform distribution of Co2MgO4 nanoparticles, increasing the number of alkali active sites and ammonia adsorption capacity.

[0026] 3. Introducing CNOs can increase the number of moderately alkaline sites, and adding K promoters can further increase the surface concentration of alkaline sites and enhance catalytic performance.

[0027] 4. CNOs, MgO, K, and Co work synergistically to regulate the structure, particle size, and performance of the catalyst. Stability tests show that Co2Mg / K-CNO' can operate stably for 90 h at 500 ℃ without significant deactivation, demonstrating its potential for industrial application.

[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0029] (1) Synergistic modification of the carrier: Through continuous pretreatment of "acid washing + potassium activation", on the one hand, rich oxygen-containing functional groups are introduced on the surface of CNOs, which enhances the metal-carrier interaction; on the other hand, strong alkaline K auxiliaries are introduced to expand the pores and increase the surface, which together provide an ideal platform for the construction of highly dispersed and small-sized active centers.

[0030] (2) Synergistic effect of active components: The active component Co and the auxiliary agent MgO form a spinel structure CoMgO4. After reduction, this structure can produce highly dispersed metal Co nanoparticles and MgO. The two interact strongly with the K-CNO' support (SMSI), which stabilizes the active center.

[0031] (3) Surface alkalinity optimization: The introduction of K and the coexistence of MgO greatly optimize the distribution of alkaline sites on the catalyst surface, increase the number and intensity of medium and strong alkaline sites, and effectively promote the adsorption and activation of NH3 and the desorption of N2, which is the key to obtaining high activity.

[0032] (4) Excellent performance: The Co2Mg / K-CNO' catalyst prepared in this invention exhibits excellent performance at 550℃ and a space velocity of 12000 mL·g. cat -1 ·h -1 Under harsh conditions, the ammonia conversion rate reached as high as 99.6%; at 500℃ and a space velocity of 600 mL·g⁻¹, the ammonia conversion rate was as high as 99.6%. cat -1 ·h -1 Under certain conditions, it can operate stably for 90 hours without significant deactivation, and its performance is significantly better than most reported non-precious metal catalysts, showing broad prospects for industrial application. Attached Figure Description

[0033] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0034] Figure 1 This is a flowchart of a method for preparing a carbon-based ammonia cracking hydrogen production catalyst disclosed in this invention;

[0035] Figure 2 This is a SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co2Mg / K-CNO' in Example 2;

[0036] Figure 3 The image shows a TEM image of the carbon-based ammonia cracking hydrogen production catalyst Co2Mg / K-CNO' in Example 2.

[0037] Figure 4 The image shows the SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co4Mg / K-CNO' in Comparative Example 1.

[0038] Figure 5 The image shows the SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co3Mg2 / K-CNO' in Comparative Example 2.

[0039] Figure 6 The image shows the SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co3Mg / K-CNO' in Comparative Example 3.

[0040] Figure 7 SEM image of the carbon-based ammonia cracking hydrogen production catalyst CoMg / K-CNO' in Comparative Example 4;

[0041] Figure 8 This is a comparison chart of the ammonia decomposition activities of different catalysts in Example 3;

[0042] Figure 9 The graph shows the ammonia cracking conversion rate versus running time of the carbon-based ammonia cracking catalyst Co2Mg / K-CNO' in Example 4. Detailed Implementation

[0043] To enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of the present application, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present application without creative effort are within the scope of protection of the present application.

[0044] In this application, the reference to "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments.

[0045] Example 1

[0046] like Figure 1As shown in the figure, this embodiment discloses a method for preparing a carbon-based ammonia cracking hydrogen production catalyst, including the following steps:

[0047] S1. Carrier pretreatment:

[0048] a. Acid washing: Nano-onion carbon (CNOs) were dispersed in a 1M hydrochloric acid (HCl) solution, ultrasonically dispersed until homogeneous, and then stirred at room temperature for 24 hours. Subsequently, vacuum filtration was performed, followed by repeated washing with deionized water until the filtrate was neutral. Finally, the filtrate was dried overnight in an oven at 120°C to obtain acid-washed CNOs, denoted as CNO'. This step aims to remove metallic impurities from the surface of CNOs and introduce oxygen-containing functional groups (such as -COOH, -OH) as active sites for subsequent anchoring of metal ions.

[0049] b. Potassium activation: The obtained CNO' was added to a 1M potassium carbonate (K2CO3) solution and stirred vigorously at 95°C for 24 hours. Then, it was vacuum filtered, dried at 120°C for 4 hours, and subsequently calcined in a muffle furnace at 350°C (heating rate 5°C / min) for 2 hours to obtain the potassium-activated support, denoted as K-CNO'. This step further increases the specific surface area of ​​the support through the etching effect of the alkali and introduces the strongly electropositive potassium element, significantly enhancing the alkalinity of the support surface.

[0050] S2, Catalyst Preparation:

[0051] A homogeneous deposition precipitation method was employed. Cobalt nitrate (Co(NO3)2·6H2O) and magnesium nitrate (Mg(NO3)2·6H2O) were weighed at a cobalt-to-magnesium molar ratio of 1-4:1 and dissolved together with excess urea in distilled water. The K-CNO' support prepared in step S1 was then added, and the mixture was vigorously stirred at 95°C for 24 hours. During this process, the slow hydrolysis of urea caused a uniform increase in the pH of the solution, promoting the uniform deposition of cobalt and magnesium hydroxides or basic carbonates on the surface of the K-CNO' support. After the reaction was complete, the mixture was filtered and washed with deionized water until neutral. The resulting solid was dried at 120°C for 4 hours. Finally, the dried precursor was calcined in a muffle furnace at 500°C (heating rate 2°C / min) for 4 hours to obtain the final catalyst, denoted as Co. x Mg y / K-CNO'.

[0052] Example 2

[0053] This embodiment further discloses a method for preparing a carbon-based ammonia cracking hydrogen production catalyst, including the following steps:

[0054] S1. Carrier pretreatment:

[0055] Acid washing: Weigh 20g of CNOs and disperse it in 500ml of 1M HCl, then sonicate. After stirring at room temperature for 24h, filter, wash with water until neutral, and dry at 120℃ overnight to obtain CNO'.

[0056] Potassium activation: Add 10g CNO' to 200ml 1M K2CO3 solution and stir at 95℃ for 24h. After filtration, dry at 120℃ for 4h, and then calcine at 350℃ (5℃ / min) for 2h to obtain K-CNO'.

[0057] S2, Catalyst Preparation:

[0058] Weigh 11.64 g Co(NO3)2·6H2O, 5.12 g Mg(NO3)2·6H2O, and 36 g urea, and dissolve them in distilled water. Add 2.84 g K-CNO' and stir at 95 °C for 24 h. After the reaction is complete, filter, wash with water until neutral, dry at 120 °C for 4 h, and finally calcine at 500 °C (2 °C / min) for 4 h to obtain the catalyst Co2Mg / K-CNO'. Figure 2 As shown, Figure 2 This is a SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co2Mg / K-CNO' prepared by adjusting the Co-Mg atomic molar ratio to 2:1. This demonstrates that Co and Mg are uniformly deposited on the K-CNO' support at an atomic molar ratio of 2:1, resulting in excellent ammonia cracking performance. Figure 3 As shown, Figure 3 This is a TEM image of the carbon-based ammonia cracking hydrogen production catalyst Co2Mg / K-CNO' prepared by adjusting the Co-Mg atomic molar ratio to 2:1. The catalyst obtained by uniform sedimentation clearly shows the lattice stripes of Co and Mg on the surface of the K-CNO' support.

[0059] Comparative Example 1

[0060] The Co4Mg / K-CNO' catalyst was prepared following the same steps as in Example 2, but 23.28 g of Co(NO3)2·6H2O was used in the catalyst preparation step. Figure 4 As shown, Figure 4 This is a SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co4Mg / K-CNO' prepared by adjusting the Co-Mg atomic molar ratio to 4:1. This allows Co and Mg to be uniformly deposited on the K-CNO' support at an atomic molar ratio of 4:1, giving the catalyst excellent ammonia cracking performance.

[0061] Comparative Example 2

[0062] The Co3Mg2 / K-CNO' catalyst was prepared using the same steps as in Example 2, except that 8.73 g of Co(NO3)2·6H2O was used in the catalyst preparation step. Figure 5This is a SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co3Mg2 / K-CNO' prepared by adjusting the Co-Mg atomic molar ratio to 3:2. This allows Co and Mg to be uniformly deposited on the K-CNO' support at an atomic molar ratio of 3:2, giving the catalyst excellent ammonia cracking performance.

[0063] Comparative Example 3

[0064] The Co3Mg / K-CNO' catalyst was prepared using the same steps as in Example 2, but 17.46 g of Co(NO3)2·6H2O was used in the catalyst preparation step. Figure 6 As shown, Figure 6 This is a SEM image of the carbon-based ammonia cracking hydrogen production catalyst Co3Mg / K-CNO' prepared by adjusting the Co-Mg atomic molar ratio to 3:1. This allows Co and Mg to be uniformly deposited on the K-CNO' support at an atomic molar ratio of 3:1, giving the catalyst excellent ammonia cracking performance.

[0065] Comparative Example 4

[0066] The CoMg / K-CNO' catalyst was prepared following the same steps as in Example 2, but 5.82 g of Co(NO3)2·6H2O was used in the catalyst preparation step. Figure 7 As shown, Figure 7 This is a SEM image of the carbon-based ammonia cracking hydrogen production catalyst CoMg / K-CNO' prepared by adjusting the Co-Mg atomic molar ratio to 1:1. This allows Co and Mg to be uniformly deposited on the K-CNO' support at an atomic molar ratio of 1:1, giving the catalyst excellent ammonia cracking performance.

[0067] Example 3: Catalyst Performance Testing

[0068] The catalysts prepared in Example 2 and the comparative example were evaluated for performance. 0.1 g of catalyst was charged into a fixed-bed reactor and reduced for 2 h at 500 °C and 30 mL / min under a 50% H₂ / Ar atmosphere. Then, the temperature was lowered to the reaction temperature, and NH₃ was introduced, controlling the space velocity (GHSV) at 12000 mL·g⁻¹. cat -1 ·h -1 The composition of the exhaust gas was analyzed by gas chromatography to calculate the ammonia conversion rate.

[0069] The results are shown in Table 1:

[0070] Table 1. Ammonia conversion results under different catalysts

[0071] catalyst Ammonia conversion rate at 550℃ (%) <![CDATA[Co2Mg / K-CNO']]> 99.6% <![CDATA[Co4Mg / K-CNO']]> 92.5% <![CDATA[Co3Mg2 / K-CNO']]> 93.8% <![CDATA[Co3Mg / K-CNO']]> 98.9% CoMg / K-CNO' 96.7%

[0072] like Figure 8The comparison of ammonia decomposition activities of different catalysts shows that the Co2Mg / K-CNO' catalyst prepared in this invention exhibits extremely excellent low-temperature ammonia decomposition activity. Performance testing of carbon-based catalysts prepared with different Co-Mg ratios demonstrates that the prepared Co2Mg / K-CNO' catalyst... x Mg y All / K-CNO' carbon-based ammonia cracking catalysts exhibit excellent ammonia cracking conversion rates, indicating that they all possess superior catalytic performance, with Co2Mg / K-CNO' showing the best performance.

[0073] Example 4: Catalyst stability test

[0074] At 500℃, GHSV = 600 mL·g cat -1 ·h -1 Under these conditions, the Co2Mg / K-CNO' catalyst underwent a continuous operation test for up to 90 hours. Figure 9 The results of the ammonia cracking conversion-runtime graph of the medium-carbon-based ammonia cracking hydrogen production catalyst Co2Mg / K-CNO' show that the ammonia conversion rate remained at around 99.7%, indicating that the catalyst exhibited excellent stability. Figure 9 As shown, Figure 9 To investigate the excellent catalytic performance of the carbon-based ammonia cracking hydrogen production catalyst Co2Mg / K-CNO', a long-term stability test was conducted, and the results showed that Co2Mg / K-CNO' maintained excellent catalytic performance at 500℃ and GHSV = 600 mL·g. cat -1 ·h -1 Under the specified conditions, the catalyst prepared by this method can operate stably for up to 90 hours, indicating that it has the ability to operate stably for a long period of time.

[0075] In summary, this invention successfully prepared a high-performance, low-cost ammonia decomposition hydrogen production catalyst through innovative carrier pretreatment and component design, solving the problems of insufficient low-temperature activity and poor stability of existing non-precious metal catalysts, and has good prospects for industrial application.

[0076] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0077] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for preparing a carbon-based ammonia cracking catalyst for hydrogen production, characterized in that, The preparation method includes the following steps: S1. Carrier pretreatment: The nano-onion carbon is sequentially subjected to acid washing and potassium salt solution immersion activation treatment. The nano-onion carbon is referred to as CNOs below to obtain the activated carrier K-CNO'. The pickling process is as follows: CNOs are dispersed in a 1M hydrochloric acid solution, stirred for 12-36 hours, filtered, washed until neutral, and dried at 100-150 °C to obtain CNO'; The potassium salt solution impregnation and activation process is as follows: CNO' obtained after acid washing and drying is added to 1M potassium carbonate K2CO3 solution, stirred at 90-100 ℃ for 12-36 hours, then filtered, dried, and calcined at 300-400 ℃ for 1-3 hours to obtain K-CNO'; S2. Catalyst Preparation: Using a uniform deposition precipitation method, cobalt salt, magnesium salt, urea, and the activated support K-CNO' are mixed in an aqueous solution and reacted under heating and stirring conditions, causing cobalt and magnesium hydroxides or carbonates to be uniformly deposited on the activated support K-CNO'. After the reaction is complete, the catalyst Co is obtained through filtration, washing, drying, and calcination. x Mg y / K-CNO'.

2. The preparation method according to claim 1, characterized in that, In step S2, the cobalt salt is cobalt nitrate Co(NO3)2·6H2O, and the magnesium salt is magnesium nitrate Mg(NO3)2·6H2O.

3. The preparation method according to claim 2, characterized in that, In step S2, the molar ratio of urea to the total of cobalt salt and magnesium salt is (3-5):

1.

4. The preparation method according to claim 1, characterized in that, In step S2, the molar ratio of cobalt to magnesium is 1-4:

1.

5. The preparation method according to claim 4, characterized in that, In step S2, the total loading of cobalt and magnesium accounts for 25%-35% of the total mass of the catalyst by metal mass.

6. The preparation method according to claim 1, characterized in that, In step S2, the temperature for heating and stirring the reaction is 90-100℃, and the time is 20-28 hours.

7. The preparation method according to claim 1, characterized in that, In step S2, the calcination conditions are as follows: in air or an inert atmosphere, the temperature is raised to 450-550℃ at a rate of 1-5℃ / min and held for 3-5 hours.

8. The application of a carbon-based ammonia cracking hydrogen production catalyst prepared according to any one of claims 1 to 7 in ammonia cracking hydrogen production, characterized in that, Before being used in the ammonia cracking reaction, the catalyst is first subjected to a reduction pretreatment at 450-550°C for 1-3 hours in a hydrogen atmosphere; The conditions for the ammonia decomposition reaction are: reaction temperature 450-600 ℃, and space velocity 6000-15000 mL·g. cat -1 ·h -1 .

Citation Information

Patent Citations

  • Nickel and / or ruthenium-based ammonia decomposition catalyst and preparation method and application thereof

    CN110270338A