Machining method of small-specification zirconium alloy bar
By combining hot rolling and cold rolling, the problems of large size, uneven microstructure and unstable performance of zirconium alloy bars in the existing technology have been solved, realizing the efficient preparation of small size and high precision zirconium alloy bars and reducing production costs.
Patent Information
- Application Number
- CN202610230519.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-26
- Publication Date
- 2026-04-21
AI Technical Summary
Existing zirconium alloy bar processing technology suffers from problems such as large size, uneven microstructure, unstable performance, low production efficiency and high cost, making it difficult to produce small-sized, high-precision zirconium alloy bars.
A combined hot rolling and cold rolling processing method is adopted, including steps such as vacuum melting, forging, quenching, hot rolling, cold rolling and vacuum annealing, to obtain small-sized zirconium alloy bars through large deformation and precise control.
This significantly shortened the processing flow, improved production efficiency, reduced costs, and yielded smaller-sized zirconium alloy bars with superior microstructure and performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of zirconium alloy material processing technology, and in particular to a method for processing small-diameter zirconium alloy bars. Background Technology
[0002] Zirconium alloys are widely used in nuclear reactor fuel elements due to their small thermal neutron absorption cross-section, high thermal conductivity, good mechanical properties, excellent machinability, and UO2 compatibility. They also exhibit good corrosion resistance and sufficient thermal strength, particularly under high-temperature, high-pressure steam operating environments. Zirconium alloy rods are primarily used as end plugs for nuclear reactor fuel assemblies. The end plugs are typically welded to the cladding tubes to ensure a tight seal and prevent the release of radioactive materials into the main circuit during normal operation. The reliability of the assembly within the reactor depends heavily on the quality of the connection between the end plug and the cladding tubes, directly impacting the safety, reliability, and economics of the nuclear power plant. Therefore, developing a high-quality zirconium alloy rod manufacturing process that meets the requirements for high burnup is crucial.
[0003] Prior art document 1 (a method for preparing zirconium alloy rods, patent number CN201910372723.7) uses extrusion to obtain zirconium alloy rods. However, due to limitations in extrusion equipment capacity and process characteristics, the finished rods are often large-sized. Prior art document 2 (a method for preparing zirconium alloy rods for nuclear fuel assembly end plugs, patent number CN202310759369.X) uses extrusion + cold rolling to obtain zirconium alloy rods. Due to problems such as poor uniformity of microstructure in rods prepared by extrusion, the performance of the finished rods needs further improvement, and the extrusion cost is often high. Comparative document three (a method for preparing Zr-Nb alloy bars, patent number CN202010235645.9) uses hot rolling / precision forging to obtain zirconium alloy bars. Due to the capabilities and process characteristics of hot rolling / precision forging equipment, similar to extrusion forming, the prepared bars are often large-sized bars, and the precision of hot rolling / precision forging is poor. Even if subsequent processing can correct deviations, the low material utilization rate leads to high production costs. Comparative document four (performance study of N36 zirconium alloy bars, hot working technology, Vol. 42, No. 2, 2013) uses extrusion + hot rolling + cold rotary forging and extrusion + hot rotary forging + cold rotary forging to obtain zirconium alloy bars, and compares the performance differences between the two, concluding that hot rolling is superior to hot rotary forging. The final deformation process in this document is cold rotary forging. Due to the characteristics of cold rotary forging, the deformation amount per pass is generally no more than 30%, and preferably between 9% and 25%. This small deformation amount leads to low production efficiency.
[0004] In summary, existing processing techniques for zirconium alloy rods either have certain problems or are only suitable for a narrow range of applications. To prepare small-sized zirconium alloy rods with excellent comprehensive performance, this patent adopts a combined hot rolling and cold rolling method, which combines the advantages of both hot and cold working and is more suitable for the preparation of small-sized, high-precision zirconium alloy rods. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to provide a processing method for small-sized zirconium alloy bars. The method adopts hot rolling + cold rolling processing technology, which obtains zirconium alloy bars with better microstructure and properties, significantly shortens the processing flow, improves production efficiency, reduces production costs, and can obtain small-sized zirconium alloy bars with a diameter of less than 10mm. To achieve the aforementioned objective, the technical solution of the present invention is implemented as follows: a method for processing small-diameter zirconium alloy bars, comprising the following steps: 1) The sponge zirconium and alloying elements that make up the zirconium alloy are proportioned according to the required composition, and the zirconium alloy ingot is obtained after multiple vacuum melting processes. 2) After heating and holding the zirconium alloy ingot obtained in step 1), it is forged and cut in sequence to obtain zirconium alloy forged rods. 3) After heating and holding the zirconium alloy forging rod obtained in step 2), it is quenched to obtain a quenched rod blank. 4) The quenched bar billet obtained in step 3) is hot rolled and slit to obtain a hot-rolled bar billet; 5) The hot-rolled billet obtained in step 4) is subjected to cold finishing rolling and slitting to obtain cold-rolled bars; 6) After degreasing / debinding the cold-rolled bar obtained in step 5), vacuum annealing is performed to obtain annealed bar. 7) The annealed bar obtained in step 6) is subjected to straightening, centerless grinding and degreasing treatment in sequence to obtain the finished bar.
[0006] Preferably, in step 1), the zirconium alloy ingot is prepared according to the alloy grade, pressed into electrodes, and then subjected to multiple vacuum melting processes.
[0007] Preferably, in step 2), the heating furnace is a box-type resistance furnace, the heating temperature of the zirconium alloy ingot is 900℃-1050℃, the holding time is 60min-300min, the forging temperature is not lower than 500℃, and an anti-oxidation coating is applied before forging.
[0008] To control the temperature drop during forging, the final forging temperature should be controlled to be no less than 500℃. If the forging dimensions cannot be achieved in one forging pass, a second forging pass can be performed. The temperature of the second forging pass can be slightly lower than that of the first forging pass.
[0009] Preferably, in step 3), the quenching treatment adopts induction or resistance quenching, the preheating temperature is 1000℃-1150℃, the quenching holding time is >3min, and the ratio of water volume in the quenching water tank to the volume of the billet is greater than 40, and the quenching transfer time does not exceed 30s.
[0010] Preferably, in step 4), the hot rolling temperature is 600℃-750℃, the holding time is 60-180min, and the total deformation of the quenched billet in the first hot rolling is insufficient, so a second hot rolling is performed until the total deformation of the quenched billet in the hot rolling is greater than 90%.
[0011] Since the amount of deformation during hot rolling is directly related to the microstructure and properties of the bar, increasing the amount of deformation promotes dynamic recrystallization, causing coarse grains to break down into fine grains, thereby obtaining excellent microstructure and properties. Therefore, the total deformation during hot rolling should be greater than 90%. The bar is then slit after hot rolling.
[0012] Preferably, in step 4), in order to better control the surface quality and defects of the finished bar, the slit bar is subjected to a centerless turning process to remove the oxide scale on the surface of the bar and obtain a bright hot-rolled bar.
[0013] Preferably, in step 5), the cold finishing feed amount is greater than 0.5 mm / time, the rolling speed is greater than 50 times / min, the number of cold rolling cycles of the cold-rolled bar is greater than or equal to 1, and the total cold rolling deformation of the cold-rolled bar is greater than 50%.
[0014] Cold forging is a common method for cold deformation of zirconium alloy bars. Due to its short deformation stroke and relatively small deformation force, the deformation per pass in cold forging is typically around 9%-25%. Multiple passes are required to achieve the required total deformation. In contrast, cold rolling, with its longer rolling stroke, generally allows for large deformation in a single pass. Furthermore, the longer deformation zone in the die design ensures that the bar surface quality meets requirements even with high feed rates. Cold forging, on the other hand, typically has a feed rate of 0.5-1.0 m / min, which is limited by the die itself. Higher feed rates can lead to uneven forging of the bar, resulting in substandard dimensions and surface quality. Moreover, cold rolling allows for stable rolling at high feed rates and speeds, significantly exceeding those of cold forging. Therefore, using a Pilger cold rolling mill for cold rolling hot-rolled bars simplifies the number of cold deformation passes and significantly improves production efficiency.
[0015] Preferably, in step 6), the holding temperature of the vacuum annealing is 540℃-700℃, and the holding time is 1h-4h.
[0016] Preferably, in step 7), the annealed bar is straightened on a straightening machine, and the straightness of the bar after straightening is ≤0.5mm / m.
[0017] Preferably, the centerless grinding process is used to remove oxide scale and defects from the surface of the rod; the degreasing process (which is essentially removing the grinding fluid from the surface of the zirconium rod, also known as degreasing) has a degreasing temperature of 65-70℃ and a degreasing time of 45-60min.
[0018] The beneficial effects of this invention are reflected in: (1) The method provided by the present invention replaces hot rolling and extrusion with hot rolling + cold rolling technology, breaks through the capabilities and process characteristics of hot rolling and extrusion equipment, and can obtain small-sized zirconium alloy rods with a diameter of less than 10mm.
[0019] (2) The method provided by the present invention obtains small-sized zirconium alloy bars with better microstructure and performance by using large deformation hot rolling and cold rolling technology, which shortens the bar processing process, improves production efficiency and reduces production costs. Detailed Implementation
[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Unless otherwise specified, the embodiments and features in the embodiments of this application can be combined with each other. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] Example 1 This embodiment includes the following steps: Step 1: According to the required composition ratio of Zr-4 alloy elements, Sn mass fraction is 1.2-1.7%, Fe mass fraction is 0.18-0.24%, Cr mass fraction is 0.07-0.13%, O mass fraction is 0.10-0.15%, and the balance is Zr. Then, three vacuum melting processes are carried out to obtain a Φ650mm zirconium alloy ingot.
[0022] Step Two: After heating and holding the ingot obtained in Step One, forge it at a heating temperature of 1015℃ (target value) for 240 minutes, free forging it into a 300mm square billet. The forging end temperature should be ≥650℃. Apply an anti-oxidation coating before forging. After forging, inspect and grind the surface of the billet to remove visible cracks and folds. After grinding, slit the billet into three equal parts. Perform a second forging at a heating temperature of 820℃ (set value) for 150 minutes, free forging it into a Φ160mm round billet. The forging end temperature should be ≥500℃. Apply an anti-oxidation coating before forging. After forging, slit the billet into sections of 800-1200mm in length.
[0023] Step 3: The forged rod obtained in Step 2 is quenched using resistance quenching. The preheating temperature is 1050℃ (set value), the quenching holding time is 60 minutes, the water volume ratio of the quenching water tank to the billet volume is greater than 40, and the quenching transfer time does not exceed 30 seconds. After quenching, the rod is machined to remove the quenching layer on the surface, resulting in a bright zirconium rod.
[0024] Step 4: The zirconium rods obtained in Step 3 are hot-rolled using a resistance heating furnace. The first hot rolling temperature is 700℃ (set value), and the holding time is 90 minutes, producing a Φ60mm billet. After hot rolling, surface defects are inspected and ground, and then the billets are slit into 800mm-1200mm billets. A second hot rolling process is then performed at 680℃ (set value), with a holding time of 60 minutes, producing a Φ15mm billet. After hot rolling, the billets are slit into 3m-5m bars, and then centerlessly machined to a Φ14.5mm bright zirconium rod. The total deformation during hot rolling is approximately 99%.
[0025] Step 5: Cold roll the zirconium rod obtained in Step 4. The cold rolling speed is 250 cycles / min, the cold rolling feed is 2.5 mm / cycle, and the cold rolled size is Φ9±0.03 mm. The total cold rolling deformation is 60%. After cold rolling, cut into 3m-5m long bars.
[0026] Step 6: Perform vacuum annealing on the zirconium rod obtained in Step 5. The annealing temperature is 565℃ (set value), the holding time is 2h, and the vacuum degree during the annealing process is better than 10-2Pa.
[0027] Step 7: The annealed bars from Step 6 are straightened using a six-roll straightener. The straightness after straightening is better than 0.5 mm / m. The straightened bars are then subjected to centerless grinding, which removes 0.5 mm, resulting in finished bars with a diameter of 9.5 mm. Finally, the bars are degreased using SD-10 degreasing agent at a temperature of 65℃ (set value) for 60 minutes. After degreasing, the bars are dried to obtain small-diameter zirconium alloy bars.
[0028] Samples of the zirconium alloy rods obtained in Example 1 were taken and their microstructure and properties were tested, as shown in Table 1: Table 1. Microstructure and properties of zirconium alloy bars
[0029] Example 2 This embodiment includes the following steps: Step 1: According to the required composition ratio of Zr-4 alloy elements, Sn mass fraction is 1.2-1.7%, Fe mass fraction is 0.18-0.24%, Cr mass fraction is 0.07-0.13%, O mass fraction is 0.10-0.15%, and the balance is Zr. Then, three vacuum melting processes are carried out to obtain a Φ650mm zirconium alloy ingot.
[0030] Step Two: After heating and holding the ingot obtained in Step One, forge it at a heating temperature of 1015℃ (target value) for 240 minutes, free forging it into a 280mm square billet. The forging end temperature should be ≥650℃. Apply an anti-oxidation coating before forging. After forging, inspect and grind the surface of the billet to remove visible cracks and folds. After grinding, slit the billet into three equal parts. Perform a second forging at a heating temperature of 820℃ (set value) for 150 minutes, radially forging it into a Φ140mm round billet. The forging end temperature should be ≥500℃. Apply an anti-oxidation coating before forging. After forging, slit the billet into sections of 800-1200mm in length.
[0031] Step 3: The forged rod obtained in Step 2 is quenched using resistance quenching. The preheating temperature is 1050℃ (set value), the quenching holding time is 60 minutes, the water volume ratio of the quenching water tank to the billet volume is greater than 40, and the quenching transfer time does not exceed 30 seconds. After quenching, the rod is machined to remove the quenching layer on the surface, resulting in a bright zirconium rod.
[0032] Step 4: The zirconium rods obtained in Step 3 are hot-rolled using a resistance heating furnace. The first hot rolling temperature is 680℃ (set value), and the holding time is 90 minutes. The first hot rolling produces a Φ50mm billet. After hot rolling, surface defects are inspected and ground, and then the billet is slit into 800-1200mm billets. After slitting, a second hot rolling process is performed at 650℃ (set value), and the holding time is 60 minutes. The second hot rolling produces a Φ10mm billet, which is then slit into 3m-5m bars. Finally, a centerless machine is used to obtain a Φ9.5mm bright zirconium rod. The total deformation during hot rolling is approximately 99%.
[0033] Step 5: Cold roll the zirconium rod obtained in Step 4. The cold rolling speed is 200 times / min, the cold rolling feed is 2mm / time, and the cold rolled size is Φ6±0.03mm. The total cold rolling deformation is 60%. After cold rolling, cut into 3m-5m long bars.
[0034] Step 6: Perform vacuum annealing on the zirconium rod obtained in Step 5. The annealing temperature is 600℃ (set value), the holding time is 1.5h, and the vacuum degree during the annealing process is better than 10-2Pa.
[0035] Step 7: The annealed bars from Step 6 are straightened using a six-roll straightener. The straightness after straightening is better than 0.5 mm / m. The straightened bars are then subjected to centerless grinding, which removes 0.5 mm, resulting in finished bars with a diameter of 5.5 mm. Finally, the bars are degreased using SD-10 degreasing agent at a temperature of 70℃ (set value) for 45 minutes. After degreasing, the bars are dried to obtain small-diameter zirconium alloy bars.
[0036] Samples of the zirconium alloy rods obtained in Example 2 were taken and their microstructure and properties were tested, as shown in Table 2: Table 2. Microstructure and properties of zirconium alloy bars
[0037] As can be seen from the above, the present invention solves the problems of uneven microstructure and unstable performance of zirconium rods by adopting a short process combining large deformation hot rolling and cold rolling, and obtains zirconium alloy rods with small specifications and high precision with a diameter of less than 10mm. Moreover, the microstructure and performance of the zirconium alloy rods are superior to those of zirconium alloy rods manufactured by existing technologies.
[0038] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for processing small-diameter zirconium alloy bars, characterized in that, Includes the following steps: 1) The sponge zirconium and alloying elements that make up the zirconium alloy are proportioned according to the required composition, and the zirconium alloy ingot is obtained after multiple vacuum melting processes. 2) After heating and holding the zirconium alloy ingot obtained in step 1), it is forged and cut in sequence to obtain zirconium alloy forged rods. 3) After heating and holding the zirconium alloy forging rod obtained in step 2), it is quenched to obtain a quenched rod blank. 4) The quenched bar billet obtained in step 3) is hot rolled and slit to obtain a hot-rolled bar billet; 5) The hot-rolled billet obtained in step 4) is subjected to cold finishing rolling and slitting to obtain cold-rolled bars; 6) After degreasing / debinding the cold-rolled bar obtained in step 5), vacuum annealing is performed to obtain annealed bar. 7) The annealed bar obtained in step 6) is subjected to straightening, centerless grinding and degreasing treatment in sequence to obtain the finished bar.
2. The processing method for small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 1), the zirconium alloy ingot is prepared according to the alloy grade, pressed into electrodes, and then subjected to multiple vacuum melting processes to obtain the ingot.
3. The processing method for small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 2), the heating temperature of the zirconium alloy ingot is 900℃-1050℃, the holding time is 60min-300min, the forging temperature is not lower than 500℃, and an anti-oxidation coating is applied before forging.
4. The processing method for small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 3), the quenching process adopts induction or resistance quenching, the preheating temperature is 1000℃-1150℃, the quenching holding time is >3min, the water volume of the quenching water tank is greater than 40 to the volume of the billet, and the quenching transfer time does not exceed 30s.
5. The processing method for small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 4), the hot rolling temperature is 600℃-750℃, the holding time is 60-180min, and the total deformation of the quenched billet in the first hot rolling is insufficient, so a second hot rolling is performed until the total deformation of the quenched billet in the hot rolling is greater than 90%.
6. The processing method for small-diameter zirconium alloy bars according to claim 5, characterized in that, In step 4), the slit billets are subjected to a centerless milling process to remove the oxide scale from the surface of the billets and obtain bright hot-rolled billets.
7. The processing method for small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 5), the cold rolling feed amount is greater than 0.5 mm / time, the rolling speed is greater than 50 times / min, the number of cold rolling cycles of the cold-rolled bar is greater than or equal to 1, and the total cold rolling deformation of the cold-rolled bar is greater than 50%.
8. The processing method for small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 6), the holding temperature of the vacuum annealing is 540℃-700℃, and the holding time is 1h-4h.
9. The processing method for small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 7), the annealed bar is straightened on a straightening machine, and the straightness of the bar after straightening is ≤0.5mm / m.
10. A method for processing small-diameter zirconium alloy bars according to claim 1, characterized in that, In step 7), the centerless grinding process is used to remove oxide scale and defects from the surface of the bar; the degreasing process is carried out at a temperature of 65-70℃ for 45-60 minutes.
Citation Information
Patent Citations
A method for preparing zirconium alloy rods
CN111889535B
Preparation method of Zr-Nb-series alloy bar
CN113462998A
Method for producing a zirconium alloy rod for a nuclear fuel assembly end plug
CN116765164B