Transparent temperature-resistant polyester composite material containing regenerated material and preparation method of transparent temperature-resistant polyester composite material

By blending RPET and PCT-G and adding composite antioxidants, the environmental protection, performance and stability issues of transparent polyester materials at high PCR content have been solved, resulting in polyester composite materials with high transparency, toughness and environmental stability, suitable for a variety of processing and application scenarios.

CN121699353APending Publication Date: 2026-03-20SHANGHAI SHENGTAIPU NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511974742.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-25
Publication Date
2026-03-20

AI Technical Summary

Technical Problem

Existing transparent polyester materials, when subjected to high PCR content, struggle to balance environmental friendliness, performance stability, compliance, and environmental stability. In particular, they are prone to yellowing, brittleness, and decreased light transmittance under high temperature and humidity conditions.

Method used

A transparent, heat-resistant polyester composite material is formed by blending recycled polyethylene terephthalate (RPET) and polyethylene glycol-1,4-cyclohexanediethanol terephthalate (PCT-G) in a specific ratio, combined with composite antioxidants, compatibilizers, anti-hydrolysis agents and nucleating agents, and through precise optimization of preparation process parameters.

Benefits of technology

It achieves high transparency, excellent toughness and impact resistance, meets food contact grade certification, is resistant to high temperature and high humidity environments, and is suitable for a variety of processing methods and application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the field of high polymer materials, and particularly relates to a transparent temperature-resistant polyester composite material containing regenerated materials and a preparation method of the transparent temperature-resistant polyester composite material. The composite material is prepared from the following raw materials in parts by weight: 30 to 70 parts of food contact grade recycled polyethylene glycol terephthalate (RPET), 30 to 70 parts of polyethylene terephthalate-1, 4-cyclohexanedimethanol ester (PCT-G), 0.3 to 0.5 part of composite antioxidant, 1 to 5 parts of compatilizer and the like. The preparation method comprises the steps of raw material pretreatment drying, premixing, melt blending granulation and the like, and component compatibility is optimized by accurately controlling drying parameters, extrusion temperature and rotating speed. The method has the advantages of high PCR content, product light transmittance of more than or equal to 88%, haze of less than or equal to 2%, impact strength of more than or equal to 60J / m, temperature resistance, hydrolysis resistance, accordance with food contact authentication, simple process, low cost and suitability for the fields of packaging, medical treatment and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials, specifically relating to a transparent heat-resistant polyester composite material containing recycled materials and its preparation method. Background Technology

[0002] Against the backdrop of a deepening global "dual-carbon" strategy and the normalization of the circular economy, the high-proportion application of recycled plastics (PCR) has become a core development trend in the polymer materials industry. Food packaging, cosmetic containers, and medical assistive devices are among the sectors that place multiple stringent requirements on the environmental properties, performance stability, and safety compliance of polyester materials. Transparent polyester materials, due to their combination of aesthetics and practicality, have maintained an annual market demand growth rate of over 8% in these areas; however, existing products generally face the industry pain point of balancing environmental protection and performance.

[0003] Recycled polyethylene terephthalate (RPET) is a mainstream recycled polyester raw material. However, molecular chain degradation is inevitable during the recycling process, leading to a decrease in intrinsic viscosity (IV). This directly causes problems such as poor thermal stability, insufficient melt strength, and brittleness in processed products. Furthermore, repeated processing can cause yellowing due to free radical accumulation, resulting in a significant decrease in light transmittance, failing to meet the requirements for high-end transparent products. To compensate for the performance deficiencies of RPET, the industry often uses blending with polyethylene terephthalate-1,4-cyclohexanediol ester (PCT-G). However, the two have significantly different molecular chain structures, poor viscosity matching, and high interfacial tension. Blending easily leads to phase separation, causing product haze to soar to over 10%, a significant decrease in impact toughness, and difficulty in balancing transparency and mechanical properties.

[0004] Furthermore, sensitive fields such as food contact and medical applications have extremely strict controls on the source of recycled raw materials, requiring multiple qualification reviews, including NOL certification from the US FDA and EFSA certification from the EU, to ensure that no harmful substances migrate from the recycled components. Currently, polyester composite materials on the market either have a recycled content of less than 20% (insufficient environmental properties), or, while increasing the RPET ratio, sacrifice transparency or toughness, or lack compliance certifications to enter sensitive fields. An integrated solution that simultaneously meets the requirements of "high PCR content, high light transmittance, high impact toughness, and food contact compliance" is extremely rare. At the same time, existing materials are prone to hydrolytic aging in high temperature and humidity environments, further limiting their application in humid areas or long-term use scenarios. There is an urgent need to develop a new type of polyester composite material that balances environmental protection, performance, compliance, and environmental stability.

[0005] Therefore, based on this, the technical solution of the present invention is proposed. Summary of the Invention

[0006] To address the problems existing in the prior art, this invention provides a transparent, heat-resistant polyester composite material containing recycled materials, comprising the following raw materials in parts by weight: 30-70 parts of recycled polyethylene terephthalate (RPET), 30-70 parts of polyethylene terephthalate-1,4-cyclohexanediol ester (PCT-G), 0.3-0.5 parts of composite antioxidant, 1-5 parts of compatibilizer, 0.4-0.6 parts of lubricant, 0.2-1 parts of anti-hydrolysis agent, and 0.4-0.6 parts of nucleating agent.

[0007] Preferably, the transparent heat-resistant polyester composite material containing recycled materials comprises the following raw materials in parts by weight: 30 parts of recycled polyethylene terephthalate, 65.1 parts of polyethylene terephthalate-1,4-cyclohexanediol ester, 0.4 parts of composite antioxidant, 3 parts of compatibilizer, 0.5 parts of lubricant, 0.5 parts of anti-hydrolysis agent, and 0.5 parts of nucleating agent.

[0008] It should be noted that the recycled polyethylene terephthalate of the present invention is of food contact grade and meets relevant certification requirements.

[0009] To facilitate understanding of this invention, the functions of the relevant raw materials are explained: Food contact grade RPET: As the core recycled component, it establishes the material's environmentally friendly properties and cost advantages. Its intrinsic viscosity (IV) is preferably between 0.70-0.85 dl / g to ensure basic processing performance.

[0010] Polyethylene terephthalate-1,4-cyclohexanediethanol (PCT-G): As a continuous phase matrix, it provides the material with inherent high transparency, excellent toughness, and processing fluidity. Its high proportion ensures the overall toughness and amorphous properties of the blend, which is the foundation for maintaining high transparency. For example, ECOZEN, a product developed by SK Chemicals in South Korea, is BPA-free, has passed international safety certifications such as the US FDA, and is safe for direct contact with food and drinking water, possessing good heat resistance and transparency.

[0011] Composite antioxidants: They can effectively capture free radicals and decompose hydrogen peroxides. They work synergistically during processing and use to prevent the thermo-oxidative degradation and yellowing of polymer chains, and maintain the color and performance stability of the material.

[0012] Compatibilizer: The compatibilizer used in this invention (such as epoxy-functionalized styrene-acrylate copolymer) can react simultaneously with the terminal functional groups of the molecular chains of RPET and PCT-G, acting as a "bridging" agent. It not only repairs the broken molecular chains of RPET caused by recycling, but also significantly improves the interfacial adhesion between the dispersed phase of RPET and the continuous phase of PCT-G, effectively suppressing phase separation and light scattering caused by poor compatibility. Therefore, even with high recycling content, it still ensures low haze, high transparency, and excellent impact resistance of the material. For example, BASF's commercially available chain extender ADR-4468 is a food-grade chain extender with an epoxy equivalent of 310, a weight-average relative molecular mass of 7250, a glass transition temperature of 59°C, and contains 9 epoxy functional groups. It can be used for chain extension and thickening of polyesters and polyamides. Its basic functions are: to extend the molecular chain to increase the molecular weight of the polymer, to introduce long branched structure, to increase the melt strength of the polymer, and to improve the processing performance of the polymer (including blowing film, blowing bottle, sheet extrusion, thermoforming, foaming, spinning and other molding).

[0013] Anti-hydrolysis agent: It can quickly react with the carboxyl groups generated by the hydrolysis of polyester during the melting process, terminate the autocatalytic hydrolysis reaction, and greatly improve the stability of the material in high temperature and high humidity environments. This is crucial for ensuring the processing quality of recycled materials and the lifespan of the products.

[0014] Lubricants and nucleating agents: Lubricants improve the processing flowability and release properties of the material. Nucleating agents can be used to fine-tune the crystallization behavior of RPET microregions, which helps improve dimensional stability even though the overall material is amorphous.

[0015] Preferably, the composite antioxidant includes, but is not limited to, a combination of two or more of the following: phenolic 1010 antioxidant, phenolic 1076 antioxidant, phenolic 1330 antioxidant, phosphite 626 antioxidant, phosphite 168 antioxidant, and thioester antioxidant DLTP.

[0016] Preferably, the compatibilizer includes, but is not limited to, one of the following: epoxy functional group styrene-acrylate copolymer, epoxy functional group methyl methacrylate-butadiene-styrene copolymer, maleic anhydride-grafted polybutylene terephthalate, ethylene-methyl acrylate-glycidyl methacrylate copolymer, and maleic anhydride-grafted styrene-ethylene-butene-styrene copolymer.

[0017] Preferably, the lubricant includes, but is not limited to, lignite wax ester, stearate, ethylene bis-stearamide, and pentaerythritol tetrastearate.

[0018] Preferably, the anti-hydrolysis agent includes, but is not limited to, one of carbodiimide anti-hydrolysis agents, phthalic anhydride anti-hydrolysis agents, and bisphenol A type epoxy resin anti-hydrolysis agents.

[0019] Preferably, the nucleating agent includes, but is not limited to, one of methyl dibenzyl sorbitol, sodium benzoate-organophosphate salt complex, calcium stearate, and talc-silica composite micro powder.

[0020] Based on the same technical concept, another aspect of the present invention is to provide a method for preparing a transparent heat-resistant polyester composite material containing recycled materials, the preparation method comprising the following steps: (1) Pretreatment and drying: All raw materials are dried to obtain dried raw materials; (2) Premixing: Mix all the dried raw materials to obtain a mixed raw material; (3) Melt blending and granulation: The mixed raw materials are put into an extruder for melt blending, extrusion, cooling and pelletizing to obtain the transparent heat-resistant polyester composite material containing recycled materials.

[0021] Preferably, in step (1): The recovered polyethylene terephthalate and polyethylene terephthalate-1,4-cyclohexanediol ester were dried at 120-130℃ for 5-6 hours to reduce the moisture content to less than 50ppm. And / or, dry the remaining raw materials at 60-80℃ for 2-3 hours.

[0022] Preferably, in step (3): The extrusion temperatures of the extruder are as follows: from zone one to zone five, the temperatures are 235℃, 250℃, 255℃, 250℃, and 245℃, respectively. And / or, the screw speed of the extruder is 300-350 r / min; And / or, the vacuum degree during the extruder operation is -0.06 to -0.08 MPa.

[0023] The beneficial effects of this invention are as follows: This invention addresses the technical problems of existing recycled polyester materials, such as the difficulty in balancing high PCR content and high performance, poor compatibility leading to deterioration in transparency and toughness, insufficient compliance, and poor environmental stability. By precisely proportioning raw material components and optimizing preparation process parameters, this invention provides a transparent, heat-resistant polyester composite material containing recycled materials and its preparation method. This achieves a synergistic balance of environmental protection properties, mechanical properties, optical properties, compliance, and processing stability, solving a core pain point in the industry.

[0024] 1. Dual compliance with environmental protection and compliance standards: Using 30-70 parts of food contact grade RPET (IV value 0.70-0.85dl / g) as the core recycled component, the PCR content meets the environmental protection requirements of mainstream brands, and the raw materials have passed authoritative certifications such as FDA and EFSA, with no risk of harmful substance migration. It can be directly applied to sensitive areas such as food contact and cosmetic packaging, with low market entry barriers.

[0025] 2. Synergistic optimization of optical and mechanical properties: Through the "bridging effect" of 1-5 parts of epoxy functional group styrene-acrylate copolymer compatibilizer, the compatibility problem between RPET and PCT-G is completely solved, suppressing phase separation and light scattering. The light transmittance of the product reaches more than 88%, and the haze is less than 2%. At the same time, the degraded molecular chains of RPET are repaired, the cantilever beam notched impact strength is maintained above 60J / m, and the tensile strength is ≥45MPa. It takes into account both high transparency and high toughness, meeting the use requirements of high-end transparent products.

[0026] 3. Excellent processing and environmental stability: The composite antioxidant (phenol 1010 + phosphite 168) and carbodiimide anti-hydrolysis agent work synergistically to effectively inhibit thermo-oxidative degradation and hydrolytic aging in the secondary processing of RPET, avoid yellowing and performance degradation of the products, and significantly extend their service life.

[0027] 4. Significant cost and process advantages: The high RPET usage significantly reduces raw material costs, and the preparation process uses a conventional twin-screw extruder, requiring no special equipment modification. The parameters of steps such as drying, premixing, and melt blending are clear and controllable, resulting in high production efficiency and easy industrial scaling.

[0028] 5. Wide range of applications: The material has multiple advantages such as high transparency, high toughness, temperature resistance, environmental protection, and compliance. It can be processed into food packaging boxes, beverage bottles, cosmetic bottles, medical trays and other products through various processing methods such as injection molding, blow molding and extrusion, covering multiple fields such as packaging, medical care and daily necessities, with huge market application potential. Detailed Implementation

[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be described in detail below. Obviously, the described embodiments are merely some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0030] Example 1 This embodiment provides a method for preparing a transparent, heat-resistant polyester composite material containing recycled materials. The preparation method includes the following steps (detailed): (1) Raw material preparation and specification confirmation The following raw materials were weighed sequentially: 30 kg of RPET granules (intrinsic viscosity IV = 0.75 dl / g, food contact grade, FDA NOL certified), 65.1 kg of PCT-G granules (model ECOZEN), 0.4 kg of composite antioxidant (a mixture of 0.2 kg of phenolic 1010 antioxidant and 0.2 kg of phosphite 168 antioxidant by weight), 3 kg of epoxy functionalized styrene-acrylate copolymer compatibilizer (epoxy value 0.3 mol / 100g, molecular weight 20000), 0.5 kg of lignite wax ester lubricant (acid value ≤ 5 mg KOH / g), 0.5 kg of carbodiimide anti-hydrolysis agent (molecular weight 3000), and 0.5 kg of sorbitol nucleating agent (DBS, purity ≥ 99%). Clearly defining the specifications and purity of the raw materials ensures the stability and compatibility of the properties of each component, avoiding performance fluctuations in the composite material due to batch differences in raw materials. Furthermore, the food contact grade raw materials and compliance certifications lay the foundation for subsequent applications in sensitive fields.

[0031] (2) Raw material pretreatment and graded drying: (2-1) Start the dehumidifying drying oven (model CD-100, wind speed 2m / s), put RPET granules and PCT-G granules into the first chamber of the drying oven, set the temperature to 125℃ and the drying time to 5h, monitor the moisture content in real time, and ensure that the final moisture content is less than 50ppm. (2-2) Add the composite antioxidant, compatibilizer, lubricant, anti-hydrolysis agent and nucleating agent into the second chamber of the drying oven, set the temperature to 60℃, the drying time to 2h, and the wind speed to 1.5m / s to remove the adsorbed moisture on the surface of the raw materials. Graded drying adapts to the moisture tolerance characteristics of different raw materials. High-temperature, long-term drying of RPET and PCT-G can completely remove internal water of crystallization and avoid hydrolysis during melt processing. Low-temperature, short-time drying of small molecule additives can prevent thermal decomposition, and wind speed control ensures uniform drying.

[0032] (3) High-speed premixed dispersion: All dried raw materials were added to a high-speed mixer in sequence. The speed was set to 1500 r / min and the mixing time to 5 min. The material temperature was monitored in real time during the mixing process (controlled to ≤40℃). After the mixing was completed, the machine was stopped to observe the material state to ensure that there were no lumps or stratification, and that a uniformly mixed raw material was obtained. High-speed, short-time mixing can achieve uniform micro-dispersion of each component, avoid agglomeration of small molecule additives such as compatibilizers and antioxidants, and material temperature control can prevent premature melting and agglomeration, laying a uniform foundation for the interface reaction of subsequent melt blending.

[0033] (4) Twin-screw melt blending extrusion: A twin-screw extruder (40:1 L / D ratio) was selected. The mixed raw materials were uniformly fed into the extruder hopper through a metering feeder. The temperatures of each zone of the extruder were set as follows: Zone 1 235℃, Zone 2 250℃, Zone 3 255℃, Zone 4 250℃, and Zone 5 245℃. The screw speed was 300 r / min, and the vacuum degree was -0.06 MPa. Metering feeding ensured a stable raw material feeding rate and avoided extruder load fluctuations. The gradient temperature setting was adapted to the melting characteristics of RPET and PCT-G. The high temperature in the three zones promoted molecular chain reaction, while the low temperature at both ends prevented material degradation. The appropriate screw speed and vacuum degree enhanced the shear dispersion effect, removed volatiles and bubbles from the melt, and improved the material density.

[0034] (5) Cooling, shaping, and pelletizing: (5-1) The molten strip extruded from the extruder die enters the water cooling tank (water temperature 25℃, water depth 15cm, cooling length 2m), cools for 30s until the surface temperature of the strip is ≤40℃, and then is uniformly pulled to the pelletizer by the traction machine (traction speed 5m / min). (5-2) Set the pelletizer speed to 500 r / min, the pellet size to 3 mm, and the pellet length to 3 ± 0.2 mm. After pelleting, the pellets are screened through a vibrating screen (screen mesh size 2.8 mm and 3.2 mm) to remove unqualified pellets. Precise control of water cooling parameters can quickly solidify the melt strip, avoiding uneven crystallization that affects transparency; matching the traction speed with the pelletizing speed ensures uniform particle size; vibration screening can remove oversized or undersized particles, ensuring product consistency and facilitating subsequent injection molding, blow molding and other processing steps.

[0035] (6) Finished product testing and storage: (6-1) Randomly select 100g of finished granules and test the moisture content (≤30ppm) and particle size distribution (pass rate ≥98%); inject the granules into standard samples and test their light transmittance, haze, impact strength and other properties. (6-2) Qualified finished products shall be vacuum-packed in aluminum foil composite bags (vacuum degree -0.09MPa) and stored in a dry and ventilated warehouse (temperature 20-25℃, humidity ≤60%), with a shelf life of 12 months; Finished product testing ensures that the product meets quality standards, while vacuum packaging and standardized storage prevent particles from absorbing moisture and oxidizing, thus extending shelf life.

[0036] Example 2 This embodiment provides a method for preparing a transparent, heat-resistant polyester composite material containing recycled materials. The preparation method includes the following steps (briefly described): (1) Raw material preparation: Weigh out 70 kg of RPET granules, 27.7 kg of PCT-G granules, 0.3 kg of composite antioxidant (including 0.15 kg of phenolic 1010 antioxidant and 0.15 kg of phosphite 168 antioxidant), 1 kg of epoxy functional group styrene-acrylate copolymer compatibilizer, 0.4 kg of lignite wax ester lubricant, 0.2 kg of carbodiimide anti-hydrolysis agent and 0.4 kg of nucleating agent in sequence.

[0037] (2) Pretreatment and drying: RPET granules and PCT-G granules were dried in a dehumidifying drying oven at 125°C for 5 hours to reduce the moisture content to less than 50 ppm; the remaining raw materials were dried at 60°C for 2 hours.

[0038] (3) Premixing: Pour the dried RPET particles, PCT-G particles, compatibilizer, anti-hydrolysis agent, composite antioxidant, lubricant and nucleating agent into a high-speed mixer and mix for 5 minutes until the mixture is uniform to obtain the mixed raw materials.

[0039] (4) Melt blending and granulation: The mixed raw materials are fed into an extruder for melt blending, extrusion, cooling and pelletizing to obtain the transparent heat-resistant polyester composite material containing recycled materials; wherein: the temperatures from zone one to zone five are set to 235℃, 250℃, 255℃, 250℃ and 245℃ respectively; the screw speed of the extruder is 300r / min; the vacuum degree during the working process of the extruder is -0.06MPa.

[0040] Example 3 This embodiment provides a method for preparing a transparent, heat-resistant polyester composite material containing recycled materials. The preparation method includes the following steps (briefly described): (1) Raw material preparation: Weigh out 50 kg of RPET granules, 43.2 kg of PCT-G granules, 0.5 kg of composite antioxidant (including 0.25 kg of phenolic 1010 antioxidant and 0.25 kg of phosphite 168 antioxidant), 5 kg of epoxy functional group styrene-acrylate copolymer compatibilizer, 0.6 kg of lignite wax ester lubricant, 0.1 kg of carbodiimide anti-hydrolysis agent and 0.6 kg of nucleating agent in sequence.

[0041] (2) Pretreatment and drying: RPET granules and PCT-G granules were dried in a dehumidifying drying oven at 125°C for 5 hours to reduce the moisture content to less than 50 ppm; the remaining raw materials were dried at 60°C for 2 hours.

[0042] (3) Premixing: The dried RPET particles, PCT-G particles, compatibilizer, anti-hydrolysis agent, composite antioxidant, lubricant and nucleating agent are poured into a high-speed mixer and mixed for 10 minutes until they are uniformly mixed to obtain the mixed raw materials.

[0043] (4) Melt blending and granulation: The mixed raw materials are fed into an extruder for melt blending, extrusion, cooling and pelletizing to obtain the transparent heat-resistant polyester composite material containing recycled materials; wherein: the temperatures from zone one to zone five are set to 235℃, 250℃, 255℃, 250℃ and 245℃ respectively; the screw speed of the extruder is 300r / min; the vacuum degree during the working process of the extruder is -0.08MPa.

[0044] Comparative Example Compared with Example 1, no compatibilizer was added in this comparative example, but all other operations were the same as in Example 1.

[0045] Verification Example The test samples obtained from Examples 1-3 and the comparative example were tested, and the results are shown in Table 1.

[0046] Table 1

[0047] As shown in Table 1, the epoxy compatibilizer in the formulation of this invention plays a crucial role. By improving interfacial compatibility, it enables the material to achieve transparency and toughness comparable to many virgin materials while maintaining a high recycled content. The technical effect is significant and unexpected.

[0048] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A transparent, heat-resistant polyester composite material containing recycled materials, characterized in that, The preparation raw materials include the following parts by weight: 30-70 parts of recycled polyethylene terephthalate, 30-70 parts of polyethylene terephthalate-1,4-cyclohexanediol ester, 0.3-0.5 parts of composite antioxidant, 1-5 parts of compatibilizer, 0.4-0.6 parts of lubricant, 0.2-1 parts of anti-hydrolysis agent, and 0.4-0.6 parts of nucleating agent.

2. The transparent, heat-resistant polyester composite material containing recycled materials according to claim 1, characterized in that, The preparation raw materials include the following parts by weight: 30 parts of recycled polyethylene terephthalate, 65.1 parts of polyethylene terephthalate-1,4-cyclohexanediol ester, 0.4 parts of composite antioxidant, 3 parts of compatibilizer, 0.5 parts of lubricant, 0.5 parts of anti-hydrolysis agent, and 0.5 parts of nucleating agent.

3. The transparent, heat-resistant polyester composite material containing recycled materials according to claim 1 or 2, characterized in that, The composite antioxidant includes a combination of two or more of the following: phenolic 1010 antioxidant, phenolic 1076 antioxidant, phenolic 1330 antioxidant, phosphite 626 antioxidant, phosphite 168 antioxidant, and thioester antioxidant DLTP.

4. The transparent, heat-resistant polyester composite material containing recycled materials according to claim 1 or 2, characterized in that, The compatibilizer is one of the following: epoxy functional group styrene-acrylate copolymer, epoxy functional group methyl methacrylate-butadiene-styrene copolymer, maleic anhydride-grafted polybutylene terephthalate, ethylene-methyl acrylate-glycidyl methacrylate copolymer, and maleic anhydride-grafted styrene-ethylene-butene-styrene copolymer.

5. The transparent, heat-resistant polyester composite material containing recycled materials according to claim 1 or 2, characterized in that, The lubricant is one of lignite wax ester, stearate, ethylene bis-stearamide, and pentaerythritol tetrastearate.

6. The transparent, heat-resistant polyester composite material containing recycled materials according to claim 1 or 2, characterized in that, The anti-hydrolysis agent is one of the following: carbodiimide anti-hydrolysis agent, phthalic anhydride anti-hydrolysis agent, and bisphenol A type epoxy resin anti-hydrolysis agent.

7. The transparent, heat-resistant polyester composite material containing recycled materials according to claim 1 or 2, characterized in that, The nucleating agent is one of the following: methyl dibenzyl sorbitol, sodium benzoate-organophosphate salt complex, calcium stearate, and talc-silica composite micro powder.

8. A method for preparing the transparent heat-resistant polyester composite material containing recycled materials according to any one of claims 1-7, characterized in that, The preparation method includes the following steps: (1) Pretreatment and drying: All raw materials are dried to obtain dried raw materials; (2) Premixing: Mix all the dried raw materials to obtain a mixed raw material; (3) Melt blending and granulation: The mixed raw materials are put into an extruder for melt blending, extrusion, cooling and pelletizing to obtain the transparent heat-resistant polyester composite material containing recycled materials.

9. The method for preparing the transparent heat-resistant polyester composite material containing recycled materials according to claim 8, characterized in that, In step (1): The recovered polyethylene terephthalate and polyethylene terephthalate-1,4-cyclohexanediol ester were dried at 120-130℃ for 5-6 hours to reduce the moisture content to less than 50ppm. And / or, dry the remaining raw materials at 60-80℃ for 2-3 hours.

10. The method for preparing the transparent heat-resistant polyester composite material containing recycled materials according to claim 8, characterized in that, In step (3): The extrusion temperatures of the extruder are as follows: from zone one to zone five, the temperatures are 235℃, 250℃, 255℃, 250℃, and 245℃, respectively. And / or, the screw speed of the extruder is 300-350 r / min; And / or, the vacuum degree during the extruder operation is -0.06 to -0.08 MPa.