Method of patterning semiconductor substrate using metallate ion liquid crystal

By employing directional self-assembly and oxidation processes of metal oxide ion liquid crystals, the problem of pattern transfer at sub-10 nm feature size in existing technologies has been solved, achieving high-resolution metal oxide patterning and providing a solution for pitch doubling.

CN122095798APending Publication Date: 2026-05-26TOKYO ELECTRON LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202480068087.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-11-09
Filing Date
2024-08-23
Publication Date
2026-05-26

Smart Images

  • Figure CN122095798A_ABST
    Figure CN122095798A_ABST
Patent Text Reader

Abstract

Embodiments of improved process flows and methods are provided to use directed self-assembly (DSA) of metallate ion liquid crystals (ILC) with metallate anions to pattern a semiconductor substrate. After the metallate ILC is self-assembled into an ordered structure, an oxidation process is used to remove organic components of the ordered structure and convert the metallate anions into a metal oxide pattern. In addition to providing a robust metal oxide pattern that can be transferred to an underlying substrate, the process flows and methods disclosed herein enable ILC to be used as a pitch multiplication means in advanced patterning techniques.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-reference of relevant patents and applications

[0001] This application relates to U.S. Patent Application Serial No. 18 / 388,240, filed November 9, 2023, and claims priority to U.S. Patent Application Serial No. 18 / 388,222, filed November 9, 2023, the disclosure of which is expressly incorporated herein by reference in its entirety. Technical Field

[0002] This disclosure relates to the fabrication of semiconductor substrates. In particular, this disclosure provides improved methods and processes for patterning semiconductor substrates using directional self-assembly (DSA) of ion-liquid crystals (ILC). Background Technology

[0003] Semiconductor devices such as integrated circuits (ICs) are fabricated by sequentially depositing and patterning dielectric, conductive, and semiconductor material layers on a semiconductor substrate to form a network of electronic components and interconnects (e.g., transistors, resistors, capacitors, metal wires, contacts, and vias) integrated into a monolithic structure. At each successive technology node, the minimum feature size is reduced to decrease cost by approximately doubling the component packing density.

[0004] A common patterning method uses photolithography, which includes photoresist coating, exposure, and development steps to form a desired pattern on a substrate surface that can be transferred to an underlying layer. In conventional photolithography, a photosensitive photoresist film is coated on the substrate surface and exposed to light to convert the exposed portions of the photoresist film into reactive photoresist. After exposure, a development step is performed to remove the reactive (or unreacted) portions of the photoresist film to achieve patterning, thereby providing a photoresist pattern on the substrate.

[0005] In this technology, the resolution of the optical system used for the photolithography steps limits the minimum feature size that can be patterned under acceptable control, as well as the minimum pitch between features within the pattern. According to the Rayleigh criterion, the minimum feature size is proportional to the wavelength (λ) of the light used for imaging and inversely proportional to the numerical aperture (NA) of the projection lens. Over time, shorter wavelengths of light—from visible (436 nm) to UV (365 nm), deep UV (248 and 193 nm), and extreme UV (EUV, 13.5 nm)—have been used to reduce the feature size and pitch achievable at advanced technology nodes. Today, EUV lithography is commonly used at the industrial level for advanced patterning at 10 nm, 7 nm, and 5 nm technology nodes.

[0006] As feature sizes continue to shrink to below 5 nm, there is a desire to generate patterns with critical dimensions (CDs) smaller than the wavelengths of light widely available for industrial applications. This necessitates new patterning methods because the resolution of optical systems remains limited by the wavelength (λ) of the light used for imaging. One approach to achieving suitable photolithography for increasingly smaller CDs is to use multiple patterning techniques for pitch splitting or pitch doubling. Examples of multiple patterning techniques include Self-Aligned Double Patterning (SADP), Self-Aligned Triple Patterning (SATP), and Self-Aligned Quadruple Patterning (SAQP). These multiple patterning techniques involve using sidewall spacers, filler layers, and selective etching to define structures with pitches smaller than the original photolithographic pitch.

[0007] Directed self-assembly (DSA) of polymers and other small molecules has recently been investigated as another pitch-multiplying technique in pattern transfer. In these methods, a large template is patterned to orient the molecular self-assembly of polymers or other small molecules within the larger template to produce patterns with significantly smaller pitches. The self-assembled patterns are then used as templates for pattern transfer.

[0008] DSA of block copolymers (BCPs) has been widely studied as a pitch-multiplying technique in pattern transfer technology due to its high resolution, low cost, ease of integration, and scalability. BCPs are macromolecules composed of homogeneous blocks (or chains) covalently bonded to chemically different monomers. Due to the dis-affinity and repulsion between these blocks, the BCP phase segregates into microdomains to generate self-assembled patterns at the nano / micro scale. After self-assembly, one of the blocks is removed, and the remaining polymer is used as a mask to pattern the underlying substrate.

[0009] Despite the considerable attention garnered for DSA of block copolymers, several issues hinder their integration into semiconductor patterning processes. First, since the feature size of BCPs is controlled by the polymer's molecular weight, the minimum pitch achievable through BCP self-assembly is currently limited to 10 nm. Therefore, DSA of block copolymers cannot be used as a pitch multiplication method for pattern transfer at sub-10 nm feature sizes. Second, BCPs are soft organic blocks that, when unguided, tend to form randomly oriented multi-domain structures. This impedes their use in pattern transfer techniques.

[0010] Ionic liquid crystals (ILCs) have recently been proposed as another class of materials for molecular self-assembly. Ionic liquid crystals are salts that possess the properties of both ionic liquids (ILs) and liquid crystals (LCs). Figure 1A A mapping of coarse-grained (CG) particles within an example ILC molecule 100 is shown. Figure 1AAs shown, ILC molecule 100 (e.g., 1-dodecyl-3-methylimidazolium tetrafluoroborate) contains a cationic head group (e.g., an imidazolium-based cation) covalently bonded to an elongated alkyl tail and an anion (e.g., tetrafluoroborate, BF4). - Due to the polarity difference between ionic groups, ILC spontaneously segregates into an ordered phase (also known as an ordered structure) at or near room temperature.

[0011] Figure 1B It shows the way Figure 1A This is an example of an ordered structure formed by the directional self-assembly of ILC molecules. One main phase of the self-assembled ILC is a layered structure 110 with alternating layers. (See example...) Figure 1B As shown, the layered structure 110 comprises a first distinct layer 120 (approximately 1 nm wide) containing a cationic head group and an anionic group of ILC, and a second distinct layer 130 (approximately 2 nm wide) containing an interpenetrating alkyl tail group of ILC. The layer pitch (p) between the alternating layers of the layered structure 110 is equal to the combined width (approximately 3 nm) of the head and tail groups of the self-assembled ILC. Although other phases can be formed, Figure 1B The layered structure 110 shown (also referred to herein as a layered structure) is particularly useful in that it can be used to pattern features on a substrate with a sub-5 nm pitch.

[0012] Similar to block copolymers, ILCs self-assemble into ordered structures, but with much smaller feature scales. The ordered structures generated by self-assembled ILCs can be used for pitch multiplication in patterning transfer methods, provided the self-assembled patterns can be transferred to the underlying substrate. However, the use of ILCs in patterning techniques remains challenging. The first challenge is generating vertically layered patterns of ILCs on the substrate surface. The second challenge is transferring these vertically layered patterns to the underlying substrate. New methods and processes are needed to overcome these challenges. Summary of the Invention

[0013] This disclosure provides various embodiments of an improved method and process for patterning semiconductor substrates using directional self-assembly (DSA) of ionic liquid crystals (ILCs). Specifically, the disclosed embodiments utilize DSA of metalate ILCs having a cationic head group, an alkyl tail group, and metal anions. During the self-assembly of the metalate ILC, the polarity difference between the cationic head group and the alkyl tail group causes the head and tail groups to segregate into an ordered structure, wherein the metal anions segregate to the head layer. Oxidation of the ordered structure involves: (a) converting the organic material within the alkyl tail layer into volatile carbon oxides, which are removed from the substrate surface during the oxidation process; and (b) converting the metal anions within the head layer into non-volatile metal oxides, which remain on the substrate surface after oxidation. In doing so, the oxidation process volatilizes the ionic liquid crystal layer but leaves a metal oxide pattern in which the metal anions are concentrated. The metal oxide pattern is more robust than the ionic liquid crystal layer and can therefore be used as a hard mask in subsequent processing steps.

[0014] In addition to providing robust metal oxide patterns that can be transferred to the underlying substrate, the improved methods and processes disclosed herein enable ion-based liquid crystals to be used as a pitch multiplication means in advanced patterning techniques. By utilizing the above-described techniques, the improved methods and processes disclosed herein can be used to form metal oxide patterns with sub-5 nm pitches (e.g., 3 nm), which is much smaller than the pitches currently achievable using EUV lithography or block copolymer DSA.

[0015] According to one embodiment, this document provides a method for patterning a semiconductor substrate. The method typically includes: generating a first pattern on an underlying layer of the semiconductor substrate, wherein the first pattern comprises a plurality of features formed at a first pitch; and depositing an ion-exchange liquid crystal (ILC) solution within each of the plurality of features. The ILC solution comprises a metal-acid ion-exchange liquid crystal (ILC) having a cationic head group, an alkyl tail group, and a metal anion. The metal-acid ILC deposited within the plurality of features self-assembles into a layered structure having alternating head layers and tail layers, wherein the metal anions segregate to the head layers. After self-assembly, the method may expose the semiconductor substrate to an oxidation process to remove the tail layers from the layered structure and transform the head layers of the layered structure into a metal oxide pattern with a second pitch smaller than the first pitch. The method may further include transferring the metal oxide pattern to an underlying layer of the semiconductor substrate.

[0016] In some embodiments, the method may expose the semiconductor substrate to an oxidation process by exposing it to an oxygen plasma ashing process, an ultraviolet (UV) ozone process, a gas-phase oxidation process, or a solution-phase oxidation process. Regardless of the oxidation process used, exposing the semiconductor substrate to an oxidation process oxidizes the layered structure to: (a) convert the tail layer into volatile carbon oxides, which are then removed from the layered structure during the oxidation process; and (b) convert metal anions in the head layer into non-volatile metal oxides, which are retained after the oxidation process. The non-volatile metal oxides generated by the oxidation of the metal anions form a metal oxide pattern, which is then transferred to the underlying layer of the semiconductor substrate.

[0017] The ILC solution deposited within the feature portion can contain a wide variety of metal acid salt ILCs having various cationic head groups, alkyl tail groups, and metal acid anions. In some embodiments, the metal acid salt ILC contained in the ILC solution can contain cationic head groups based on imidazolium, pyrazolium, pyrrolidineonium, pyridinium, piperidinium, morpholinium, ammonium, phosphonium, sulfonium, or cholineonium. In some embodiments, the metal acid salt ILC can contain a cationic head group based on imidazolium in the form of 1-R1-3-R2-imidazolium, where R1 is an alkyl chain with a chain length ranging from 8 to 18 carbons, and R2 is hydrogen, methyl, ethyl, propyl, butyl, substituted or unsubstituted phenyl, or other hydrocarbon groups. In an example embodiment, the metal acid salt ILC can be composed of a 1-dodecyl-3-methylimidazolium cation and a metal acid anion. A wide variety of metal acid anions can be used, including aluminochloroaluminate anion, ferrochlorochloroaluminate anion, stanchlorochloroaluminate anion, indium chloride anion, or zinc chloride anion. In one example embodiment, the metal acid salt ILC can be 1-dodecyl-3-methylimidazolium tetrachloroaluminate. In another example embodiment, the metal acid salt ILC can be 1-dodecyl-3-methylimidazolium tetrachloroferrate.

[0018] In some embodiments, the method may generate a first pattern on an underlying layer of a semiconductor substrate by: (a) depositing a neutral layer on the underlying layer of the semiconductor substrate; (b) depositing a hydrophilic layer on the neutral layer; and (c) using a photolithography process to generate the first pattern within the hydrophilic layer, such that the bottom of the neutral layer is exposed at each feature and the sidewall surface of each feature is exposed. In some embodiments, the photolithography process may form a plurality of trenches within the hydrophilic layer to form a pattern of hydrophilic lines on the neutral layer, and an ILC solution may be deposited within the plurality of trenches. In other embodiments, the photolithography process may form a pattern of holes extending through the hydrophilic layer to the neutral layer, and an ILC solution may be deposited within each hole formed within the hydrophilic layer.

[0019] In some embodiments, metalate ILCs deposited within multiple feature portions can self-assemble into a vertically layered structure with alternating head and tail layers, wherein the head layers of the vertically layered structure are oriented toward the sidewall surfaces of the feature portions. The layer pitch between the alternating layers of the vertically layered structure is equal to the combined width of the head and tail groups of the self-assembled ILC and typically depends on the chain length of the alkyl tail group. In some embodiments, the width of each feature portion can be an integer multiple of the layer pitch between the alternating layers of the vertically layered structure. This allows the metalate ILCs to orient themselves and self-assemble into a vertically layered structure within the feature portions.

[0020] In some embodiments, the method may further include controlling the layer pitch between alternating layers of a vertically layered structure by controlling the chain length of the alkyl tail. For example, the method may utilize metal acid salt ILCs with longer alkyl chain lengths to increase the layer pitch, or utilize metal acid salt ILCs with smaller alkyl chain lengths to decrease the layer pitch. By selecting metal acid salt ILCs that self-assemble into vertically layered structures with a layer pitch smaller than the first pitch between a plurality of features, and oxidizing the vertically layered structure to produce a metal oxide pattern with a second pitch equal to that layer pitch, the method disclosed herein can be used to provide pitch multiplication for advanced patterning techniques.

[0021] According to another embodiment, this document provides a pitch multiplication method, which typically includes: (a) generating a first pattern on a semiconductor substrate, the first pattern comprising a plurality of features formed at a first pitch; and (b) generating a second pattern within each of the plurality of features using oriented self-assembly (DSA) of a metal-ion liquid crystal (ILC), followed by oxidation to convert metal anions contained within the metal-ion ILC into metal oxides. The second pattern comprising metal oxides may be formed at a second pitch smaller than the first pitch.

[0022] In some embodiments, the method may generate a second pattern by: (a) depositing an ion-soluble liquid crystal (ILC) solution comprising a metal acid salt ILC in each of a plurality of features, wherein the metal acid salt ILC comprises a cationic head group, an alkyl tail group and a metal anion, and wherein the metal acid salt ILC deposited in the plurality of features self-assembles into a layered structure having alternating layers of head and tail layers, wherein the metal anion segregates to the head layer; and (b) exposing a semiconductor substrate to an oxidation process to remove the tail layer from the layered structure and convert the metal anion into a metal oxide.

[0023] In some embodiments, the method can generate a first pattern by: (a) depositing a neutral layer on a semiconductor substrate, (b) depositing a hydrophilic layer on the neutral layer, and (c) using a photolithography process to generate a first pattern within the hydrophilic layer, such that the neutral layer is exposed at the bottom of each feature and the hydrophilic layer is exposed on the sidewall surface of each feature. When metallate ILCs are deposited within multiple features, the metallate ILCs can self-assemble into a vertically layered structure having alternating head and tail layers, wherein the head layer is oriented toward the sidewall surface of the feature.

[0024] The semiconductor substrate is exposed to an oxidation process to remove the tail layer from the vertically layered structure and convert metal anions into metal oxides. A variety of oxidation processes can be used in this method. For example, the semiconductor substrate can be exposed to an oxygen plasma ashing process, an ultraviolet (UV) ozone process, a gas-phase oxidation process, or a solution-phase oxidation process. Regardless of the oxidation process used, the vertically layered structure formed within multiple feature areas is oxidized to: (a) convert the tail layer into volatile carbon oxides, which are removed from the vertically layered structure during the oxidation process; and (b) convert the metal anions within the head layer into non-volatile metal oxides, which remain on the substrate after the oxidation process.

[0025] In some embodiments, the method may further include controlling the layer pitch between alternating layers of the vertically layered structure by controlling the chain length of the alkyl tail group contained within the metal acid salt ILC. In some embodiments, the width of each feature may be an integer multiple of the layer pitch between alternating layers of the vertically layered structure, and the second pitch (between the metal oxides of the second pattern) may be equal to that layer pitch.

[0026] As noted above and further described herein, this disclosure provides various embodiments of a method for patterning semiconductor substrates using directional self-assembly (DSA) of metal-acid ILCs. Of course, for clarity, the order of discussion of the different steps described herein has been presented. Generally, these steps can be performed in any suitable order. Additionally, although each of the different features, techniques, configurations, etc., herein may be discussed in different places, it is intended that each of these concepts can be carried out independently of or in combination with each other. Therefore, the invention can be embodied and viewed in many different ways.

[0027] Note that the Summary of the Invention does not specify every embodiment and / or incremental novelty aspect of this disclosure or the claimed invention. Rather, the Summary provides only a preliminary discussion of different embodiments and corresponding novelty relative to conventional techniques. For additional details and / or possible perspectives on the invention and its embodiments, the reader is directed to the Detailed Description of the Invention and the corresponding accompanying drawings, which are discussed further below. Attached Figure Description

[0028] A more complete understanding of the invention and its advantages can be obtained by referring to the following description taken in conjunction with the accompanying drawings, in which similar reference numerals indicate similar features. However, it should be noted that the drawings only illustrate exemplary embodiments of the disclosed concepts and are therefore not intended to limit the scope, as the disclosed concepts may imply other equally effective embodiments.

[0029] Figure 1A This is a mapping of coarse-grained (CG) particles in an example ion-ion liquid crystal (ILC).

[0030] Figure 1B An example of an ordered structure formed at room temperature by directional self-assembly (DSA) of ILC is shown.

[0031] Figure 2 (a)- Figure 2 (c) A coarse-grained simulation is provided showing that the DSA of the ILC can be controlled by adjusting the hydrophobicity of the guiding surface.

[0032] Figure 3 This is a coarse-grained simulation illustrating the challenges encountered when attempting to form a vertically layered ILC structure on the surface of a periodic substrate in a vacuum.

[0033] Figure 4 This is a flowchart illustrating one embodiment of a method for patterning a semiconductor substrate using a metallate ILC followed by oxidation.

[0034] Figure 5 It is for demonstration and use. Figure 4 The method shown is a block diagram of an example process flow for patterning a semiconductor substrate.

[0035] Figure 6 This is a flowchart illustrating an embodiment of a pitch multiplication method using a metal salt ILC with DSA followed by oxidation. Detailed Implementation

[0036] This disclosure provides various embodiments of an improved method and process for patterning semiconductor substrates using directional self-assembly (DSA) of ionomer liquid crystals (ILCs). Specifically, the disclosed embodiments utilize DSA of metalate ILCs having a cationic head group, an alkyl tail group, and metal anions. During the self-assembly of the metalate ILC, the polarity difference between the cationic head group and the alkyl tail group causes the head and tail groups to segregate into an ordered structure, wherein the metal anions segregate to the head layer. Oxidation of the ordered structure involves: (a) converting the organic material within the alkyl tail layer into volatile carbon oxides, which are removed from the substrate surface during the oxidation process; and (b) converting the metal anions within the head layer into non-volatile metal oxides, which remain on the substrate surface after oxidation. In doing so, the oxidation process volatilizes the ionomer liquid crystal layer but leaves a metal oxide pattern in which the metal anions are concentrated. The metal oxide pattern is more robust than the ionomer liquid crystal layer and can therefore be used as a hard mask in subsequent processing steps.

[0037] In addition to providing robust metal oxide patterns that can be transferred to the underlying substrate, the improved methods and processes disclosed herein enable ion-based liquid crystals to be used as a pitch multiplication means in advanced patterning techniques. By utilizing the above-described techniques, the improved methods and processes disclosed herein can be used to form metal oxide patterns with sub-5 nm pitches (e.g., 3 nm), which is much smaller than the pitches currently achievable using EUV lithography or block copolymer DSA.

[0038] Similar to block copolymers, the ordered structure of ionic liquid crystals can be controlled by the chain length of the alkyl tails, the balance of electrostatic and van der Waals interactions, temperature, and interactions with the substrate. For example, the periodicity or pitch between ordered structures can be controlled by adjusting the chain length of the alkyl tails. The orientation of the ordered structure is also highly influenced by the hydrophobicity of the guiding surfaces (such as the underlying substrate surface and / or the sidewalls of larger template patterns).

[0039] Figure 2 (a)- Figure 2 (c) Shows coarse-grained (CG) simulation results of various layered structures formed by directional self-assembly (DSA) of example ILCs (e.g., 1-dodecyl-3-methylimidazolium tetrafluoroborate). Figure 2 In embodiment 200 shown in (a), the substrate 210 is provided with a hydrophilic surface layer 220. For example... Figure 2 As shown in (a), the self-assembly of ILC on the hydrophilic surface layer 220 produces a horizontal layered structure 222, which comprises alternating horizontal layers of cationic head groups 224 and interpenetrating alkyl tail groups 226.

[0040] Vertically layered structures can be formed by assembling ILCs on the surface of other substrates, such as... Figure 2 (b) and Figure 2 As shown in (c). In Figure 2 (b) In embodiment 230 shown, the substrate 210 is provided with a periodic surface 240, which comprises alternating hydrophilic and hydrophobic surface layers. Figure 2 As shown in (b), the self-assembly of the ILC on the periodic surface 240 produces a vertically layered structure 242 comprising alternating vertical layers of cationic head groups 244 and interpenetrating alkyl tail groups 246. Figure 2 (c) In embodiment 250 shown, the feature portion formed on the substrate 210 is provided with a neutral bottom surface 260 and a hydrophilic sidewall 261. Figure 2 As shown in (c), the self-assembly of the ILC within the feature portion produces a vertically layered structure 262, which comprises alternating vertical layers of cationic head groups 264 and interpenetrating alkyl tail groups 266.

[0041] like Figure 2 (a)- Figure 2 As shown in (c), the polarity difference between the cationic head group 224 / 244 / 264 and the alkyl tail group 226 / 246 / 266 promotes the self-assembly of the ILC molecule and causes the head and tail groups to segregate into layered structures, including horizontally oriented ( Figure 2 (a) and vertical orientation ( Figure 2 (b)- Figure 2 (c) Both. For example Figure 2 (b) and Figure 2 As shown in (c), the layer pitch (p) between alternating layers in a vertically oriented layered structure is equal to the combined width of the head and tail groups of the self-assembled ILC molecule. Since the layer pitch (p) is much smaller than the layer pitch currently achievable using photolithography, therefore... Figure 2 (b) and Figure 2 The vertical layered structure shown in (c) can be used as a pattern for pitch multiplication, provided that these patterns can be successfully transferred to the underlying substrate 210. However, both forming the vertical layered pattern of the ILC and transferring the vertical layered pattern to the underlying substrate present challenges.

[0042] A method for forming a vertically layered pattern of ILC involves depositing an ILC solution onto a periodic substrate surface, such as, for example... Figure 2 As shown in (b), the upper surface of the ILC solution is simultaneously exposed to a vacuum. Coarse-grained simulation 300 is shown in... Figure 3 This is illustrated by the challenges encountered when attempting to form vertically layered ILC structures on the surface of a periodic substrate in a vacuum. Figure 3As shown, due to the hydrophobic nature of vacuum, vertical patterns cannot propagate from the bottom to the top of the ILC film formed in vacuum. This hydrophobicity attracts the alkyl tails of the ILC, causing them to face upwards at the interface. This results in defects / distortions in the pattern of the self-assembled ILC on the substrate surface.

[0043] Filing November 9, 2023, and incorporated herein in its entirety, co-pending U.S. Patent Application Serial No. 18 / 388,240 overcomes the challenges encountered when forming vertically layered ILC structures on a periodic substrate surface by depositing an ILC solution in the presence of a gaseous nonpolar solvent. Since the nonpolar solvent is not attracted to the polar molecules of the ILC (e.g., cationic head groups and anionic groups), exposing the ILC solution to a gaseous nonpolar solvent allows the ILC molecules to orient themselves into a vertically layered structure on the periodic substrate surface. Another method for forming vertically layered patterns of ILC involves providing an ILC film within a feature portion having a neutral bottom surface and hydrophilic sidewalls, such as… Figure 2 As shown in (c), the hydrophilic sidewall surface attracts the polar molecules of ILC, enabling the ILC molecules to orient themselves into a vertically layered structure within the feature region.

[0044] After forming a vertically layered pattern of a self-assembled ILC on a substrate surface, additional challenges must be overcome to successfully transfer the vertically layered pattern to the underlying surface. For example, removing alkyl tails from the ILC film leaves an ionic liquid on the substrate surface. On the other hand, removing cationic head groups from the ILC film leaves alkyl tails, which are also liquid at room temperature. Residual groups within the ILC film (e.g., organic anions) are mobile in both options, so if one or more groups of the self-assembled ILC are removed, the patterning information cannot be preserved. To overcome these challenges, this disclosure provides a novel method for transferring the patterning information of a self-assembled ILC to the underlying substrate.

[0045] like Figure 1A As shown, ionic liquid crystals (ILCs) typically consist of imidazolium-based cations and anions (such as tetrafluoroborate) with long-chain hydrocarbons as alkyl tails. However, other ILCs with other cations and / or anions can be formed. For example, ILCs with cationic head groups based on imidazolium, pyrazolium, pyrrolidineonium, pyridinium, piperidinium, morpholinium, ammonium, phosphonium, sulfonium, or cholineonium can be formed. Anions commonly used to form ILCs include tetrafluoroborate (BF4). - ), chloride ions (Cl) - Acetate (CH3COO) - ), hexafluorophosphate (PF6) - ), trifluoromethylacetate (C3H3F3O2) - ), nitrate (NO3)- ), dicyandiamide (C2HN3) - ), tetracyanoboronate (B(CN)4) - ), trifluoromethanesulfonate (CF3O3S) - ) and bis((trifluoromethyl)sulfonyl)imide ([(CF3SO2)2N] - ).

[0046] In this disclosure, the anions typically used to form ILCs are replaced by metal acid anions to form metal salt ILCs. In addition to preserving the self-assembly properties of ILCs, metal acid anions enable a new method for pattern transfer after the metal salt ILCs self-assemble into desired layered structures (e.g., vertically or horizontally oriented layered structures).

[0047] As is known in the art, a metal anion (or "metal anion") is a complex anion containing a metal attached to several atoms or small groups. Metal anions can contain any metal and a wide variety of ligands. Examples of metals that can be contained within metal anions include transition metals (such as iron (Fe), copper (Cu), cobalt (Co), zinc (Zn), cadmium (Cd), etc.), post-transition metals (such as aluminum (Al), indium (In), tin (Sn), lead (Pb), bismuth (Bi), etc.), and lanthanides (such as cerium (Ce), neodymium (Nd), samarium (Sm), etc.). Examples of ligands that can be contained within metal anions include oxo, halogenated, cyano (CN), thiocyano (SCN), nitrate, sulfonic acid, phosphate, phosphine, trifluoromethanesulfonic acid, sulfo, and carbonate ligands.

[0048] In some embodiments, the metal anion may be a metal chloride anion. Examples of metal chloride anions that can be used to form the metal salt ILC described herein include, but are not limited to, aluminochlorochloroacid anions (e.g., like [AlCl4]). - [Al2Cl7] - [Al3Cl] 10 ] - [Al4Cl] 13 ] - (etc.), ferric chloride anions (such as Cl4Fe), - ), chlorostannate anions (e.g., like [SnCl3]). - [Sn2Cl5] - (etc.), indium chloride anions (e.g., like [InCl6]), 3- [InCl5] 2- [InCl4] - (etc.) and zinc chloride anions (e.g., like [ZnCl4]). 2-[Zn2Cl6] 2- [Zn3Cl8] 2- wait).

[0049] In some embodiments, metal acid salt ILCs can be synthesized by dissolving a stoichiometric amount of a metal halide in an imidazolium-based ionic liquid crystal (ILC) containing a halide anion. The imidazolium-based ILCs used for the synthesis of metal acid salt ILCs typically have the form 1-R1-3-R2-imidazolium, where R1 is an alkyl chain ranging from 8 to 18 carbons in length, and R2 is hydrogen, methyl, ethyl, propyl, butyl, substituted or unsubstituted phenyl, or other hydrocarbon group. In one example, the imidazolium-based ILC may contain 1-dodecyl-3-methylimidazolium. However, ILCs with other cationic head groups can also be used to synthesize the metal acid salt ILCs described herein. A wide variety of metal halides and halide anions can be combined with imidazolium-based ILCs to synthesize metal acid salt ILCs. For example, aluminum chloride (AlCl3) can be dissolved in 1-dodecyl-3-methylimidazolium chloride to form 1-dodecyl-3-methylimidazolium tetrachloroaluminate. The metal acid salt ILC formed in this synthesis contains an imidazolium-based cationic head group covalently bonded to an elongated alkyl tail and a metal anion (e.g., tetrachloroaluminate (AlCl4)). - Other metal acid salts (ILCs) can be formed by dissolving other metal halides in ion-exchange liquid crystal (ILC) halide salts. For example, aluminum trifluoromethanesulfonate (AlOTf3) can be dissolved in 1-dodecyl-3-methylimidazolium trifluoromethanesulfonate to form the [AlOTf4]- anion.

[0050] Similar to other ILCs, metalate ILCs can self-assemble into a solid (crystalline phase) ordered structure at or near room temperature. The polarity difference between the cationic head group and the alkyl tail group promotes the directional self-assembly of metalate ILC molecules by causing the head and tail groups to segregate into an ordered structure. In some embodiments, the head and tail groups can segregate into a layered structure (or “layered structure”) with horizontal or vertical orientation. Metal anions within the metalate ILC segregate to the head layer. Similar to other ILCs, the self-assembly of metalate ILCs and the pitch between layers (i.e., layer pitch) can be controlled by adjusting the chain length of the alkyl tail group, the temperature of the deposition system, and the hydrophobicity of one or more surfaces on which the metalate ILC is deposited. For metalate ILCs based on 1-dodecyl-3-methylimidazolium, the layer pitch can be approximately 3 nm.

[0051] After self-assembly, oxidation processes (e.g., oxygen plasma ashing, ultraviolet (UV) ozone, gas-phase oxidation, or solution-phase oxidation) can be used to oxidize the metalate ILC film and form a more robust pattern that can be transferred to the underlying substrate. The oxidation process converts the organic material within the alkyl tail layer into volatile carbon oxides, which are removed from the substrate surface during the oxidation process. However, the metal anions within the head layer are converted into non-volatile metal oxides, which remain on the substrate surface after oxidation. In doing so, the oxidation process volatilizes the iono-liquid layer but leaves behind a pattern of metal oxides in which the metal anions are concentrated. The metal oxide pattern remaining on the substrate surface is more robust than the iono-liquid film and can therefore be used as a hard mask in subsequent processing steps.

[0052] Figure 4 An embodiment of a method 400 for patterning a semiconductor substrate using the techniques described herein is illustrated. More specifically, method 400 uses directional self-assembly (DSA) of metal-ion carbonate ILCs, followed by oxidation of the self-assembled metal-ion carbonate ILC film to generate a metal oxide pattern that can be transferred to an underlying layer of the semiconductor substrate. It will be appreciated that... Figure 4 The embodiments of method 400 shown are merely exemplary, and additional methods may utilize the techniques described herein. Furthermore, because the described steps are not intended to be exclusive, additional processing steps may be added. Figure 4 Method 400 is shown. Furthermore, the order of the steps is not limited to the order shown in the figure, as different orders may occur and / or various steps may be performed in combination or simultaneously.

[0053] Figure 4 The method 400 shown begins by: generating a first pattern on an underlying layer of a semiconductor substrate (in step 410), wherein the first pattern comprises a plurality of features formed at a first pitch; and depositing an ion-exchange liquid crystal (ILC) solution within each of the plurality of features (in step 420). The ILC solution deposited in step 420 comprises a metal-acid ion-exchange liquid crystal (ILC) having a cationic head group, an alkyl tail group, and a metal anion. The metal-acid ILC deposited within the features self-assembles into a layered structure having alternating head layers and tail layers, wherein metal anions segregate to the head layers. After self-assembly, method 400 exposes the semiconductor substrate to an oxidation process (in step 430) to remove the tail layers from the layered structure and transform the head layers of the layered structure into a metal oxide pattern having a second pitch smaller than the first pitch. Method 400 further includes transferring the metal oxide pattern to an underlying layer of the semiconductor substrate (in step 440).

[0054] Because metal salt ILCs self-assemble into a solid (crystalline phase) ordered structure at or near room temperature, a variety of different methods can be used to deposit an ILC solution within the feature (in step 420). In some embodiments, the ILC solution containing the metal salt ILC can be dispensed at a temperature above the melting point of the ILC. After depositing the ILC solution within the feature (in step 420), the substrate can be cooled to promote the self-assembly of the metal salt ILC and solidify the ILC film. In other embodiments, an ILC solution containing a dilute solution of the metal salt ILC in a solvent can be dispensed and deposited within the feature (in step 420) at or near room temperature. After deposition, the solvent can be evaporated, leaving only the ILC film within the feature. In some cases, the evaporation method may be preferred due to its ability to produce a very thin ILC film. Some ILCs are known to be sensitive to air and / or water. To accommodate such ILCs, in some embodiments, the ILC solution can be dispensed in a controlled atmosphere, in an oxygen-free and anhydrous environment.

[0055] In step 430, the semiconductor substrate can be exposed to a variety of oxidation processes. For example, the semiconductor substrate can be exposed to oxygen plasma ashing, ultraviolet (UV) ozone, gas-phase oxidation, or solution-phase oxidation. Regardless of the oxidation process used, a layered structure is formed within multiple features to: (a) convert the tail layer into volatile carbon oxides, which are then removed from the layered structure during the oxidation process; and (b) convert metal anions in the head layer into non-volatile metal oxides, which remain on the substrate after the oxidation process. The non-volatile metal oxides generated by the oxidation of the metal anions form a metal oxide pattern, which is then transferred to the underlying layer of the semiconductor substrate (in step 440).

[0056] As noted above, metal acid salt ILCs comprise a cationic head group, an alkyl tail group, and a metal anion. In some embodiments, the metal acid salt ILC may comprise a cationic head group based on imidazolium, pyrazolium, pyrrolidineonium, pyridinium, piperidinium, morpholinium, ammonium, phosphonium, sulfonium, or cholineonium, and a metal anion selected from aluminochloroaluminate anion, ferrochlorochloroaluminate anion, stanchlorochlorochloroaluminate anion, indium chlorochloroaluminate anion, and zinc chlorochloroaluminate anion. In one example embodiment, the metal acid salt ILC contained in the ILC solution may be 1-dodecyl-3-methylimidazolium tetrachloroaluminate. In another example embodiment, the metal acid salt ILC contained in the ILC solution may be 1-dodecyl-3-methylimidazolium tetrachloroferrate. Other metal acid salt ILCs not specifically mentioned herein may also be used.

[0057] In some embodiments, metal-acid ILC deposited within multiple features (in step 420) can self-assemble into a vertically layered structure. A variety of methods can be used to form a self-assembled vertically layered structure of metal-acid ILC. For example, co-pending U.S. Patent Application Serial No. 18 / 388,240 describes a method for forming a vertically layered ILC structure on a periodic substrate surface by exposing the upper surface of an ILC solution containing ILC to a gaseous nonpolar solvent. Similar methods can be used herein to form a self-assembled vertically layered structure of metal-acid ILC on a periodic substrate surface. However, the vertically layered structure can also be formed by depositing metal-acid ILC within features (e.g., trenches, holes, etc.) having a neutral bottom surface and hydrophilic sidewall surfaces, such as... Figure 2 (c) and Figure 5 As illustrated in the examples provided, when deposited within such features, metallo-ILCs can self-assemble into a vertically layered structure with alternating head and tail layers, wherein the head layer is oriented toward the hydrophilic sidewall surface of the feature. Because the hydrophilic sidewall surface acts as a guiding surface for molecular self-assembly (by attracting the polar molecules of the metallo-ILC), the metallo-ILCs can self-assemble within the feature with or without the use of nonpolar solvents.

[0058] In some embodiments, method 400 may generate a first pattern (in step 410) by: (a) depositing a neutral layer on an underlying layer of a semiconductor substrate, (b) depositing a hydrophilic layer on the neutral layer, and (c) using a photolithography process to generate the first pattern within the hydrophilic layer, such that the neutral layer is exposed at the bottom of each feature and the hydrophilic layer is exposed on the sidewall surfaces of each feature. In some embodiments, the photolithography process may form a plurality of trenches within the hydrophilic layer to form a pattern of hydrophilic lines on the neutral layer, and an ILC solution may be deposited within the trenches interspersed between each line (in step 420). In other embodiments, the photolithography process may form a pattern of holes extending through the hydrophilic layer to the neutral layer, and an ILC solution may be deposited within the holes formed within the hydrophilic layer (in step 420).

[0059] In step 410, a variety of photolithography processes can be used to create the first pattern. For example, UV (365 nm), deep UV (248 and 193 nm), and extreme UV (EUV, 13.5 nm) photolithography processes can be used. In one example embodiment, a photolithography process including EUV photoresist coating, exposure, baking, and development steps is used to form the first pattern within the hydrophilic layer (in step 410). When the hydrophilic layer is patterned using EUV lithography, the first pitch between the plurality of features can be as small as approximately 28 nm.

[0060] Metalate ILCs deposited within multiple feature areas (in step 420) self-assemble into a vertically layered structure with alternating head and tail layers. For example... Figure 2 (c) As shown and as noted above, the layer pitch (p) between alternating layers of the vertically layered structure is equal to the combined width of the head and tail groups of the self-assembled ILC and typically depends on the chain length of the alkyl tail group. In some embodiments, when a metal acid ILC (having 12 hydrocarbon molecules) based on 1-dodecyl-3-methylimidazolium is used in an ILC solution, the layer pitch (p) between the vertically layered structures can be approximately 3 nm.

[0061] In some embodiments, method 400 controls the layer pitch (p) between alternating layers of a vertically layered structure by controlling the chain length of the alkyl tail. For example, depending on the metal acid salt ILC used in the ILC solution, the chain length of the alkyl tail can range from 8 to 18 hydrocarbon molecules. In some embodiments, method 400 may utilize metal acid salt ILCs with longer alkyl chain lengths to increase the layer pitch, or utilize metal acid salt ILCs with smaller alkyl chain lengths to decrease the layer pitch. By selecting metal acid salt ILCs that self-assemble into ordered structures with pitches smaller than the first pitch between multiple feature portions (e.g., a minimum of about 28 nm) (e.g., about 3 nm) and oxidizing the ordered structures, robust metal oxide patterns are produced. Figure 4 The method 400 shown can be used to provide pitch multiplication for advanced patterning techniques.

[0062] Figure 5 Demonstrated the use of Figure 4 The method 400 shown is an example process flow 500 for patterning a semiconductor substrate using metallate ILC. (See also...) Figure 5 As shown, process flow 500 begins by depositing a neutral layer 510 on an underlying layer 512 disposed on the surface of a semiconductor substrate 514. Neutral layer 510 contains a material having equal affinity for both the cationic head group and the alkyl tail group of the metal acid salt ILC. In one example, neutral layer 510 may contain polytetrafluoroethylene (PTFE). Alternatively, neutral layer 510 may contain other PTFE-like polymers, polymers deposited on surfaces exposed to fluorocarbon or hydrofluorocarbon plasma, graphene, and other film layers having functional groups tuned to provide a neutral surface. After depositing neutral layer 510, a hydrophilic layer 516 is deposited on neutral layer 510. Hydrophilic layer 516 may contain a wide variety of materials having a water contact angle of less than or equal to 60°. For example, hydrophilic layer 516 may contain amorphous carbon (aC), silicon oxycarbide (SiOC), silicon carbide (SiC), amorphous silicon, or silicon dioxide (SiO2). In one instance, hydroxyl-terminated SiO2 was used to form the hydrophilic layer 516.

[0063] A variety of deposition processes can be used to deposit the neutral layer 510 and the hydrophilic layer 516. For example, the neutral layer 510 and the hydrophilic layer 516 can be deposited using one or more deposition techniques, including but not limited to spin coating deposition, chemical vapor deposition (CVD), plasma-enhanced CVD (PECVD), physical vapor deposition (PVD), atomic layer deposition (ALD), and / or other deposition processes.

[0064] After the hydrophilic layer 516 is deposited on the neutral layer 510, a photolithography process is used to form a first pattern within the hydrophilic layer 516. For example, a photolithography process including resist coating, exposure, baking, and development / etching steps can be used to form a plurality of trenches 518 within the hydrophilic layer 516, thereby forming a first pattern of hydrophilic lines 520 on the neutral layer 510 at a first pitch (p1). In some embodiments, when EUV lithography is used to form the first pattern, the first pitch (p1) can be greater than approximately 28 nm.

[0065] like Figure 5 As shown, the trench 518 formed within the hydrophilic layer 516 has a neutral bottom surface and a hydrophilic sidewall surface. In order to enable vertical alignment and layering of the metal acid salt ILC in the next process step, the width (w) of the trench 518 is specifically selected as an integer multiple of the layer pitch (p2) between the alternating layers of the vertical layered structure 522 subsequently formed within the trench 518.

[0066] After the first pattern is formed, process flow 500 deposits an ionomer liquid crystal (ILC) solution containing metallate ILCs on the substrate surface. In some embodiments, spin coating can be used to deposit the ILC solution. A thin layer of metallate ILCs can be obtained by dissolving the metallate ILCs in a suitable solvent and distributing the ILC solution over the substrate surface. The choice of solvent depends on the metallate ILCs contained in the solution. For 1-dodecyl-3-methylimidazolium pentachloroindium, for example, the solvent can include alcohols (e.g., methanol, isopropanol (IPA), etc.), ethers, acetates (e.g., ethyl acetate, acetone, etc.), water, hexane, toluene, acetonitrile, and other organic solvents. The final thickness of the ILC film can be controlled by adjusting the wet film thickness during spin coating and the concentration of metallate ILCs in the solution. By using a dilute solution of metallate ILCs, a very thin ILC film can be obtained once the solvent evaporates. Ideally, the trenches 518 formed during the photolithography process are filled with the ILC solution, while the top of the hydrophilic lines 520 is free of ILCs.

[0067] like Figure 5As shown, the metallate ILC deposited within the trench 518 self-assembles into a vertically layered structure 522 having alternating layers of a head layer 524 and a tail layer 526, wherein the head layer 524 is oriented toward the hydrophilic sidewall surface of the trench 518. In some embodiments, an annealing step may be performed to facilitate the formation of the vertically layered structure 522. Figure 5 As further shown, the layer pitch (p2) between the alternating layers of the vertical layered structure 522 is: (a) equal to the combined width of the head base layer and the tail base layer, and (b) an integer divisor (e.g., 4) of the width (w) of the trench 518. This spacing allows the head base layer and the tail base layer of the metallate ILC to be vertically aligned within the trench 518.

[0068] After the vertically layered structure 522 self-assembles, the semiconductor substrate can be transferred to a plasma tool for oxygen (O2) plasma ashing. For example... Figure 5 As shown, the vertical layered structure 522 is exposed to oxygen plasma 528 to remove the organic components and non-metals of the metal acid salt ILC (e.g., by converting the alkyl tail layer into volatile carbon oxides), while simultaneously converting the metal acid anions in the vertical layered structure 522 into metal oxides. This produces a metal oxide pattern 530 with a second pitch (p2) that is the same as the layer pitch (p2) between the alternating layers of the vertical layered structure 522. The metal oxide pattern 530 can then be used as a hard mask in a subsequent processing step to transfer the metal oxide pattern 530 to the underlying layer 512, thereby forming a pattern 532 in the underlying layer 512.

[0069] Figure 4 Method 400 and shown Figure 5 The process flow 500 shown combines conventional photolithography with directional self-assembly (DSA) and oxidation of metallate ILCs to provide pitch multiplication for advanced patterning techniques. As indicated above and Figure 5 As shown, the width (w) of the features (e.g., trenches, holes, etc.) formed within the first pattern is an integer multiple of the layer pitch (p2, e.g., 3 nm) between the alternating layers of the vertical layer structure 522. When the vertical layer structure 522 is subsequently oxidized, the tail layer 526 is removed from the vertical layer structure 522, and the head layer 524 is transformed into a metal oxide pattern 530 with a second pitch (p2), which is the same as the layer pitch (p2) between the alternating layers of the vertical layer structure 522. This is achieved by utilizing the DSA of metal salt ILCs and oxidizing the metal salt ILCs after self-assembly. Figure 4 and Figure 5 The pattern transfer method and process shown enable advanced patterning at a 3 nm pitch, which is currently impossible with block copolymers or typical ion-soluble liquid crystals in DSA.

[0070] Figure 6 An embodiment of method 600 is illustrated, which uses the techniques described herein to provide pitch multiplication in a patterning transfer process. More specifically, pitch multiplication method 600 uses directional self-assembly (DSA) of metalate ILCs, followed by oxidation of the self-assembled metalate ILC film to generate a metal oxide pattern that can be transferred to an underlying layer of a semiconductor substrate. It will be appreciated that... Figure 6 The embodiment of method 600 shown is merely exemplary, and additional methods may utilize the techniques described herein. Furthermore, because the described steps are not intended to be exclusive, additional processing steps may be added. Figure 6 Method 600 is shown. Furthermore, the order of the steps is not limited to the order shown in the figure, as different orders may occur and / or various steps may be performed in combination or simultaneously.

[0071] Figure 6 The method 600 shown begins by generating a first pattern on a semiconductor substrate (in step 610) and using oriented self-assembly (DSA) of a metal-ion liquid crystal (ILC), followed by oxidation to convert the metal anions contained within the metal-ion ILC into metal oxides, generating a second pattern in each of a plurality of features (in step 620). The first pattern generated in step 610 comprises a plurality of features formed at a first pitch (p1). The second pattern generated in step 620 comprises metal oxides formed at a second pitch (p2), the second pitch being smaller than the first pitch (p1).

[0072] In some embodiments, method 600 may generate a second pattern (in step 620) by: (a) depositing an ion-soluble liquid crystal (ILC) solution comprising a metallate ILC in each of the plurality of features, and (b) exposing a semiconductor substrate to an oxidation process after the metallate ILC self-assembles into an ordered structure. As noted above, the metallate ILC comprises a cationic head group, an alkyl tail group, and a metal anion. When the metallate ILC is deposited in the plurality of features, the metallate ILC self-assembles into a vertically layered structure having alternating head and tail layers, wherein metal anions segregate to the head layer.

[0073] In some embodiments, method 600 may generate a first pattern (in step 610) by: (a) depositing a neutral layer on a semiconductor substrate, (b) depositing a hydrophilic layer on the neutral layer, and (c) using a photolithography process to generate a first pattern within the hydrophilic layer, such that the neutral layer is exposed at the bottom of each feature and the hydrophilic layer is exposed on the sidewall surface of each feature. When the metallate ILC is deposited within multiple features (in step 620), the metallate ILC may self-assemble into a vertically layered structure having alternating head and tail layers, wherein the head layer is oriented toward the sidewall surface of the feature.

[0074] The semiconductor substrate is exposed to an oxidation process to remove the tail layer from the vertically layered structure and convert metal anions into metal oxides. A variety of oxidation processes can be used in method 600. For example, the semiconductor substrate can be exposed to an oxygen plasma ashing process, an ultraviolet (UV) ozone process, a gas-phase oxidation process, or a solution-phase oxidation process. Regardless of the oxidation process used, the vertically layered structure formed within multiple feature areas is oxidized to: (a) convert the tail layer into volatile carbon oxides, which are removed from the vertically layered structure during the oxidation process; and (b) convert the metal anions within the head layer into non-volatile metal oxides, which remain on the substrate after the oxidation process.

[0075] In some embodiments, method 600 may further include controlling the layer pitch between alternating layers of the vertically layered structure by controlling the chain length of the alkyl tail group contained in the metal acid salt ILC. In some embodiments, the width of each feature may be an integer multiple of the layer pitch between alternating layers of the vertically layered structure, and the second pitch (p2) may be equal to that layer pitch.

[0076] This disclosure provides various embodiments of improved process flows and methods for patterning semiconductor substrates using metal-acid ion-liquid crystals (ILCs). The disclosed embodiments improve conventional process flows and pattern transfer methods by utilizing a novel class of ion-liquid crystal (ILC) molecules for directional self-assembly. Specifically, the disclosed embodiments use metal-acid ILCs with metal anions. Metal-acid ILCs allow pattern transfer after the metal-acid ILCs self-assemble and oxidize the ordered structure to remove organic components and convert the metal anions into metal oxide patterns. In addition to providing robust metal oxide patterns that can be transferred to the underlying substrate, the process flows and methods disclosed herein enable ILCs to be used as a pitch multiplication means in advanced patterning techniques. By utilizing the above techniques, the process flows and methods disclosed herein can be used to form metal oxide patterns with sub-5 nm pitches (e.g., approximately 3 nm), which is much smaller than the pitches currently achievable using EUV lithography or block copolymer DSA.

[0077] As used herein, the term "semiconductor substrate" or "substrate" means and includes a base material or structure on which material is formed. It should be understood that a substrate can include a single material, multiple layers of different materials, one or more layers having different material regions or different structural regions, etc. These materials can include semiconductors, insulators, conductors, or combinations thereof. For example, a substrate can be a semiconductor substrate, a base semiconductor layer on a support structure, a metal electrode, or a semiconductor substrate having one or more layers, structures, or regions formed thereon. A substrate can be a conventional silicon substrate or other bulk substrate including layers of semiconducting material. As used herein, the term "bulk substrate" means and includes not only silicon wafers but also silicon-on-insulator ("SOI") substrates (such as silicon-on-sapphire ("SOS") and silicon-on-glass ("SOG") substrates), silicon epitaxial layers on a base semiconductor substrate, and other semiconductor or optoelectronic materials (such as silicon-germanium, germanium, gallium arsenide, gallium nitride, and indium phosphide). Substrates can be doped or undoped.

[0078] The substrate may also include any material portion or structure of the device (particularly semiconductor or other electronic equipment) and may be, for example, a substrate structure (such as a semiconductor substrate) or a layer on or covering a substrate structure. Therefore, the term “substrate” is not intended to be limited to any particular substrate structure, underlying or overlay layer, patterned or unpatterned layer, but is contemplated to include any such layer or substrate structure, and any combination of layers and / or substrate structures.

[0079] It should be noted that references to "one embodiment" or "embodiment" throughout this specification mean that a particular feature, structure, material, or characteristic described in connection with that embodiment is included in at least one embodiment of the invention, but do not imply that they are present in every embodiment. Therefore, the phrases "in one embodiment" or "in an embodiment" appearing in various places throughout this specification do not necessarily refer to the same embodiment of the invention. Furthermore, these particular features, structures, materials, or characteristics can be combined in one or more embodiments in any suitable manner. In other embodiments, various additional layers and / or structures may be included, and / or the features may be omitted.

[0080] Those skilled in the art will recognize that various embodiments can be practiced in the absence of one or more specific details, or by utilizing other alternatives and / or additional methods, materials, or components. In other instances, well-known structures, materials, or operations have not been shown or described in detail to avoid obscuring aspects of the various embodiments of the invention. Similarly, specific figures, materials, and configurations are set forth for illustrative purposes to provide a thorough understanding of the invention. Nevertheless, the invention can be practiced without specific details. Furthermore, it should be understood that the various embodiments shown in the accompanying drawings are illustrative representations and are not necessarily drawn to scale.

[0081] In light of this description, further modifications and alternative embodiments of the methods described herein will be apparent to those skilled in the art. Therefore, it will be appreciated that the described methods are not limited to these exemplary arrangements. It should be understood that the forms of the methods shown and described herein are to be considered exemplary embodiments. Various changes may be made in the implementation. Therefore, although the invention has been described herein with reference to specific embodiments, various modifications and changes may be made without departing from the scope of the invention. Therefore, the specification and drawings are to be regarded in an illustrative rather than restrictive sense, and such modifications are intended to be included within the scope of the invention. Furthermore, any benefits, advantages, or solutions to problems described herein with respect to specific embodiments are not intended to be construed as key, essential, or fundamental features or elements of any or all claims.

Claims

1. A method for patterning a semiconductor substrate, the method comprising: A first pattern is formed on the underlying layer of the semiconductor substrate, the first pattern comprising a plurality of features formed at a first pitch; In each of the plurality of features, an ion-liquid crystal (ILC) solution is deposited, wherein the ILC solution comprises a metal-acid ion-liquid crystal (ILC) having a cationic head group, an alkyl tail group and a metal anion, and wherein the metal-acid ILC deposited in the plurality of features self-assembles into a layered structure having alternating head layers and tail layers, wherein the metal anions segregate to the head layers. The semiconductor substrate is exposed to an oxidation process to remove the tail layers from these layered structures and to transform the head layers of these layered structures into metal oxide patterns with a second pitch smaller than the first pitch. as well as The metal oxide pattern is transferred to the underlying layer of the semiconductor substrate.

2. The method as described in claim 1, wherein, The process of exposing the semiconductor substrate to the oxidation process includes exposing the semiconductor substrate to an oxygen plasma ashing process, an ultraviolet (UV) ozone process, a gas phase oxidation process, or a solution phase oxidation process.

3. The method as described in claim 1, wherein, The process of exposing the semiconductor substrate to the oxidation process oxidizes these layered structures to: These tailings are converted into volatile carbon oxides, which are then removed from these layered structures during the oxidation process. as well as These metal anions within the head base are converted into non-volatile metal oxides, which are then retained after the oxidation process.

4. The method of claim 1, wherein, The cationic head groups within these metal acid ILCs include cationic head groups based on imidazolium, pyrazolium, pyrrolidineonium, pyridinium, piperidinium, morpholinium, ammonium, phosphonium, sulfonium, or cholineonium.

5. The method of claim 1, wherein, Metallic acid salts (ILCs) contain an imidazolium-based cationic head group in the form of 1-R1-3-R2-imidazolium, wherein R1 is an alkyl chain with a chain length ranging from 8 to 18 carbons, and R2 is hydrogen, methyl, ethyl, propyl, butyl, substituted or unsubstituted phenyl, or other hydrocarbon group.

6. The method of claim 5, wherein, These metal acid salts within the ILC contain metal anions including aluminochloroaluminate anion, ferrochlorochloroaluminate anion, stanchlorochloroaluminate anion, indiumchlorochloroaluminate anion, or zincchlorochloroaluminate anion.

7. The method of claim 1, wherein, These metal acid salts (ILCs) include 1-dodecyl-3-methylimidazolium tetrachloroaluminate or 1-dodecyl-3-methylimidazolium tetrachloroferrate.

8. The method of claim 1, wherein, The generation of the first pattern includes: A neutral layer is deposited on the underlying layer of the semiconductor substrate; A hydrophilic layer is deposited on the neutral layer; and The first pattern is created within the hydrophilic layer using a photolithography process, such that the neutral layer is exposed at the bottom of each feature and the hydrophilic layer is exposed on the sidewall surface of each feature.

9. The method of claim 8, wherein, These metallate ILCs deposited within the multiple features self-assemble into a vertically layered structure with alternating head and tail layers, wherein the head layers of these vertically layered structures are oriented toward the sidewall surfaces of these features.

10. The method of claim 9, further comprising controlling the layer pitch between the alternating layers of the vertically layered structure by controlling the chain length of the alkyl tail groups.

11. The method of claim 9, wherein, The width of each feature is equal to an integer multiple of the pitch between these alternating layers of these vertically layered structures, and the second pitch is equal to the pitch between the layers.

12. The method of claim 9, wherein, The use of photolithography to produce the first pattern includes: The photolithography process is used to form multiple trenches within the hydrophilic layer to create a pattern of hydrophilic lines on the neutral layer; and The ILC solution is deposited in each of the multiple trenches.

13. The method of claim 9, wherein, The use of photolithography to produce the first pattern includes: The photolithography process is used to form a pattern of holes extending through the hydrophilic layer to the neutral layer; and The ILC solution is deposited in each of these pores.

14. A pitch doubling method, the method comprising: A first pattern is formed on a semiconductor substrate, the first pattern comprising a plurality of features formed at a first pitch; as well as Directional self-assembly (DSA) of metal-ion liquid crystals (ILCs) is used, followed by oxidation to convert the metal anions contained in these metal-ion ILCs into metal oxides, thereby generating a second pattern in each of the plurality of features, the second pattern containing these metal oxides formed at a second pitch smaller than the first pitch.

15. The pitch doubling method as described in claim 14, wherein, The generation of the second pattern includes: An ionomer liquid crystal (ILC) solution comprising these metal acid salt ILCs is deposited within each of the plurality of feature portions, wherein the metal acid salt ILCs comprise cationic head groups, alkyl tail groups, and the metal acid anions, and wherein the metal acid salt ILCs deposited within the plurality of feature portions self-assemble into a layered structure having alternating head and tail layers, wherein the metal acid anions segregate to the head layers; and The semiconductor substrate is exposed to an oxidation process to remove the tail layers from these layered structures and convert the metal anions into metal oxides.

16. The pitch doubling method as described in claim 15, wherein, The process of exposing the semiconductor substrate to the oxidation process includes exposing the semiconductor substrate to an oxygen plasma ashing process, an ultraviolet (UV) ozone process, a gas phase oxidation process, or a solution phase oxidation process.

17. The pitch doubling method as described in claim 15, wherein, The process of exposing the semiconductor substrate to the oxidation process oxidizes these layered structures to: These tailings are converted into volatile carbon oxides, which are then removed from these layered structures during the oxidation process. as well as These metal anions within the head base are converted into non-volatile metal oxides, which are then retained after the oxidation process.

18. The pitch doubling method as described in claim 15, wherein, The generation of the first pattern includes: A neutral layer is deposited on the semiconductor substrate; A hydrophilic layer is deposited on the neutral layer; and The first pattern is created within the hydrophilic layer using a photolithography process, such that the neutral layer is exposed at the bottom of each feature and the hydrophilic layer is exposed on the sidewall surface of each feature.

19. The pitch doubling method as described in claim 18, wherein, These metallate ILCs deposited within multiple features self-assemble into a vertically layered structure with alternating head and tail layers, wherein the head layers of this vertically layered structure are oriented toward the sidewall surfaces of these features.

20. The pitch multiplication method of claim 19, further comprising controlling the layer pitch between the alternating layers of the vertically layered structure by controlling the chain length of the alkyl tail groups.

21. The pitch doubling method as described in claim 19, wherein, The width of each feature is equal to an integer multiple of the pitch between these alternating layers of these vertically layered structures, and the second pitch is equal to the pitch between the layers.

Citation Information

Patent Citations

  • Methods for forming vertically layered ionic liquid crystal (ILC) structures on a semiconductor substrate