Sandwich-type alpha-diimine ligand and preparation method thereof, nickel catalyst and preparation method and application thereof

By using a sandwich-type α-diimine ligand and nickel catalyst, the problem of synthesizing bimodal polyethylene in a single reactor was solved, achieving efficient preparation of bimodal polyethylene with a wide distribution and improving the processing and application performance of the polymer.

CN121872944APending Publication Date: 2026-04-17CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610034213.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-12
Publication Date
2026-04-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to achieve efficient synthesis of bimodal polyethylene in a single reactor, especially when introducing two active centers into the polymerization system to achieve simultaneous synthesis of high and low molecular weight polymers.

Method used

By employing sandwich-type α-diimine ligands and nickel catalysts, a nickel catalyst with dual active centers was prepared through the reaction of ligands and catalysts with specific structures in an organic solvent, enabling the preparation of bimodal polyethylene in a single reactor.

Benefits of technology

This method enables the efficient preparation of bimodal polyethylene with a wide molecular weight distribution in a single reactor. The polymer has a wide molecular weight distribution, including both high and low molecular weight fractions, which improves the processing and performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121872944A_ABST
    Figure CN121872944A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysis, and particularly relates to a sandwich-type alpha-diimine ligand, a preparation method thereof, a nickel catalyst and a preparation method and application thereof. The sandwich-type alpha-diimine ligand provided by the invention has a structure shown as a formula (I), and in the formula (I), R1 is perfluoro-n-butyl or n-butyl, and R2 is hydrogen or tert-butyl. The nickel catalyst prepared from the ligand disclosed by the invention can present two different configurations in ethylene polymerization to realize double active centers, so that wide-distribution bimodal polyethylene can be produced in a single reactor. Formula (I).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalysis technology, and particularly relates to a sandwich-type α-diimine ligand, its preparation method, a nickel catalyst and its preparation method and application. Background Technology

[0002] Polyethylene is the world's most produced and widely used synthetic polymer material. Its varied chain structure gives it a broad spectrum of properties, including rigid ultra-high molecular weight polyethylene (UHMWPE) and high-density polyethylene (HDPE), as well as softer polyolefin elastomers (POE) and polyolefin oils and waxes. The polymer's microstructure determines the material's performance, while the control of the polymer's molecular weight distribution corresponds to its processing performance. Polyethylene with a broad molecular weight distribution often has better processing performance. Its microstructure contains both high and low molecular weight segments. The low molecular weight segments act as lubricants to improve the material's processing performance, while the high molecular weight segments ensure the material's performance in use. Ziegler-Natta catalysts and Phillips catalysts, due to their multi-center characteristics, produce polymers with a broad molecular weight distribution, but they are less effective at controlling the polymer structure. In contrast, catalysts with a single active center and a well-defined structure produce polymers with better control over their structure, but the distribution is generally narrower, such as post-transition nickel catalysts.

[0003] Bimodal polyethylene is a typical type of broadly distributed polyethylene, and in industry, it is often synthesized using a multi-reactor series process. Currently, the preparation of bimodal polyethylene using a single reactor is mostly still in the experimental research stage. The key lies in introducing two active centers into the polymerization system to achieve the simultaneous synthesis of high and low molecular weight polymers. Summary of the Invention

[0004] In view of this, the purpose of the present invention is to provide a sandwich-type α-diimine ligand, its preparation method, a nickel catalyst, its preparation method and application, wherein the nickel catalyst prepared by the ligand of the present invention can realize the preparation of bimodal polyethylene in a single reactor.

[0005] This invention provides a sandwich-type α-diimine ligand having the structure of formula (I):

[0006] Formula (I);

[0007] In equation (I), R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0008] Preferably, the sandwich-type α-diimine ligand is any one of formulas (I-1) to (I-4):

[0009] Formula (I-1); Formula (I-2);

[0010] Formula (I-3); Formula (I-4).

[0011] This invention provides a method for preparing the sandwich-type α-diimine ligand described above, comprising the following steps:

[0012] Compound of formula (II) and catalyst are mixed in an organic solvent and heated to react, yielding sandwich-type α-diimine ligand of formula (I);

[0013] Formula (I);

[0014] Formula (II); Formula (III);

[0015] Among them, R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0016] Preferably, the molar ratio of the compound with structure (II) to the compound with structure (III) is (2~2.5):1.

[0017] Preferably, the catalyst is p-toluenesulfonic acid.

[0018] This invention provides a nickel catalyst having the structure of formula (IV):

[0019] Formula (IV);

[0020] In equation (IV), R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0021] Preferably, the nickel catalyst is any one of formulas (IV-1) to (IV-4):

[0022] Formula (IV-1); Formula (IV-2);

[0023] Formula (IV-3); Formula (IV-4).

[0024] This invention provides a method for preparing the nickel catalyst described in the above technical solution, comprising the following steps:

[0025] The ligand of formula (I) and nickel bromide of ethylene glycol dimethyl ether were mixed and reacted in an organic solvent to obtain the nickel catalyst of formula (IV);

[0026] Formula (I); Formula (IV);

[0027] Among them, R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0028] Preferably, the molar ratio of the ligand of formula (I) to nickel dimethyl ether ethylene glycol bromide is 1:(1~5).

[0029] This invention provides a method for ethylene polymerization, comprising the following steps:

[0030] Ethylene undergoes catalytic polymerization in the presence of a catalyst to obtain polyethylene;

[0031] The catalyst includes the nickel catalyst described in the above technical solution or the nickel catalyst prepared by the preparation method described in the above technical solution.

[0032] Compared with the prior art, the present invention provides a sandwich-type α-diimine ligand, its preparation method, a nickel catalyst, the preparation method thereon, and its application. The sandwich-type α-diimine ligand provided by the present invention has the structure of formula (I), where R... 1 It is perfluoro-n-butyl or n-butyl, R 2 It can be hydrogen or tert-butyl. The nickel catalyst prepared by the ligands of this invention can achieve dual active centers by exhibiting two different configurations in ethylene polymerization, thereby enabling the production of broadly distributed bimodal polyethylene in a single reactor. Attached Figure Description

[0033] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.

[0034] Figure 1 This is the 1H NMR spectrum of the perfluoroaromatic amine provided in the embodiments of the present invention;

[0035] Figure 2 This is the proton NMR spectrum of ligand L-C4H9 provided in this embodiment of the invention;

[0036] Figure 3This is a single-crystal structure diagram of the nickel catalyst Ni-C4H9 provided in the embodiments of the present invention. Detailed Implementation

[0037] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0038] This invention provides a sandwich-type α-diimine ligand having the structure of formula (I):

[0039] Formula (I);

[0040] In equation (I), R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0041] In this invention, the sandwich-type α-diimine ligand can specifically be any one of formulas (I-1) to (I-4):

[0042] Formula (I-1); Formula (I-2);

[0043] Formula (I-3); Formula (I-4).

[0044] The present invention also provides a method for preparing the sandwich-type α-diimine ligand described in the above technical solution, comprising the following steps:

[0045] Compound of formula (II) and catalyst are mixed in an organic solvent and heated to react, yielding sandwich-type α-diimine ligand of formula (I);

[0046] Formula (I);

[0047] Formula (II); Formula (III);

[0048] Among them, R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0049] In the ligand preparation method provided by the present invention, the molar ratio of the compound with structure (II) to the compound with structure (III) is preferably (2~2.5):1, specifically 2:1, 2.05:1, 2.1:1, 2.15:1, 2.2:1, 2.25:1, 2.3:1, 2.35:1, 2.4:1, 2.45:1 or 2.5:1.

[0050] In the ligand preparation method provided by the present invention, the catalyst is preferably p-toluenesulfonic acid; the amount of the catalyst is preferably sufficient.

[0051] In the ligand preparation method provided by the present invention, the organic solvent is preferably one or more of toluene, benzene, acetonitrile, acetic acid and tetrahydrofuran.

[0052] In the ligand preparation method provided by the present invention, the heating reaction is preferably carried out under reflux conditions; the heating reaction is preferably carried out under stirring conditions; the heating reaction time is preferably 1 to 14 days, specifically 1 day, 2 days, 3 days, 4 days, 5 days, 6 days, 7 days, 8 days, 9 days, 10 days, 11 days, 12 days, 13 days or 14 days.

[0053] In the ligand preparation method provided by the present invention, after the heating reaction is completed, the reaction product is post-processed to obtain the ligand with the structure of formula (I). Preferably, the post-processing includes: after the heating reaction is completed, cooling, solvent removal, and column chromatography purification to obtain the sandwich-type α-diimine ligand with the structure of formula (I).

[0054] The present invention also provides a nickel catalyst having the structure of formula (IV):

[0055] Formula (IV);

[0056] In equation (IV), R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0057] In this invention, the nickel catalyst may specifically be any one of formulas (IV-1) to (IV-4):

[0058] Formula (IV-1); Formula (IV-2);

[0059] Formula (IV-3); Formula (IV-4).

[0060] The present invention also provides a method for preparing the nickel catalyst described in the above technical solution, comprising the following steps:

[0061] The ligand of formula (I) and nickel ethylene glycol dimethyl ether bromide (NiBr2(DME)) were mixed and reacted in an organic solvent to obtain the nickel catalyst of formula (IV);

[0062] Formula (I); Formula (IV);

[0063] Among them, R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

[0064] In the nickel catalyst preparation method provided by the present invention, the molar ratio of the ligand of formula (I) structure to nickel bromide of ethylene glycol dimethyl ether is preferably 1: (1~5), specifically 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0065] In the nickel catalyst preparation method provided by the present invention, the organic solvent is preferably dichloromethane and / or chloroform.

[0066] In the nickel catalyst preparation method provided by the present invention, the mixing reaction is preferably carried out under stirring conditions; the temperature of the mixing reaction is preferably 20~50℃, specifically 20℃, 25℃, 30℃, 35℃, 40℃, 45℃ or 50℃; the time of the mixing reaction is preferably 12~60h, specifically 12h, 16h, 20h, 24h, 28h, 32h, 36h, 40h, 44h, 48h, 52h, 56h or 60h.

[0067] In the nickel catalyst preparation method provided by the present invention, after the mixing reaction is completed, the reaction product is post-treated to obtain a nickel catalyst with formula (IV). Preferably, the post-treatment process includes: after the mixing reaction is completed, solvent removal, washing with n-hexane, filtration, washing with diethyl ether, and drying to obtain the nickel catalyst with formula (IV).

[0068] The present invention also provides a method for ethylene polymerization, comprising the following steps:

[0069] Ethylene undergoes catalytic polymerization in the presence of a catalyst to obtain polyethylene;

[0070] The catalyst includes the nickel catalyst described in the above technical solution or the nickel catalyst prepared by the preparation method described in the above technical solution.

[0071] In the ethylene polymerization method provided by the present invention, the catalyst preferably further includes a co-catalyst, which includes, but is not limited to, one or more of diethylaluminum chloride (DEAC), sesquiethylaluminum chloride (EASC), modified methylaluminoxane (MMAO), trimethylaluminum (TMA), and triisobutylaluminum (TIBA).

[0072] In the ethylene polymerization method provided by the present invention, the ethylene pressure for catalytic polymerization is preferably 6-20 bar, specifically 6 bar, 7 bar, 8 bar, 9 bar, 10 bar, 11 bar, 12 bar, 13 bar, 14 bar, 15 bar, 16 bar, 17 bar, 18 bar, 19 bar, or 20 bar; the temperature for catalytic polymerization is preferably 40-60°C, specifically 40°C, 45°C, 50°C, 55°C, or 60°C; and the time for catalytic polymerization is preferably 20-60 min, specifically 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, or 60 min.

[0073] For clarity, the following examples will be used to provide a detailed description.

[0074] Example 1

[0075] The chemical reaction formula for the preparation of perfluoroaromatic amines is as follows:

[0076] .

[0077] The specific preparation steps include:

[0078] Step 1: Under an inert atmosphere (nitrogen), 5-bromo-6-nitro-1,2-dihydroacenaphthene (a, 1 equivalent, 3 g, 0.01 mol), copper powder (5 equivalent, 3.43 g, 0.05 mol), perfluoroiodobutane (b, 1 equivalent, 4.11 g), and 150 mL of DMSO were placed in a reactor and stirred at 100 °C for 3 days in the dark. After the reaction was completed, the mixture was cooled to room temperature, and the reddish-brown suspension was poured into 300 mL of water and stirred for another 30 minutes. The mixture was then filtered and washed three times with diethyl ether. The filtrates were combined, separated, and the aqueous phase was washed twice with 100 mL of diethyl ether. The organic phases were then combined, washed with water and brine, dried over anhydrous sodium sulfate, and the solvent was removed by vacuum rotary evaporation. The mixture was then subjected to silica gel column chromatography (hexane / dichloromethane = 1:1 (v / v)). f After adding 0.50, a solid intermediate product (c) was obtained, with a yield of approximately 35.6%.

[0079] The NMR characterization results of intermediate product (c) are as follows: 1H NMR (500 MHz, 298 K, CDCl3, 7.26 ppm): δ = 7.97 (d, J = 7.6 Hz, 1H), 7.87 (d, J = 7.5 Hz, 1H), 7.54 (d, J = 7.6 Hz, 1H), 7.41 (d, J = 7.5 Hz, 1H), 3.51 (d, J = 6.9 Hz, 4H) ppm; 19 F NMR (500 MHz, 298 K, CDCl3): δ = -80.85, -98.78, -118.50, -125.50 ppm.

[0080] Step 2: Under an inert atmosphere (nitrogen), the intermediate product (c, 1 equivalent, 0.8 g, 1.9 mmol) was reacted with stannous chloride dihydrate (SnCl2·2H2O, 5 equivalent, 2.16 g, 9.6 mmol) and 30 mL of ethyl acetate in a round-bottom flask. The mixture was heated and stirred at 38 °C for 2 days. After the reaction was complete, the mixture was cooled to room temperature, and 30 mL of 1 M sodium hydroxide aqueous solution was added. After filtering to remove insoluble matter, the aqueous phase was extracted with ethyl acetate. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by vacuum rotary evaporation. The mixture was then subjected to silica gel column chromatography (hexane / dichloromethane = 2:1 (v / v)). f The product was purified by refining (=0.20) and the target product was a yellow solid (d), with a yield of approximately 79.5%.

[0081] The NMR characterization results of perfluoroaromatic amines (d) are as follows: 1 H NMR (500 MHz, 298 K, CDCl3, 7.26 ppm): δ = 7.74 (s, 1H), 7.28 (s, 1H), 7.20 (s, 1H), 6.92 (s, 1H), 4.27 (s, 2H,NH2), 3.38 (s, 2H), 3.34 (s, 2H) ppm (with Figure 1 ); 13 C NMR (125 MHz, 298 K, CDCl3, 77.16ppm): δ = 153.31, 141.67, 139.05, 137.14, 130.25, 121.35, 117.88, 117.52,77.16, 30.64, 29.28 ppm; 19 F NMR (500 MHz, 298 K, CDCl3): δ = -80.80, -95.19, -118.47, -125.68 ppm.

[0082] Example 2

[0083] The chemical reaction formula for the synthesis of the sandwich-type α-diimine ligand L-C4H9 is as follows:

[0084] .

[0085] The specific synthesis steps include:

[0086] 8-Butylnaphthyl-1-amine (a, 300 mg, 1.5 mmol), the dibenzo-p-benzoenedione skeleton (b, 153 mg, 0.65 mmol), p-toluenesulfonic acid (catalytic amount, approximately 5 mg), and toluene (5 mL) were added to a pressure-resistant flask, and the mixture was heated to reflux and stirred for 2 days. After the reaction was complete, the solvent was removed under reduced pressure. The residue was analyzed by column chromatography (hexane / dichloromethane = 2 / 1 (v / v), R... f Purification with 0.40 yielded a yellow oily ligand L-C4H9, with a yield of 75.5%.

[0087] The NMR characterization results of ligand L-C4H9 are as follows: 1 H NMR (500 MHz, 298 K, CDCl3, 7.26 ppm): δ= 7.73 (s, 4H), 7.52 (s, 2H), 7.40 (s, 2H), 7.31-7.27 (m, 2H), 7.22 (s, 8H), 6.65 (s, 2H), 5.56 (s, 2H), 1.09 (s, 4H), 0.87 (s, 6H), 0.42 (s, 6H) ppm (attached Figure 2 ); 13 C NMR (125 MHz, 298 K, CDCl3, 77.16 ppm): δ = 157.19 (N=C-Ar), 147.95,141.38, 139.68, 136.34, 128.32, 127.80, 126.72, 126.49, 126.11, 126.07,124.89, 115.10, 77.16, 50.30, 36.44, 35.69, 22.64, 13.76 ppm.

[0088] Example 3

[0089] Sandwich-type α-diimine ligand L tBu The chemical reaction formula for the synthesis of -C4H9 is as follows:

[0090] .

[0091] The specific synthesis steps include:

[0092] 8-Butylnaphthyl-1-amine (a, 300 mg, 1.5 mmol), a tert-butyl-substituted dibenzo[a]benzenedione skeleton (b, 237 mg, 0.65 mmol), p-toluenesulfonic acid (catalytic amount, approximately 5 mg), and toluene (5 mL) were added to a pressure-resistant flask, and the mixture was heated to reflux and stirred for 2 days. After the reaction was complete, the solvent was removed under reduced pressure. The residue was analyzed by column chromatography (hexane / dichloromethane = 9 / 1 (v / v), R... f After purification (=0.50), a yellow solid ligand L was obtained. tBu -C4H9, with a yield of 83.5%.

[0093] ligand L tBu The NMR characterization results of -C4H9 are as follows: 1 H NMR (500 MHz, 298 K, CDCl3, 7.26 ppm): δ = 7.74 (m, 6H), 7.50 (s, 4H), 7.40 (m, 4H), 7.22 (m, 4H), 6.63 (d, 2H), 5.46 (s, 2H), 1.25 (s, 24H), 0.87 (m, 4H, Me), 0.74 (s, 2H), 0.38 (m, 6H)ppm; 13 C NMR (125 MHz, 298 K, CDCl3, 77.16 ppm): δ = 157.86 (N=C-Ar), 151.01,148.22, 141.49, 139.56, 136.72, 136.31, 128.12, 126.68, 126.55, 126.11,125.86, 124.87, 124.65, 115.17, 77.16, 50.25, 36.45, 34.89, 31.51, 13.80 ppm.

[0094] Example 4

[0095] The chemical reaction formula for the synthesis of the sandwich-type α-diimine ligand L-C4F9 is as follows:

[0096] .

[0097] The specific synthesis steps include:

[0098] 6-(perfluorobutyl)-1,2-dihydroacenaphthene-5-amine (a, 300 mg, 0.8 mmol), dibenzo-terpenoid skeleton (b, 82.5 mg, 0.35 mmol), p-toluenesulfonic acid (catalytic amount, approximately 5 mg), and toluene (5 mL) were added to a pressure-resistant flask, heated to reflux, and stirred for 2 days. After the reaction was complete, the solvent was removed under reduced pressure. The residue was analyzed by column chromatography (hexane / dichloromethane = 1 / 1 (v / v), R... f Purification with 0.20 g of the compound yielded a yellow solid ligand L-C4F9 with a yield of 77.3%.

[0099] The NMR characterization results of ligand L-C4F9 are as follows: 1 H NMR (500 MHz, 298 K, CDCl3, 7.26 ppm): δ= 7.75 (d, J = 7.4 Hz, 2H), 7.42 (dd, J = 46.4, 7.3 Hz, 6H), 7.06 (d, J =31.7 Hz, 4H), 6.71 (d, J = 7.3 Hz, 2H), 5.52 (s, 2H), 3.51 (s, 8H) ppm; 13 C NMR (125 MHz, 298 K, CDCl3, 77.16 ppm): δ = 157.77 (N=C-Ar), 152.20, 143.65,142.64, 141.40, 130.92, 127.66, 127.16, 125.43, 124.19, 120.56, 119.92,118.63, 77.16, 50.92, 30.65, 29.85 ppm.

[0100] Example 5

[0101] Sandwich-type α-diimine ligand L tBu The chemical reaction formula for the synthesis of -C4F9 is as follows:

[0102] .

[0103] The specific synthesis steps include:

[0104] 6-(perfluorobutyl)-1,2-dihydroacenaphthene-5-amine (a, 300 mg, 0.8 mmol), a tert-butyl-substituted dibenzo[a]benzenedione skeleton (b, 127.8 mg, 0.35 mmol), p-toluenesulfonic acid (catalytic amount, approximately 5 mg), and toluene (5 mL) were added to a pressure-resistant flask, and the mixture was heated to reflux and stirred for 2 days. After the reaction was complete, the solvent was removed under reduced pressure. The residue was analyzed by column chromatography (hexane / dichloromethane = 2 / 1 (v / v), R...f After purification (=0.20), a yellow solid ligand L was obtained. tBu -C4F9, yield 77.3%.

[0105] ligand L tBu The NMR characterization results of -C4F9 are as follows: 1 H NMR (500 MHz, 298 K, CDCl3, 7.26 ppm): δ = 7.75 (d, J = 7.4 Hz, 2H), 7.42 (dd, J = 46.4, 7.3 Hz, 6H), 7.06 (d, J =31.7 Hz, 4H), 6.71 (d, J = 7.3 Hz, 2H), 5.52 (s, 2H), 3.51 (s, 8H) ppm; 13 C NMR (125 MHz, 298 K, CDCl3, 77.16 ppm): δ = 157.77 (N=C-Ar), 152.20, 143.65,142.64, 141.40, 130.92, 127.66, 127.16, 125.43, 124.19, 120.56, 119.92,118.63, 77.16, 50.92, 30.65, 29.85 ppm.

[0106] Example 6

[0107] The synthesis of the sandwich-type α-diimine nickel catalyst Ni-C4H9 includes the following specific steps:

[0108] L-C4H9 (0.35 mmol) and NiBr2(DME) (0.35 mmol) were dissolved in 30 mL of dichloromethane and stirred at 25 °C for 24 hours to obtain a deep red liquid. After evaporating the solvent under vacuum, an orange solid was obtained. The solid was washed three times with n-hexane, filtered, and finally washed three times with diethyl ether. The solid was then dried under vacuum to obtain the nickel catalyst Ni-C4H9 (97.4% yield).

[0109] The synthesized nickel catalyst Ni-C4H9 was analyzed by matrix-assisted laser desorption / ionization time-of-flight mass spectrometry (MALDI-TOF-MS), and the results were: MALDI-TOF-MS (m / z): 596.8 [M-Ni-2Br] + .

[0110] The single-crystal structure of the synthesized nickel catalyst Ni-C4H9 was analyzed, and the results are as follows: Figure 3 As shown.

[0111] Example 7

[0112] Sandwich-type α-diimine nickel catalyst Ni tBu The synthesis of -C4H9 involves the following steps:

[0113] L tBu -C4H9 (0.35 mmol) and NiBr2(DME) (0.35 mmol) were dissolved in 30 mL of dichloromethane and reacted with the solution at 25 °C for 24 hours to obtain a deep red liquid. After evaporating the solvent under vacuum, an orange solid was obtained. The solid was washed three times with n-hexane, filtered, and finally washed three times with diethyl ether. The solid was then dried under vacuum to obtain the nickel catalyst Ni. tBu -C4H9 (93.4% yield).

[0114] For the synthesized nickel catalyst Ni tBu Matrix-assisted laser desorption / ionization time-of-flight mass spectrometry (MALDI-TOF-MS) analysis of -C4H9 yielded the following results: MALDI-TOF-MS (m / z): 708.4 [M-Ni-2Br] + .

[0115] Example 8

[0116] The synthesis of the sandwich-type α-diimine nickel catalyst Ni-C4F9 includes the following specific steps:

[0117] L-C4F9 (0.35 mmol) and NiBr2 (DME) (0.35 mmol) were dissolved in 30 mL of dichloromethane and stirred at 25 °C for 24 hours to obtain a deep red liquid. After evaporating the solvent under vacuum, an orange solid was obtained. The solid was washed three times with n-hexane, filtered, and finally washed three times with diethyl ether. The solid was then dried under vacuum to obtain the nickel catalyst Ni-C4F9 (91.4% yield).

[0118] The synthesized nickel catalyst Ni-C4F9 was analyzed by matrix-assisted laser desorption / ionization time-of-flight mass spectrometry (MALDI-TOF-MS), and the results were: MALDI-TOF-MS (m / z): 972.7 [M-Ni-2Br] + .

[0119] Example 9

[0120] Sandwich-type α-diimine nickel catalyst Ni tBu The synthesis of -C4F9 involves the following steps:

[0121] L tBu-C4F9 (0.35 mmol) and NiBr2(DME) (0.35 mmol) were dissolved in 30 mL of dichloromethane and reacted with the solution at 25 °C for 24 hours to obtain a deep red liquid. After evaporating the solvent under vacuum, an orange solid was obtained. The solid was washed three times with n-hexane, filtered, and finally washed three times with diethyl ether. The solid was then dried under vacuum to obtain the nickel catalyst Ni. tBu -C4F9 (99.1% yield).

[0122] The synthesized nickel catalyst Ni-C4F9 was analyzed by matrix-assisted laser desorption / ionization time-of-flight mass spectrometry (MALDI-TOF-MS), and the results were: MALDI-TOF-MS (m / z): 1084.8 [M-Ni-2Br] + .

[0123] Example 10

[0124] The effects of different co-catalysts on the Ni-C4H9-catalyzed ethylene polymerization are shown in Table 1:

[0125] Table 1. Effects of different co-catalysts on Ni-C4H9-catalyzed ethylene polymerization

[0126]

[0127] Table 1. Reaction conditions: Nickel catalyst Ni-C4H9 (1 μmol), co-catalyst (500 μmol), toluene or hexane (80 mL), ethylene pressure (8 bar), polymerization time (30 minutes), polymerization temperature (50 °C). Activity: at 10 6 g mol -1 h -1 Unit: M w PDI: Weight-average molecular weight and polymer molecular weight distribution index, respectively, determined by GPC at 150°C in 1,2,4-trichlorobenzene, relative to polystyrene standards. Branching degree = number of branches per 1000 carbon atoms, determined by 1H NMR spectroscopy. DEAC is diethylaluminum chloride, EASC is sesquiethylaluminum chloride, MMAO is modified methylaluminoxane, TMA is trimethylaluminum, and TIBA is triisobutylaluminum.

[0128] Table 1. Polymerization process: First, a 350 mL glass pressure reactor connected to a high-pressure gas pipeline was vacuum dried at 90 °C for at least 1 hour. Then, the reactor was adjusted to 50 °C, and 78 mL of toluene and 500 μmol of co-catalyst were added to the reactor under an inert atmosphere. Then, 1 μmol of Ni catalyst was dissolved in 2 mL of dichloromethane (or chloroform) and injected into the polymerization system via a syringe. Ethylene was introduced under rapid stirring (above 600 rpm) and maintained at 8 bar. After 30 minutes, the pressure reactor was vented, and a large amount of acidic ethanol (a hydrochloric acid ethanol solution of above 5 wt%) was added. The polymer was filtered and dried to constant weight in a vacuum oven.

[0129] Table 1. Conclusions of Polymerization Data: In terms of polymerization activity, chlorine-containing co-catalysts such as diethylaluminum chloride (DEAC) and sesquiethylaluminum chloride (EASC) showed the highest activation efficiency, reaching 3.80 × 10⁻⁶. 6 and 3.62×10 6 g mol -1 h -1 In contrast, when the cocatalysts are modified methylaluminoxane (MMAO) without chlorine atoms, as well as trimethylaluminum (TMA) and triisobutylaluminum (TIBA), the ethylene activity of Ni-C4H9 is relatively low (Table 1, entries 3-5, 0.72 × 10⁻⁶). 6 ~1.30×10 6 g mol -1 h -1 It is worth mentioning that DEAC, EASC, and MMAO can all successfully activate Ni-C4H9 to prepare typical bimodal polyethylene, with an overall polymer PDI as high as 20.2~39.3 (Table 1, entries 1~3). Among them, the high molecular weight fraction, peak 1, has a weight average molecular weight of 50×10⁻⁶. 4 g mol -1 Around 10, while the weight-average molecular weight of the low molecular weight fraction is <10. 4 g mol -1 Under TMA and TIBA activation, Ni-C4H9 can only catalyze the formation of narrowly distributed (PDI=1.8) polymers from ethylene, with a polymer molecular weight (M... w =51.8×10 4 and 44.3×10 4 g mol -1 This is similar to the high molecular weight portion of the aforementioned bimodal polyethylene. Furthermore, the polymers obtained from highly polymerizable catalytic systems (Table 1, entries 1-2, DEAC and EASC) have a higher content of low molecular weight components, reaching 69-74%, while exhibiting moderate polymer branching [Brs(DEAC) = 57 / 1000C, Brs(EASC) = 63 / 1000C] and a lower melting point. m=91~94℃. In contrast, the polymers obtained from the low polymerization activity catalytic systems (Table 1, entries 3~5, MMAO, TMA, and TIBA) had lower low molecular weight components (14% and 0%), and lower polymer branching [Brs(MMAO)=36 / 1000C, Brs(TMA)=20 / 1000C, Brs(TIBA)=36 / 1000C], and higher melting points. m =109~115℃.

[0130] Example 11

[0131] Different nickel catalysts (with different substituents R) 1 R 2 The results of the study on ethylene polymerization at different temperatures are shown in Table 2:

[0132] Table 2. Results of ethylene polymerization using different nickel catalysts at different temperatures

[0133]

[0134] Table 2 Reaction conditions: Nickel catalyst (1 μmol), DEAC co-catalyst (500 μmol), toluene or hexane (80 mL), ethylene pressure (8 bar), polymerization time (30 minutes). Activity: at 10 6 g mol -1 h -1 Unit: M w PDI: Weight-average molecular weight and polymer molecular weight distribution index, respectively, determined by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Branching degree = number of branches per 1000 carbon atoms, determined by 1H NMR spectroscopy.

[0135] Table 2. Polymerization process: First, a 350 mL glass pressure reactor connected to a high-pressure gas pipeline was vacuum dried at 90 °C for at least 1 hour. Then, the reactor was adjusted to 50 °C, and 78 mL of toluene and 500 μmol of co-catalyst were added to the reactor under an inert atmosphere. Then, 1 μmol of Ni catalyst was dissolved in 2 mL of dichloromethane (or chloroform) and injected into the polymerization system via a syringe. Ethylene was introduced under rapid stirring (above 600 rpm) and maintained at 8 bar. After 30 minutes, the pressure reactor was emptied, and a large amount of acidic ethanol (a hydrochloric acid ethanol solution of above 5 wt%) was added. The polymer was filtered and dried to constant weight in a vacuum oven.

[0136] Table 2: Conclusions from aggregated data:

[0137] (1) As the temperature increased from 50℃ to 90℃, the four catalysts exhibited the same regularity: decreased polymerization activity, decreased polymer molecular weight, and increased polymer branching degree. Increased temperature reduced the solubility of ethylene monomers and led to catalyst deactivation, thus decreasing apparent polymerization activity. Furthermore, increased temperature exacerbated the tendency for β-H elimination, leading to intensified chain transfer and chain walking reactions, resulting in decreased polymer molecular weight and increased branching degree. The increased branching structure in the polymer hindered crystallization, thus lowering the melting point of the polymer product.

[0138] (2) All four catalysts designed in the examples can withstand a high temperature of 90°C. Compared to Ni with greater steric hindrance... tBu -C4H9 and Ni-C4F9 containing fluorine effects, as well as Ni tBu Ni-C4F9 and Ni-C4H9 exhibit higher activity across the entire temperature range of 50–90 °C. In terms of molecular weight, Ni-C4F9 and Ni containing fluorine effects show higher activity. tBu -C4F9 was significantly higher than the other two catalysts, reaching a maximum of 96.5 gmol. -1 Meanwhile, its polymer branching degree is also the lowest among these four catalysts. The presence of the fluorine effect inhibits chain transfer and chain walking, thereby increasing the polymer molecular weight and reducing the branching degree. Simultaneously, the sterically hindered structure also inhibits chain transfer and chain walking; therefore, Ni... tBu -C4H9 exhibits a similar phenomenon to Ni-C4H9, namely, a slightly higher molecular weight and a slightly lower degree of branching.

[0139] (3) Polymer polydispersity index (PDI) is one of the key parameters of polyolefin materials. Overall, within the temperature range of 30–90 °C, the polymers prepared by these four catalysts exhibited a wide molecular weight distribution (PDI = 6.7–62.0), which varied with temperature. Among them, Ni-C4H9 and Ni… tBu The polymer prepared from -C4H9 is a typical bimodal polyethylene, with a large interval between its high molecular weight and low molecular weight fractions. In contrast, Ni-C4F9 and Ni... tBu Although -C4F9 has a wide distribution, it has fewer low-molecular-weight fractions, resulting in a relatively high overall molecular weight. This is likely due to the fluorine effect inhibiting chain transfer. As the temperature increases, chain transfer intensifies, and the molecular weights of both peaks in the bimodal polymers prepared by the three catalysts decrease.

[0140] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A sandwich-type α-diimine ligand, characterized in that, It has the structure of formula (I): Equation (I); In equation (I), R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

2. The sandwich-type α-diimine ligand according to claim 1, characterized in that, The sandwich-type α-diimine ligand is any one of formulas (I-1) to (I-4): Equation (I-1); Equation (I-2); Equation (I-3); Equation (I-4).

3. A method for preparing the sandwich-type α-diimine ligand according to claim 1 or 2, characterized in that, Includes the following steps: Compound of formula (II) and catalyst are mixed in an organic solvent and heated to react, yielding sandwich-type α-diimine ligand of formula (I); Equation (I); Formula (II); Formula (III); Among them, R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

4. The preparation method according to claim 3, characterized in that, The molar ratio of the compound with structure (II) to the compound with structure (III) is (2~2.5):

1.

5. The preparation method according to claim 3, characterized in that, The catalyst is p-toluenesulfonic acid.

6. A nickel catalyst, characterized in that, It has the structure of formula (IV): Formula (IV); In equation (IV), R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

7. The nickel catalyst according to claim 6, characterized in that, The nickel catalyst is any one of formulas (IV-1) to (IV-4): Formula (IV-1); Formula (IV-2); Formula (IV-3); Formula (IV-4).

8. A method for preparing the nickel catalyst according to claim 6 or 7, characterized in that, Includes the following steps: The ligand of formula (I) and nickel bromide of ethylene glycol dimethyl ether were mixed and reacted in an organic solvent to obtain the nickel catalyst of formula (IV); Formula (I); Formula (IV); Among them, R 1 It is perfluoro-n-butyl or n-butyl, R 2 It is hydrogen or tert-butyl.

9. The preparation method according to claim 8, characterized in that, The molar ratio of the ligand of the formula (I) structure to nickel dimethyl ether ethylene glycol bromide is 1:(1~5).

10. A method for ethylene polymerization, characterized in that, Includes the following steps: Ethylene undergoes catalytic polymerization in the presence of a catalyst to obtain polyethylene; The catalyst includes the nickel catalyst according to any one of claims 6 to 7 or the nickel catalyst prepared by the preparation method according to any one of claims 8 to 9.