Copolymerized flame-retardant polycarbonate and preparation method thereof

By embedding flame-retardant monomers with phenylacetylene and benzoimide structures into polycarbonate, and combining isosorbide and aliphatic diols, a cross-linking network is formed through copolymerization, which solves the problem of insufficient flame retardant performance of polycarbonate and achieves UL94 V-0 flame retardant performance and excellent comprehensive performance.

CN122071577APending Publication Date: 2026-05-22CHINA NAT PETROLEUM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411676983.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-21
Publication Date
2026-05-22

AI Technical Summary

Technical Problem

Existing technologies struggle to improve the flame retardant properties of polycarbonate without compromising its thermal and mechanical properties, especially for applications in the electronics and electrical appliance industries that require a UL94 V-0 flame retardant rating. Furthermore, blending traditional flame retardants may lead to a decline in performance.

Method used

By copolymerization, flame-retardant monomers with phenylacetylene and benzoimide structures are embedded into the polycarbonate molecular chain, combined with isosorbide and aliphatic diols, and transesterification and polycondensation reactions are carried out to form a cross-linked network structure to improve flame retardant performance. The thermal and mechanical properties are also improved through the synergistic effect of phenylacetylene and benzoimide.

Benefits of technology

It achieves an improvement in the flame retardant performance of polycarbonate to UL94 V-0 level, while maintaining or improving thermal properties, mechanical properties and light transmittance, and possesses good weather resistance and safety and environmental protection performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122071577A_ABST
    Figure CN122071577A_ABST
Patent Text Reader

Abstract

The invention discloses copolymerized flame-retardant polycarbonate and a preparation method thereof. The preparation method comprises the following steps; diester carbonate, isosorbide, aliphatic diol, a first flame-retardant monomer and a second flame-retardant monomer are subjected to a reaction in the presence of a catalyst, and the copolymerized flame-retardant polycarbonate is obtained, wherein the first flame-retardant monomer comprises one or more than two of compounds with a structure as shown in a formula I: in the formula I, R1 and R2 are respectively and independently selected from one of carboxyl, alkyl ester group and hydroxyalkyl ester group; the second flame-retardant monomer comprises one or more than two of compounds with a structure as shown in a formula II; in the formula II, R3 and R4 are independently selected from one of carboxyl and alkyl ester. The polycarbonate provided by the invention has better thermal properties and mechanical properties while the flame retardant property is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of flame-retardant polymer technology, specifically to a copolymer flame-retardant polycarbonate and its preparation method. Background Technology

[0002] Polycarbonate (PC) is a widely used engineering plastic with excellent processing and mechanical properties. It also possesses self-extinguishing char properties and its flame retardant performance can reach UL94 V-2. However, for applications in electronics and electrical appliances, PC requires even higher flame retardancy, with a flame retardant rating of UL94 V-0.

[0003] The raw materials for polycarbonate production are mostly derived from petroleum derivatives, with bisphenol A (BPA) being one of the most commonly used. However, BPA has estrogenic effects and chronic toxicity, which may harm human health, greatly limiting the application areas of BPA-type polycarbonate. Isosorbide, on the other hand, is a chemically and thermally stable bicyclic diol. It is a renewable monomer derived from biomass and has a similar rigid structure to BPA, making it considered the most promising monomer to replace BPA in the synthesis of PC.

[0004] Isosorbide-based polycarbonate differs significantly in structure from traditional bisphenol A polycarbonate. It exhibits high transparency and brightness in optical properties, and high surface hardness, rigidity, toughness, and scratch resistance in physical and mechanical properties. However, compared to bisphenol A polycarbonate, isosorbide-based polycarbonate shows decreased temperature resistance, impact strength, and flame retardancy.

[0005] Therefore, to expand the application of PC in electronics and electrical appliances, it is necessary to further improve its flame retardant properties. The traditional method to improve the flame retardant properties of PC is to add flame retardants. However, since most flame retardants have some degree of incompatibility with the PC matrix, phenomena such as overflow and thermal decomposition may occur, thus affecting the original performance of PC. Besides blending, embedding flame-retardant monomers into the PC molecular chain through copolymerization can also improve the flame retardant properties of PC and avoid the negative impact of blending on PC performance.

[0006] CN114539754A discloses a weather-resistant, halogen-free, flame-retardant bio-based polycarbonate material and its preparation method. This method involves blending isosorbide-based polycarbonate with polyphosphate flame retardants and polyphenylsiloxane flame retardants to obtain the weather-resistant, halogen-free, flame-retardant bio-based polycarbonate material. However, this method modifies the bio-based polycarbonate by blending flame retardants, which significantly affects the polycarbonate's properties.

[0007] The paper "Copolymerization of Bisphenol S and Bisphenol A with Diphenyl Carbonate to Synthesize Flame-Retardant Polycarbonate" employs a melt transesterification method, using BPS, BPA, and diphenyl carbonate (DPC) as monomers to copolymerize and embed flame-retardant sulfur-containing groups into the PC molecular chain, thereby synthesizing flame-retardant copolymer PC to improve the flame-retardant properties of PC. However, the bisphenol A used in this method is biotoxic, and bisphenol S is a major alternative to the estrogen-like disruptor bisphenol A, which can also have negative effects on the body.

[0008] Therefore, developing novel copolymer flame-retardant polycarbonates and their preparation methods without affecting the thermal and mechanical properties of PC is one of the urgent problems to be solved in this field. Summary of the Invention

[0009] To address the aforementioned technical problems, the present invention aims to provide a copolymer flame-retardant polycarbonate and its preparation method. The polycarbonate of the present invention exhibits improved flame-retardant properties while also possessing superior thermal and mechanical properties.

[0010] To achieve the above objectives, the first aspect of the present invention provides a method for preparing a copolymer flame-retardant polycarbonate, comprising the following steps: reacting a carbonate diester, isosorbide, aliphatic diol, a first flame-retardant monomer, and a second flame-retardant monomer in the presence of a catalyst to obtain the copolymer flame-retardant polycarbonate.

[0011] Wherein, the first flame-retardant monomer comprises one or more compounds having the structure shown in Formula I:

[0012]

[0013] In Formula I, R1 and R2 are each independently selected from one of carboxyl, alkyl ester, and hydroxyalkyl ester groups;

[0014] The second flame-retardant monomer comprises one or more compounds having the structure shown in Formula II:

[0015]

[0016] In Formula II, R3 and R4 are each independently selected from carboxyl and alkyl ester groups.

[0017] According to a specific embodiment of the present invention, preferably, in Formula I, R1 and R2 are each independently selected from one of carboxyl, methyl ester and hydroxyethyl ester groups.

[0018] According to a specific embodiment of the present invention, preferably, the first flame-retardant monomer includes one or more of 4-phenylethynyl phthalic acid, dimethyl 4-phenylethynyl phthalate, and di(ethylene glycol) 4-phenylethynyl phthalate.

[0019] According to a specific embodiment of the present invention, preferably, in Formula II, R3 and R4 are each independently selected from one of carboxyl and methyl ester groups.

[0020] According to a specific embodiment of the present invention, preferably, the second flame-retardant monomer includes one or two of 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalic acid and dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate.

[0021] According to a specific embodiment of the present invention, preferably, the carbonate diester includes one or more of dimethyl carbonate, diphenyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, dipentyl carbonate, and dioctyl carbonate.

[0022] According to a specific embodiment of the present invention, preferably, the aliphatic diol includes one or more of 1,4-cyclohexanediol, 1,4-butanediol, 1,5-pentanediol and 1,6-hexanediol.

[0023] According to a specific embodiment of the present invention, preferably, the molar ratio of the total amount of isosorbide, aliphatic diol, first flame retardant monomer and second flame retardant monomer to the diester is (0.7-1):1.

[0024] According to a specific embodiment of the present invention, preferably, the molar ratio of isosorbide, the aliphatic diol, the first flame retardant monomer and the second flame retardant monomer is (0.5-0.7):(0.1-0.2):(0.05-0.15):(0.05-0.15).

[0025] According to a specific embodiment of the present invention, preferably, the catalyst includes one or more of the following: sodium tert-butoxide, lithium acetylacetonate, tetramethylammonium hydroxide, sodium tetraborate, lithium hydroxide monohydrate, lithium chloride, potassium dihydrogen phosphate, cesium carbonate, tetraisopropyl titanate, sodium methoxide, and sodium borohydride; the amount of the catalyst is 0.01% to 0.1% of the molar amount of the diester.

[0026] According to a specific embodiment of the present invention, preferably, the reaction includes an ester exchange reaction and a polycondensation reaction; the conditions for the ester exchange reaction include: a reaction temperature of 100℃~200℃, a pressure of 10kPa~50kPa, and a time of 0.5h~3h; the conditions for the polycondensation reaction include: a reaction temperature of 200℃~260℃, a pressure of 0kPa~1kPa, and a time of 0.5h~3h.

[0027] A second aspect of the present invention provides a copolymer flame-retardant polycarbonate, which is prepared by the above-described method for preparing copolymer flame-retardant polycarbonate.

[0028] According to a specific embodiment of the present invention, preferably, the number average molecular weight of the copolymer flame-retardant polycarbonate is 10,000 to 50,000 g / mol.

[0029] According to a specific embodiment of the present invention, preferably, the glass transition temperature of the copolymer flame-retardant polycarbonate is 110-140°C.

[0030] According to a specific embodiment of the present invention, preferably, the copolymer flame-retardant polycarbonate has an elongation at break of 70-120%, a tensile strength of 60-90 MPa, and a notched impact strength of 7-10 kJ / m. 2 .

[0031] According to a specific embodiment of the present invention, preferably, the limiting oxygen index of the copolymer flame-retardant polycarbonate is 35-40%, and the flame retardant rating of the copolymer flame-retardant polycarbonate is UL94 V-0.

[0032] According to a specific embodiment of the present invention, preferably, the light transmittance of the copolymer flame-retardant polycarbonate is 80% or more.

[0033] The present invention has at least the following beneficial effects:

[0034] This invention introduces a first and a second flame-retardant monomer through copolymerization during the preparation of polycarbonate, employing isosorbide and aliphatic diols. These monomers work synergistically, resulting in polycarbonate with improved flame retardancy while also exhibiting superior thermal, mechanical, and weather resistance properties, without significantly impacting light transmittance, thus meeting broader market demands. Furthermore, both the first and second flame-retardant monomers are halogen-free, offering excellent safety and environmental performance. The preparation method of this invention is simple, efficient, and easily scalable for mass production. Attached Figure Description

[0035] Figure 1 This is a schematic flowchart illustrating the preparation method of copolymer flame-retardant polycarbonate according to a specific embodiment of the present invention. Detailed Implementation

[0036] To provide a clearer understanding of the technical features, objectives, and beneficial effects of the present invention, the present invention will now be described in detail below, but this should not be construed as limiting the scope of the invention.

[0037] According to a specific embodiment of the first aspect of the present invention, the present invention provides a method for preparing a copolymer flame-retardant polycarbonate, which includes the following steps: reacting carbonate diester, isosorbide, aliphatic diol, a first flame-retardant monomer and a second flame-retardant monomer in the presence of a catalyst to obtain the copolymer flame-retardant polycarbonate;

[0038] Wherein, the first flame-retardant monomer comprises one or more compounds having the structure shown in Formula I:

[0039]

[0040] In Formula I, R1 and R2 are each independently selected from one of carboxyl, alkyl ester, and hydroxyalkyl ester groups;

[0041] The second flame-retardant monomer comprises one or more compounds having the structure shown in Formula II:

[0042]

[0043] In Formula II, R3 and R4 are each independently selected from carboxyl and alkyl ester groups.

[0044] This invention employs a carboxylic acid compound or ester compound containing a phenylacetylene group as the first flame-retardant monomer, and a carboxylic acid compound or ester compound containing both phenylacetylene and benzoimide structures as the second flame-retardant monomer. This allows the polycarbonate of this invention to improve its flame-retardant properties while also possessing superior thermal and mechanical properties, without significantly affecting its light transmittance. Specifically, the phenylacetylene group can provide a cross-linked network structure at high temperatures, which improves the thermal and flame-retardant properties of the polycarbonate. Simultaneously, the π-π stacking structure of the phenylacetylene group enhances the inter-chain interactions, thereby improving the mechanical properties of the polycarbonate. Furthermore, the phenylacetylene group and the benzoimide structure can synergistically cross-link during combustion, further enhancing the flame-retardant properties of the polycarbonate. Simultaneously, both the phenylacetylene group and the benzoimide structure contain conjugated structures. These conjugated structures can absorb ultraviolet light, reducing the attack of ultraviolet rays on the polycarbonate molecular chain. Furthermore, the presence of the phenylacetylene group and the benzoimide structure can alter the electron cloud distribution of polycarbonate, improving its antioxidant capacity; thus, it enhances the weather resistance of polycarbonate. This invention, through the synergistic effect of the two flame-retardant monomers, improves the flame-retardant properties, thermal properties, mechanical properties, and weather resistance of polycarbonate. Moreover, the synergistic effect between the two flame-retardant monomers and the aliphatic diol further enhances the mechanical properties of polycarbonate.

[0045] The first flame-retardant monomer of the present invention can be commercially available or prepared using methods in the prior art, for example: esterifying 4-phenylethynyl phthalic anhydride with an alkyl alcohol to obtain 4-phenylethynyl phthalate diester; or further transesterifying the obtained 4-phenylethynyl phthalate diester with an alkyl diol to obtain 4-phenylethynyl phthalate dihydroxyalkyl ester. The conditions and specific steps of these reactions can be conventionally adjusted by those skilled in the art.

[0046] The second flame-retardant monomer of the present invention can be prepared using methods in the prior art, for example, by imidizing 4-phenylethynyl phthalic anhydride and 5-aminoisophthalic acid or 5-aminoisophthalic acid diester to obtain the second flame-retardant monomer. The reaction conditions and specific steps can be conventionally adjusted by those skilled in the art.

[0047] In some embodiments, in Formula I, R1 and R2 are each independently selected from one of carboxyl, methyl ester, and hydroxyethyl ester groups. Specifically, the first flame-retardant monomer includes one or more of 4-phenylethynyl phthalic acid, dimethyl 4-phenylethynyl phthalate, and di(ethylene glycol) 4-phenylethynyl phthalate. Both 4-phenylethynyl phthalic acid and dimethyl 4-phenylethynyl phthalate are commercially available. Di(ethylene glycol) 4-phenylethynyl phthalate can be prepared by methods in the prior art, for example, by transesterifying dimethyl 4-phenylethynyl phthalate with ethylene glycol to obtain di(ethylene glycol) 4-phenylethynyl phthalate. The catalyst used in this reaction can be, for example, zinc acetate, and the reaction is carried out in a protective gas atmosphere (e.g., nitrogen) at a temperature of 170–180°C for 5–7 hours.

[0048] In some embodiments, in Formula II, R3 and R4 are each independently selected from a carboxyl group and a methyl ester group. Specifically, the second flame-retardant monomer includes one or two of 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalic acid and dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate. These two compounds can be prepared by at least the following steps: mixing 5-aminoisophthalic acid or dimethyl 5-aminoisophthalate with an appropriate amount of organic solvent (e.g., N-methylpyrrolidone), then adding 4-phenylethynyl phthalic anhydride in a protective gas atmosphere (e.g., nitrogen), and stirring continuously at 70–80 °C for 2–3 h; then adding toluene as an azeotropic agent and heating to 170–180 °C for 6–8 h to obtain 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalic acid or dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate.

[0049] In some embodiments, the diester includes one or more of dimethyl carbonate, diphenyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, dipentyl carbonate, and dioctyl carbonate. Preferably, the diester includes one or two of dimethyl carbonate and diphenyl carbonate.

[0050] In some embodiments, the aliphatic diol includes one or more of 1,4-cyclohexanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol. Preferably, the aliphatic diol includes 1,4-cyclohexanediol.

[0051] In some embodiments, the total amount of isosorbide, aliphatic diol, first flame retardant monomer and second flame retardant monomer to the diester is in a molar ratio of (0.7 to 1):1.

[0052] In some embodiments, the molar ratio of isosorbide, the aliphatic diol, the first flame retardant monomer, and the second flame retardant monomer is (0.5–0.7):(0.1–0.2):(0.05–0.15):(0.05–0.15). Preferably, the molar ratio of the first flame retardant monomer to the second flame retardant monomer is 1:3 to 3:1.

[0053] In some embodiments, the catalyst comprises one or more of the following: sodium tert-butoxide, lithium acetylacetonate, tetramethylammonium hydroxide, sodium tetraborate, lithium hydroxide monohydrate, lithium chloride, potassium dihydrogen phosphate, cesium carbonate, tetraisopropyl titanate, sodium methoxide, and sodium borohydride; the amount of the catalyst used is 0.01% to 0.1% of the molar amount of the diester. Preferably, the catalyst comprises cesium carbonate.

[0054] In some embodiments, the reaction includes transesterification and polycondensation. The conditions for the transesterification reaction include: a reaction temperature of 100°C to 200°C, a pressure of 10 kPa to 50 kPa, and a time of 0.5 h to 3 h. The conditions for the polycondensation reaction include: a reaction temperature of 200°C to 260°C, a pressure of 0 kPa to 1 kPa, and a time of 0.5 h to 3 h. Preferably, the conditions for the transesterification reaction include: a reaction temperature of 180°C to 200°C, a pressure of 10 kPa to 30 kPa, and a time of 1.5 h to 3 h. The conditions for the polycondensation reaction include: a reaction temperature of 240°C to 250°C, a pressure of 0 kPa to 0.5 kPa, and a time of 0.5 h to 2 h.

[0055] In some embodiments, such as Figure 1 As shown, the preparation method of the copolymer flame-retardant polycarbonate includes the following steps:

[0056] (1) Air tightness check: The reaction apparatus is replaced with a protective gas (e.g., nitrogen) several times (e.g., three times), and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0057] (2) Addition: In a protective gas atmosphere (e.g., nitrogen), add the carbonate diester, isosorbide, aliphatic diol, first flame retardant monomer and second flame retardant monomer into the reaction apparatus;

[0058] (3) Pulping: Set the temperature inside the reaction device to 100℃~200℃ to melt the carbonate, isosorbide, aliphatic diol, first flame retardant monomer and second flame retardant monomer, and turn on the stirring device inside the reaction device (preferably 100~250rpm) to fully mix the raw materials.

[0059] (4) Transesterification reaction: The catalyst is added to the reaction apparatus, and the temperature inside the reaction apparatus is set to 100℃~200℃ (preferably 180℃~200℃) and the pressure is set to 10kPa~50kPa (preferably 10kPa~30kPa). The transesterification reaction is carried out under stirring conditions for 0.5h~3h (preferably 1.5h~3h). Byproducts can be removed by conventional methods (e.g., distilling the alcohol and / or phenol generated in the reaction out of the reaction apparatus).

[0060] (5) Polycondensation reaction: Then, the temperature in the reaction device is gradually increased to 200℃~260℃ (preferably 240℃~250℃) and the pressure is gradually decreased to 0kPa~1kPa (preferably 0kPa~0.5kPa). The polycondensation reaction is carried out under stirring conditions for 0.5h~3h (preferably 0.5h~2h). After removing the by-products by conventional methods, melt copolymer flame-retardant polycarbonate is obtained.

[0061] (6) Extrusion and pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain the copolymer flame-retardant polycarbonate.

[0062] According to a specific embodiment of the second aspect of the present invention, the present invention provides a copolymer flame-retardant polycarbonate, which is prepared by the above-described method for preparing copolymer flame-retardant polycarbonate.

[0063] In some embodiments, the number average molecular weight of the copolymer flame-retardant polycarbonate is 10,000 to 50,000 g / mol, preferably 25,000 to 40,000 g / mol.

[0064] In some embodiments, the glass transition temperature of the copolymer flame-retardant polycarbonate is 110–140°C, preferably 120–140°C.

[0065] In some embodiments, the copolymer flame-retardant polycarbonate has an elongation at break of 70–120%, a tensile strength of 60–90 MPa, and a notched impact strength of 7–10 kJ / m. 2 .

[0066] In some embodiments, the limiting oxygen index of the copolymer flame-retardant polycarbonate is 35-40%, and the flame retardant rating of the copolymer flame-retardant polycarbonate is UL94 V-0.

[0067] In some embodiments, the light transmittance of the copolymer flame-retardant polycarbonate is 80% or higher.

[0068] The present invention is illustrated in detail below by way of examples, but the present invention is not limited to these examples. Of course, various modifications can be made within the scope of the present invention.

[0069] Test method:

[0070] Number average molecular weight: obtained by gel permeation chromatography (GPC) with DMF as solvent and polystyrene as standard.

[0071] Glass transition temperature: Tested according to the specifications in GB / T 11998-1989.

[0072] Elongation at break, tensile strength, and notched impact strength: Tensile strength and elongation at break were tested according to GB / T 1040.1-2018 at a test rate of 50 mm / min, using dumbbell-shaped samples with the sample size of Type 1A as specified in GB / T1040.2-2022. Notched impact strength was tested according to GB / T 1043.1-2008 with a Type A notch.

[0073] Limiting oxygen index: Tested according to the description in GB 2406.2-2009.

[0074] Flame retardancy rating: Tested according to the method described in the vertical burning test in UL94-2018.

[0075] Light transmittance: Tested according to the specifications in GB / T 2410-2008. A circular piece with a diameter of 50 mm or a square piece of 50 mm × 50 mm was used for the test.

[0076] Weather resistance: Samples were aged using a xenon lamp aging tester, and the elongation at break, tensile strength, and notched impact strength of the aged samples were tested. Test conditions included: xenon lamp aging tester (ISO 4892.2-2013), irradiance of 0.51 W / m². 2 The wavelength was 340nm, the chamber temperature was 60℃, the humidity was 50 (±10)%, and the irradiation time was 1500h.

[0077] Yield: (Actual product mass / Theoretical product mass) × 100%. Theoretical product mass is the mass of all raw materials after attachment to the main chain and removal of small molecules.

[0078] Example 1

[0079] (1) Air tightness check: The reaction apparatus is replaced with nitrogen three times, and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0080] (2) Addition: Under a nitrogen atmosphere at room temperature, diphenyl carbonate, isosorbide, 1,4-cyclohexanediol, di(ethylene glycol) 4-phenylethynyl phthalate and dimethyl isophthalate in a molar ratio of 1:0.7:0.1:0.05:0.05 are added to the reaction apparatus.

[0081] (3) Pulping: Set the temperature inside the reaction device to 100℃ to melt the raw materials, and turn on the stirring device inside the reaction device at a stirring speed of 150 rpm to fully mix the raw materials;

[0082] (4) Transesterification reaction: Cesium carbonate was added to the reaction apparatus at a rate of 0.01 mol% of the amount of diphenyl carbonate. The temperature in the reaction apparatus was set to 180 °C and the pressure was set to 10 kPa. The transesterification reaction was carried out under stirring conditions for 3 hours. The alcohol produced by the reaction was then distilled off the reaction apparatus.

[0083] (5) Polycondensation reaction: Then the temperature in the reaction device is gradually increased to 240℃ and the pressure is gradually decreased to 100Pa. The polycondensation reaction is carried out under stirring conditions for 0.5h. After the reaction is completed, melt copolymer flame retardant polycarbonate is obtained.

[0084] (6) Extrusion pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain copolymer flame-retardant polycarbonate.

[0085] Di(ethylene glycol) 4-phenylethynyl phthalate was prepared via the following steps: Dimethyl 4-phenylethynyl phthalate and ethylene glycol were subjected to transesterification in a nitrogen atmosphere and in the presence of zinc acetate as a catalyst. The amount of zinc acetate was 0.5 mol% of the amount of dimethyl 4-phenylethynyl phthalate. The reaction temperature was 180℃ and the reaction time was 5 h. After the reaction, the product was washed, filtered, and then rotary evaporated at 50℃ to obtain di(ethylene glycol) 4-phenylethynyl phthalate. Infrared spectroscopy was performed on the product, and the results showed that the product was precipitated in the range of 3300-3400 cm⁻¹. -1 A stretching vibration peak of -OH appears; in the range of 2882-2997 cm⁻¹. -1 A stretching vibration peak of -CH2 appears; at 3069 cm⁻¹ -1 CH stretching vibrations of the benzene ring are observed nearby; at 2210 cm⁻¹ -1 A stretching vibration peak of an asymmetric disubstituted alkyne group appears nearby; at 1250 cm⁻¹ -1 Antisymmetric stretching vibration peaks of ester groups appear nearby.

[0086] The structural formula of 4-phenylethynyl phthalate di(ethylene glycol) ester is shown below:

[0087]

[0088] Dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate was prepared by the following steps: 15 g of 5-aminoisophthalate and 250 mL of N-methylpyrrolidone were mixed by stirring at room temperature; then 17.8 g of 4-phenylethynyl phthalic anhydride was added, and the resulting mixture was stirred at 75 °C for 2 h under a nitrogen atmosphere; then 70 mL of toluene was added as an azeotropic agent, and the mixture was gradually heated to 170 °C for 8 h until the reaction was complete; the mixture was then cooled to 120 °C and poured into excess water to obtain a precipitate; the precipitate was filtered, washed, and dried to obtain dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate.

[0089] The structural formula of dimethyl isophthalate 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl) isophthalate is shown below:

[0090]

[0091] The copolymer flame-retardant polycarbonate was tested using the method described above, and the test results are shown in Table 1. It should be noted that the test used the sample size specified in the standard described above; therefore, the test samples can be prepared from granules or directly prepared without pelletizing.

[0092] Example 2

[0093] (1) Air tightness check: The reaction apparatus is replaced with nitrogen three times, and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0094] (2) Addition: Under a nitrogen atmosphere at room temperature, diphenyl carbonate, isosorbide, 1,4-cyclohexanediol, di(ethylene glycol) 4-phenylethynyl phthalate and dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate in a molar ratio of 1:0.7:0.15:0.05:0.1 are added to the reaction apparatus.

[0095] (3) Pulping: Set the temperature inside the reaction device to 100℃ to melt the raw materials, and turn on the stirring device inside the reaction device at a stirring speed of 150 rpm to fully mix the raw materials;

[0096] (4) Transesterification reaction: Cesium carbonate was added to the reaction apparatus at a rate of 0.01 mol% of the amount of diphenyl carbonate. The temperature in the reaction apparatus was set to 200 °C and the pressure to 30 kPa. The transesterification reaction was carried out under stirring conditions for 1.5 h. The alcohol produced by the reaction was then distilled off the reaction apparatus.

[0097] (5) Polycondensation reaction: Then the temperature in the reaction device is gradually increased to 250℃ and the pressure is gradually decreased to 500Pa. The polycondensation reaction is carried out under stirring conditions for 1 hour. After the reaction is completed, melt copolymer flame-retardant polycarbonate is obtained.

[0098] (6) Extrusion pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain copolymer flame-retardant polycarbonate.

[0099] The copolymer flame-retardant polycarbonate was tested using the method described above, and the test results are shown in Table 1.

[0100] Example 3

[0101] (1) Air tightness check: The reaction apparatus is replaced with nitrogen three times, and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0102] (2) Addition: Under a nitrogen atmosphere at room temperature, diphenyl carbonate, isosorbide, 1,4-cyclohexanediol, di(ethylene glycol) 4-phenylethynyl phthalate and dimethyl isophthalate in a molar ratio of 1:0.6:0.1:0.075:0.075 are added to the reaction apparatus.

[0103] (3) Pulping: Set the temperature inside the reaction device to 100℃ to melt the raw materials, and turn on the stirring device inside the reaction device at a stirring speed of 150 rpm to fully mix the raw materials;

[0104] (4) Transesterification reaction: Cesium carbonate was added to the reaction apparatus at a rate of 0.01 mol% of the amount of diphenyl carbonate. The temperature in the reaction apparatus was set to 190 °C and the pressure was set to 20 kPa. The transesterification reaction was carried out under stirring conditions for 2 hours. The alcohol produced by the reaction was then distilled off the reaction apparatus.

[0105] (5) Polycondensation reaction: Then, the temperature in the reaction device is gradually increased to 240℃ and the pressure is gradually decreased to 100Pa. The polycondensation reaction is carried out under stirring conditions for 2 hours. After the reaction is completed, melt copolymer flame-retardant polycarbonate is obtained.

[0106] (6) Extrusion pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain copolymer flame-retardant polycarbonate.

[0107] The copolymer flame-retardant polycarbonate was tested using the method described above, and the test results are shown in Table 1.

[0108] Example 4

[0109] (1) Air tightness check: The reaction apparatus is replaced with nitrogen three times, and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0110] (2) Addition: Under a nitrogen atmosphere at room temperature, diphenyl carbonate, isosorbide, 1,4-cyclohexanediol, di(ethylene glycol) 4-phenylethynyl phthalate and dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate are added to the reaction apparatus in a molar ratio of 1:0.5:0.2:0.15:0.05.

[0111] (3) Pulping: Set the temperature inside the reaction device to 150℃ to melt the raw materials, and turn on the stirring device inside the reaction device at a stirring speed of 150 rpm to fully mix the raw materials;

[0112] (4) Transesterification reaction: Cesium carbonate was added to the reaction apparatus at a rate of 0.05 mol% of the amount of diphenyl carbonate. The temperature in the reaction apparatus was set to 190 °C and the pressure was set to 20 kPa. The transesterification reaction was carried out under stirring conditions for 3 hours. The alcohol produced by the reaction was then distilled off the reaction apparatus.

[0113] (5) Polycondensation reaction: Then the temperature in the reaction device is gradually increased to 250℃ and the pressure is gradually decreased to 200Pa. The polycondensation reaction is carried out under stirring conditions for 0.5h. After the reaction is completed, melt copolymer flame retardant polycarbonate is obtained.

[0114] (6) Extrusion pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain copolymer flame-retardant polycarbonate.

[0115] The copolymer flame-retardant polycarbonate was tested using the method described above, and the test results are shown in Table 1.

[0116] Example 5

[0117] (1) Air tightness check: The reaction apparatus is replaced with nitrogen three times, and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0118] (2) Addition: Under a nitrogen atmosphere at room temperature, dimethyl carbonate, isosorbide, 1,4-cyclohexanediol, di(ethylene glycol) 4-phenylethynyl phthalate and dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate were added to the reaction apparatus in a molar ratio of 1.4:0.6:0.2:0.05:0.15;

[0119] (3) Pulping: Set the temperature inside the reaction device to 180℃ to melt the raw materials, and turn on the stirring device inside the reaction device at a stirring speed of 150 rpm to fully mix the raw materials;

[0120] (4) Transesterification reaction: Cesium carbonate is added to the reaction apparatus at a rate of 0.1 mol% of the amount of dimethyl carbonate. The temperature in the reaction apparatus is set to 190°C and the pressure is set to 30 kPa. The transesterification reaction is carried out under stirring conditions for 3 hours. The alcohol produced in the reaction is then distilled off the reaction apparatus.

[0121] (5) Polycondensation reaction: Then the temperature in the reaction device is gradually increased to 240℃ and the pressure is gradually decreased to 100Pa. The polycondensation reaction is carried out under stirring conditions for 0.5h. After the reaction is completed, melt copolymer flame retardant polycarbonate is obtained.

[0122] (6) Extrusion pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain copolymer flame-retardant polycarbonate.

[0123] The copolymer flame-retardant polycarbonate was tested using the method described above, and the test results are shown in Table 1.

[0124] Example 6

[0125] (1) Air tightness check: The reaction apparatus is replaced with nitrogen three times, and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0126] (2) Addition: Under a nitrogen atmosphere at room temperature, diethyl carbonate, isosorbide, 1,4-butanediol, 4-phenylethynyl phthalic acid and dimethyl isophthalate in a molar ratio of 1:0.7:0.15:0.1:0.05 are added to the reaction apparatus.

[0127] (3) Pulping: Set the temperature inside the reaction device to 100℃ to melt the raw materials, and turn on the stirring device inside the reaction device at a stirring speed of 150 rpm to fully mix the raw materials;

[0128] (4) Transesterification reaction: Lithium acetylacetonate was added to the reaction apparatus. The amount of lithium acetylacetonate was 0.05 mol% of the amount of diethyl carbonate. The temperature in the reaction apparatus was set to 100℃ and the pressure was set to 50 kPa. The transesterification reaction was carried out under stirring conditions for 3 hours. The alcohol produced by the reaction was distilled out of the reaction apparatus.

[0129] (5) Polycondensation reaction: Then the temperature in the reaction device is gradually increased to 260℃ and the pressure is gradually decreased to 1kPa. The polycondensation reaction is carried out under stirring conditions for 0.5h. After the reaction is completed, melt copolymer flame retardant polycarbonate is obtained.

[0130] (6) Extrusion pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain copolymer flame-retardant polycarbonate.

[0131] The copolymer flame-retardant polycarbonate was tested using the method described above, and the test results are shown in Table 1.

[0132] Example 7

[0133] (1) Air tightness check: The reaction apparatus is replaced with nitrogen three times, and the pressure gauge is observed to check the air tightness of the reaction apparatus.

[0134] (2) Addition: Under a nitrogen atmosphere at room temperature, diphenyl carbonate, isosorbide, 1,5-pentanediol, dimethyl 4-phenylethynyl phthalate and 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalic acid in a molar ratio of 1:0.7:0.15:0.1:0.05 are added to the reaction apparatus.

[0135] (3) Pulping: Set the temperature inside the reaction device to 100℃ to melt the raw materials, and turn on the stirring device inside the reaction device at a stirring speed of 150 rpm to fully mix the raw materials;

[0136] (4) Transesterification reaction: Tetraisopropyl titanate was added to the reaction apparatus. The amount of tetraisopropyl titanate was 0.1 mol% of the amount of diphenyl carbonate. The temperature in the reaction apparatus was set to 150℃ and the pressure was set to 40 kPa. The transesterification reaction was carried out under stirring conditions for 0.5 h. The alcohol produced by the reaction was distilled off the reaction apparatus.

[0137] (5) Polycondensation reaction: Then the temperature in the reaction device is gradually increased to 200℃ and the pressure is gradually decreased to 800Pa. The polycondensation reaction is carried out under stirring conditions for 3 hours. After the reaction is completed, melt copolymer flame-retardant polycarbonate is obtained.

[0138] (6) Extrusion pelletizing: The melt copolymer flame-retardant polycarbonate is extruded and pelletized to obtain copolymer flame-retardant polycarbonate.

[0139] The preparation steps of 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalic acid are basically the same as those of 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalic acid dimethyl ester in Example 1, except that 5-aminoisophthalic acid dimethyl ester is replaced with 5-aminoisophthalic acid, and its molar ratio with 4-phenylethynyl phthalic anhydride is 1:1.

[0140] The copolymer flame-retardant polycarbonate was tested using the method described above, and the test results are shown in Table 1.

[0141] Comparative Example 1

[0142] This comparative example is compared with Example 1, which is basically the same as Example 1, except that: 4-phenylethynyl phthalate di(ethylene glycol) ester and 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl) dimethyl isophthalate were not added, and the molar ratio of diphenyl carbonate, isosorbide and 1,4-cyclohexanediethanol was 1:0.7:0.1. All other aspects are the same as in Example 1.

[0143] The polycarbonate of this comparative example was tested using the method described above, and the test results are shown in Table 2.

[0144] Comparative Example 2

[0145] This comparative example is compared with Example 1, which is basically the same as Example 1, except that: 4-phenylethynyl phthalate di(ethylene glycol) ester was not added, and the molar ratio of diphenyl carbonate, isosorbide, 1,4-cyclohexanediol and 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)dimethyl isophthalate was 1:0.7:0.1:0.05. All other aspects are the same as in Example 1.

[0146] The copolymer flame-retardant polycarbonate of this comparative example was tested using the method described above, and the test results are shown in Table 2.

[0147] Comparative Example 3

[0148] This comparative example is compared with Example 1, which is basically the same as Example 1, except that: dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate was not added, and the molar ratio of diphenyl carbonate, isosorbide, 1,4-cyclohexanediethanol and di(ethylene glycol) 4-phenylethynyl phthalate was 1:0.7:0.1:0.05. All other aspects are the same as in Example 1.

[0149] The copolymer flame-retardant polycarbonate of this comparative example was tested using the method described above, and the test results are shown in Table 2.

[0150] Comparative Example 4

[0151] This comparative example is compared with Example 1, which is basically the same as Example 1, except that: 1,4-cyclohexanediethanol is not added, and the molar ratio of diphenyl carbonate, isosorbide, di(ethylene glycol) 4-phenylethynyl phthalate and dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate is 1:0.7:0.05:0.05. All other aspects are the same as in Example 1.

[0152] The copolymer flame-retardant polycarbonate of this comparative example was tested using the method described above, and the test results are shown in Table 2.

[0153] Table 1

[0154]

[0155] Table 2

[0156]

[0157] As can be seen from Tables 1 and 2, the copolymer flame-retardant polycarbonate of the various embodiments of the present invention introduces a first flame-retardant monomer and a second flame-retardant monomer, and uses isosorbide and aliphatic diol. The synergistic effect between them makes the polycarbonate have better flame retardant properties, thermal properties, mechanical properties, light transmittance and weather resistance. However, each comparative example omits one or two raw materials in the examples, resulting in the prepared polycarbonate having poor performance in at least one aspect of flame retardant properties, thermal properties, mechanical properties, light transmittance and weather resistance.

[0158] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. For those skilled in the art, other variations or modifications can be made based on the above description. It is impossible to exhaustively list all the implementation methods here. All obvious variations or modifications derived from the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing a copolymer flame-retardant polycarbonate, comprising the following steps: reacting a carbonate diester, isosorbide, an aliphatic diol, a first flame-retardant monomer, and a second flame-retardant monomer in the presence of a catalyst to obtain the copolymer flame-retardant polycarbonate; in, The first flame-retardant monomer comprises one or more compounds having the structure shown in Formula I: In Formula I, R1 and R2 are each independently selected from one of carboxyl, alkyl ester and hydroxyalkyl ester groups; The second flame-retardant monomer comprises one or more compounds having the structure shown in Formula II: In Formula II, R3 and R4 are each independently selected from carboxyl and alkyl ester groups.

2. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, In Formula I, R1 and R2 are each independently selected from one of carboxyl, methyl ester and hydroxyethyl ester groups.

3. The method for preparing the copolymer flame-retardant polycarbonate according to claim 2, wherein, The first flame-retardant monomer includes one or more of 4-phenylethynyl phthalic acid, dimethyl 4-phenylethynyl phthalate, and di(ethylene glycol) 4-phenylethynyl phthalate.

4. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, In Formula II, R3 and R4 are each independently selected from one of the carboxyl group and the methyl ester group.

5. The method for preparing the copolymer flame-retardant polycarbonate according to claim 4, wherein, The second flame-retardant monomer includes one or both of 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalic acid and dimethyl 5-(1,3-dioxy-5-(phenylethynyl)isoindol-2-yl)isophthalate.

6. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, The carbonate diester includes one or more of dimethyl carbonate, diphenyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, dipentyl carbonate, and dioctyl carbonate.

7. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, The aliphatic diols include one or more of 1,4-cyclohexanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol.

8. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, The molar ratio of the total amount of isosorbide, aliphatic diol, first flame retardant monomer, and second flame retardant monomer to the diester is (0.7-1):

1.

9. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, The molar ratio of isosorbide, the aliphatic diol, the first flame retardant monomer, and the second flame retardant monomer is (0.5-0.7):(0.1-0.2):(0.05-0.15):(0.05-0.15).

10. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, The catalyst comprises one or more of sodium tert-butoxide, lithium acetylacetonate, tetramethylammonium hydroxide, sodium tetraborate, lithium hydroxide monohydrate, lithium chloride, potassium dihydrogen phosphate, cesium carbonate, tetraisopropyl titanate, sodium methoxide, and sodium borohydride; the amount of the catalyst used is 0.01% to 0.1% of the molar amount of the diester.

11. The method for preparing the copolymer flame-retardant polycarbonate according to claim 1, wherein, The reaction includes transesterification and polycondensation. The conditions for the transesterification reaction are: a reaction temperature of 100℃ to 200℃, a pressure of 10 kPa to 50 kPa, and a time of 0.5 h to 3 h. The conditions for the polycondensation reaction are: a reaction temperature of 200℃ to 260℃, a pressure of 0 kPa to 1 kPa, and a time of 0.5 h to 3 h.

12. A copolymer flame-retardant polycarbonate, which is prepared by the method of any one of claims 1-11.

13. The copolymer flame-retardant polycarbonate according to claim 12, wherein, The number-average molecular weight of the copolymer flame-retardant polycarbonate is 10,000 to 50,000 g / mol.

14. The copolymer flame-retardant polycarbonate according to claim 12, wherein, The glass transition temperature of the copolymer flame-retardant polycarbonate is 110–140°C.

15. The copolymer flame-retardant polycarbonate according to claim 12, wherein, The copolymer flame-retardant polycarbonate has an elongation at break of 70–120%, a tensile strength of 60–90 MPa, and a notched impact strength of 7–10 kJ / m. 2 .

16. The copolymer flame-retardant polycarbonate according to claim 12, wherein, The limiting oxygen index of the copolymer flame-retardant polycarbonate is 35-40%, and the flame retardant rating of the copolymer flame-retardant polycarbonate is UL94 V-0.

17. The copolymer flame-retardant polycarbonate according to claim 12, wherein, The light transmittance of the copolymer flame-retardant polycarbonate is above 80%.