A method and apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composites

By using an organic solvent swelling and peracetic acid in-situ generation system to degrade epoxy resin at ambient pressure and low temperature, the complexity of equipment and high energy consumption in high-temperature and high-pressure carbon fiber recycling have been solved, achieving efficient recycling and low-damage treatment of high-strength carbon fibers.

CN122325839APending Publication Date: 2026-07-03TIANMUSHAN LABORATORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610680730.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-18
Publication Date
2026-07-03

AI Technical Summary

Technical Problem

Existing chemical recycling technologies for carbon fiber reinforced composites rely on high-temperature and high-pressure environments, resulting in complex equipment, high energy consumption, and safety risks. Furthermore, they suffer significant fiber strength loss, making it difficult to achieve efficient and low-damage recycling.

Method used

An organic solvent swelling pretreatment combined with an in-situ peracetic acid generation system was used to degrade the epoxy resin matrix under normal pressure and low temperature conditions. The resin matrix was then dissolved using DMF and the cross-linking network was broken by peracetic acid, thus achieving high-quality recycling of carbon fibers.

Benefits of technology

The system achieves efficient recycling of carbon fiber under mild conditions, with a fiber strength retention rate of over 90%. The equipment is simple, reduces energy consumption and safety risks, and meets green and environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122325839A_ABST
    Figure CN122325839A_ABST
Patent Text Reader

Abstract

This invention discloses a method and apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite materials. The method utilizes an organic solvent to pretreat the composite material sample through solvent swelling, followed by the use of an in-situ peracetic acid generation system to degrade the epoxy resin matrix, thereby achieving complete recycling of the carbon fibers. The recycling method of this invention operates at a reaction temperature not exceeding 160°C and under normal pressure throughout the entire recycling process, effectively avoiding surface damage and mechanical property impairment to the fibers caused by high-temperature pyrolysis (typically above 500°C) or high-pressure reactions (e.g., supercritical hydrolysis). The carbon fibers recovered using this method retain over 90% of the original fiber tensile strength, exhibiting extremely high reuse value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of material recycling technology, and in particular to a method and apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite materials. Background Technology

[0002] Fiber-reinforced composite materials are widely used in wind power, aerospace, and automotive industries due to their excellent properties such as lightweight, high specific strength, and flexible design. With the exponential growth in demand for composite materials, the "retirement wave" of their waste is approaching. However, current disposal of solid waste from composite materials still relies mainly on landfill and incineration, and these extensive methods have caused serious environmental and resource problems. Landfilling leads to long-term material retention, consuming large amounts of land resources and posing a potential risk of soil and groundwater pollution; while incineration not only releases large amounts of carbon dioxide but also produces toxic substances such as carbon monoxide, volatile organic compounds, black carbon, and even dioxins, exacerbating global warming and threatening ecosystems and human health. Meanwhile, the high energy consumption and high cost of carbon fiber make its waste problem particularly prominent; large amounts of high-value-added carbon fiber materials are directly discarded along with retired products, resulting in huge resource waste. Therefore, establishing an efficient carbon fiber recycling and reuse system is urgently needed.

[0003] Currently, recycling technologies for carbon fiber reinforced composites are mainly divided into three categories: mechanical recycling, pyrolysis recycling, and chemical recycling. Mechanical recycling processes waste composites into fillable short fibers or powder through cutting, crushing, and sieving. This method involves simple equipment and low energy consumption, but the fiber length is typically between 0.05 and 10 mm, resulting in limited reuse value and low economic benefits. Pyrolysis recycling decomposes resin at high temperatures of 450 to 800°C under an inert atmosphere. It has been demonstrated in aerospace and automotive waste treatment, but high-temperature pyrolysis often leads to carbonization of the fiber surface and significant strength loss, with strength only reaching 4% to 85% of the original fiber. Furthermore, it often requires subsequent surface treatment, resulting in high overall energy consumption. In contrast, chemical recycling decomposes resin using solvents or catalysts at relatively lower temperatures, such as 20 to 400°C and pressures below 25 MPa, simultaneously recovering high-quality carbon fibers and matrix monomers. The fiber strength retention rate obtained through this method is typically higher than 85%, and the surface is clean and free of carbon deposition. It also has relatively low energy consumption, making it an effective way to obtain high-quality recycled fibers.

[0004] Currently, chemical recycling technology is transitioning from the laboratory to engineering. Adherent Technologies in the US has built a pilot plant with a single batch capacity of 45 kg, using wet chemical recycling to obtain carbon fiber and oil and gas byproducts. Aditya Birla in India focuses on developing easily recyclable dynamic covalent epoxy resins, whose chemical bonds can break and reform during heating or chemical reactions, allowing the company to establish a low-temperature chemical recycling pilot line. Universities in Japan and Europe are focusing on developing subcritical / supercritical water and enzymatic hydrolysis systems to achieve the recycling of semi-long carbon fibers. Domestic universities, such as Hefei University of Technology, are also exploring small-scale applications of supercritical interfacial depolymerization reactors, with temperatures ranging from 200 to 400℃ and pressures from 3 to 20 MPa. Harbin Institute of Technology uses a strong acid-Lewis acid synergistic system composed of nitric acid and Lewis acid to degrade epoxy resin through its strong corrosiveness and strong oxidizing properties to recover carbon fibers. Northwestern Polytechnical University uses organic alcohols such as ethylene glycol and glycerol as solvents and alkali metal hydroxides such as sodium hydroxide and potassium hydroxide as catalysts to degrade thermosetting resin matrices through catalytic alcoholysis under moderate temperature conditions of 160 to 220°C, thereby achieving the recycling of carbon fibers.

[0005] As we can see from the above introduction, current mainstream chemical recycling technologies still rely on strong acid / alkali systems and high temperature and high pressure environments, which have problems such as complex equipment, high energy consumption and safety risks. Summary of the Invention

[0006] To address the aforementioned technical problems, this invention provides a method and apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite materials. This method uses a specific chemical solvent to precisely break the resin's cross-linking network under mild conditions (normal pressure, low temperature), thereby achieving high-quality, low-damage recycling of carbon fibers, offering significant environmental and economic advantages.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] A method for recycling amine-cured epoxy resin carbon fiber reinforced composites involves pretreating the composite sample with an organic solvent to induce solvent swelling, followed by using an in-situ peracetic acid generation system to degrade the epoxy resin matrix, thereby achieving complete recycling of the carbon fiber.

[0009] The method specifically includes the following steps:

[0010] S1: Immerse the amine-cured epoxy resin carbon fiber reinforced composite material in an organic solvent;

[0011] S2: Stir and heat the mixture obtained in step S1 to cause the amine-cured epoxy resin carbon fiber reinforced composite material to swell;

[0012] S3: After cooling the product of step S2 to room temperature, take out the swollen amine-cured epoxy resin carbon fiber reinforced composite material and dry it.

[0013] S4: Immerse the dried amine-cured epoxy resin carbon fiber reinforced composite material obtained in step S3 into an in-situ reaction system, wherein the in-situ reaction system is a mixed solution of acetic acid and hydrogen peroxide;

[0014] S5: Stir and heat the mixture obtained in step S4; in this step, peracetic acid will effectively break the cross-linking network of epoxy resin, causing it to dissolve and separate from the carbon fiber.

[0015] S6: Perform solid-liquid separation on the product obtained in step S5 and collect the solid product;

[0016] S7: Wash and dry the solid product obtained in step S6.

[0017] In step S1, the organic solvent is a polar solvent containing strongly polar functional groups (C=O, S=O, etc.), containing electron-donating atoms, and lacking active hydrogen. Preferably, the dielectric constant of the organic solvent is 20~40, and the dipole moment is 3.5~5.0D.

[0018] More preferably, the organic solvent in step S1 is one or a mixture of several of N,N-dimethylformamide, dimethyl sulfoxide, N,N-dimethylacetamide, N-methylpyrrolidone or γ-valerolactone.

[0019] In step S2, the heating temperature is 100℃~160℃ and the heating time is 2~10 hours.

[0020] In step S4, the volume ratio of hydrogen peroxide to sample mass is 2 mL:1 g to 10 mL:1 g, and the volume ratio of acetic acid to hydrogen peroxide is 3:1 to 20:1, ensuring that the mixed solution completely submerges the sample.

[0021] In step S5, the heating temperature is 50℃~100℃ and the heating time is 1~24 hours.

[0022] In step S2, the stirring is either magnetic stirring or mechanical stirring.

[0023] In steps S2 and S5, the condenser reflux device is activated simultaneously with the heating process. The heating device is a conventional heating device.

[0024] In step S7, the drying temperature is 80℃~120℃ and the drying time is more than 12 hours.

[0025] An apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite materials includes a reactor shell, a support, and several layers of trays; the support and several layers of trays are all located inside the reactor shell.

[0026] The brackets are multiple, and multiple support structures for supporting the tray are provided on the brackets; the tray is fixed in the corresponding support structures of the multiple brackets.

[0027] The tray has multiple hollow structures and multiple circumferentially distributed opening structures, with the support located in the opening structures.

[0028] The support structure is a groove structure, and the opening structure corresponds to and cooperates with the bracket, so that the tray can move along the axial direction of the bracket; when the tray moves to the groove structure position of the bracket, the non-opening part of the tray is rotated to engage with the groove structure, thereby fixing the tray on the bracket.

[0029] The beneficial effects of this invention are as follows:

[0030] (1) The recycling method of the present invention operates at a reaction temperature not exceeding 160°C and under normal pressure throughout the entire recycling process, effectively avoiding damage to the fiber surface and mechanical properties caused by high-temperature pyrolysis (usually temperatures above 500°C) or high-pressure reactions (e.g., supercritical hydrolysis). The carbon fibers recycled by this method retain more than 90% of the original fiber tensile strength, and have extremely high reuse value.

[0031] (2) Since a high temperature and high pressure environment is not required, the present invention has low requirements for reaction equipment and does not require expensive pressure-resistant or special alloy equipment, which greatly reduces equipment investment and operation difficulty, and provides convenience for pilot-scale amplification and industrial production.

[0032] (3) This invention achieves efficient and precise degradation of amine-cured epoxy resins. On the one hand, DMF preferentially penetrates and swells the epoxy resin, greatly promoting the diffusion and contact of subsequent peracetic acid and accelerating the resin degradation process. Especially for the recycling of large-sized material components, the solvent swelling method is preferentially used to open the solution penetration channels, which plays a key role in the deep penetration and uniform reaction of subsequent peracetic acid. On the other hand, the peracetic acid generated in situ by acetic acid and hydrogen peroxide can break the resin crosslinking network while causing minimal damage to the carbon fibers. Through this method, the resin removal rate can reach over 95%, and the recovered fiber surface is clean with very little residue.

[0033] (4) The reaction system of this method uses hydrogen peroxide and acetic acid as raw materials. No toxic gases are generated during the reaction process. All the chemicals used are biodegradable. It is a green and environmentally friendly recycling technology that meets the requirements of sustainable development. Attached Figure Description

[0034] Figure 1 This is an overall schematic diagram of the apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to the present invention.

[0035] Figure 2 This is a photograph of the swollen sample to be recovered in Example 1.

[0036] Figure 3 This is a photograph of the recycled carbon fiber obtained in Example 1.

[0037] Figure 4 This is a scanning electron microscope image of the recycled carbon fiber obtained in Example 1.

[0038] The reference numerals in the attached figures are as follows: 100 - outer shell of the reactor; 200 - support; 210 - groove structure; 300 - tray; 310 - hollow structure; 320 - opening structure. Detailed Implementation

[0039] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0040] This invention provides a method for chemically degrading and recovering amine-cured epoxy resin-based carbon fiber reinforced composite materials under mild conditions. The core of this method lies in using an organic solvent to pre-treat the composite material sample through solvent swelling, followed by using an in-situ peracetic acid generation system to degrade the epoxy resin matrix, thereby achieving complete recovery of the carbon fibers.

[0041] Preferably, the organic solvent is a polar solvent containing strongly polar functional groups (C=O, S=O, etc.), containing electron-donating atoms, and without active hydrogen.

[0042] The specific steps are as follows:

[0043] S1: Weigh 1~10g of amine-cured epoxy resin-based carbon fiber reinforced composite material sample and place it in a corrosion-resistant reaction vessel; then pour in organic solvent to ensure that the solution completely submerges the sample.

[0044] S2: Place the reaction vessel on a heated magnetic stirrer and turn on the stirrer (carefully control the speed to prevent the rotor from hitting the glass vessel walls and entangled with the recycled carbon fibers), and raise the temperature of the reaction system to the set temperature of 100℃~160℃. At this temperature, turn on the reflux condenser and maintain the reaction temperature for 2~10 hours. During this period, the DMF solution penetrates into the epoxy resin matrix, increasing the porosity and cracks inside the sample, causing the sample to expand.

[0045] S3: Cool the reaction vessel to room temperature, remove the sample, rinse it, and dry it for later use.

[0046] S4: Add the dried sample to acetic acid and 30% hydrogen peroxide solution to form an in-situ peracetic acid generation system, wherein the volume ratio of hydrogen peroxide to sample mass is 2mL:1g~10mL:1g, and the volume ratio of acetic acid to hydrogen peroxide solution is 3:1~20:1.

[0047] S5: Start stirring and raise the reaction system temperature to the set temperature of 50℃~100℃. At this temperature, turn on the reflux condenser and maintain the reaction temperature for 1~24 hours. During this period, peracetic acid will effectively break the cross-linking network of the epoxy resin, causing it to dissolve and separate from the carbon fibers. After the reaction is complete, the original composite material sample can be observed to disintegrate, yielding a solution and clustered carbon fibers.

[0048] S6: Use a vacuum filtration device to separate the reaction mixture into solid and liquid components and collect the solid product (i.e., the recovered carbon fiber).

[0049] S7: Wash the carbon fiber multiple times with sufficient deionized water until the filtrate is neutral to remove residual degradation products and attached solutions on the fiber surface; transfer the washed carbon fiber to a vacuum drying oven and dry it at 80℃~120℃ for more than 12 hours to completely remove moisture and obtain dry recycled carbon fiber, thus completing the recycling of amine-cured epoxy resin-based carbon fiber composite material.

[0050] S8: To quantitatively evaluate the resin removal effect, the following procedures can be performed:

[0051] S81: Weigh the dried carbon fiber and estimate the resin removal rate by measuring the mass change before and after recycling and the theoretical mass fraction of carbon fiber in the original composite material.

[0052] S82: Accurately weigh approximately 50 mg of the dried carbon fiber sample and perform thermogravimetric analysis. Under nitrogen protection, heat the sample from 30°C to 800°C at a heating rate of 10°C / min to completely decompose the residual resin on the fiber surface, obtaining a mass-temperature curve. By combining the mass change of the sample before and after drying, the resin removal rate can be accurately calculated.

[0053] See Figure 1 The present invention also provides an apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite material, which includes a reactor shell 100, a support 200 and several layers of trays 300; the support 200 and the several layers of trays 300 are all located inside the reactor shell 100; there are multiple supports 200, and multiple support structures for supporting the trays 300 are provided on the supports 200; the trays 300 are fixed in the corresponding support structures of the multiple supports 200.

[0054] The tray-support structure of the device of the present invention includes multiple trays 300, which mainly have the following functions: 1) to achieve effective separation of the rotor and the sample, and avoid carbon fiber entanglement or crossing; 2) to ensure that the carbon fiber and composite material samples are completely immersed in the liquid medium and prevent them from being exposed above the liquid surface; 3) to separate and position the materials to be processed, increase their contact area with the solution, and thereby improve mass transfer and reaction efficiency.

[0055] Preferably, multiple support structures are provided on the bracket 200 along the axial direction of the bracket 200, with corresponding support structures on all brackets 200, thereby allowing the bracket 200 to accommodate multiple trays 300. The support structure can be a protrusion extending from the bracket 200, or it can be... Figure 1 The groove structure 210 is shown. See also... Figure 1 In this embodiment, there are three brackets 200, and each bracket 200 is provided with multiple groove structures 210 of the same height.

[0056] Preferred, see Figure 1 The tray 300 has multiple perforated structures 310, and openings 320 are evenly distributed circumferentially on the tray 300. These openings 320 are designed to engage with the support 200, allowing the tray 300 to move axially along the support 200. When the tray 300 moves to the corresponding position of the grooved structure 210, its non-opening portion engages with the grooved structure 210 by relative rotation, thus fixing the tray 300 to the support 200. In other words, the support structure of the support 200 engages with the non-opening structure of the tray 300. This allows for quick and stable assembly between the tray 300 and the support 200 via the openings 320, and the number of tray layers can be flexibly stacked according to experimental needs, achieving adjustable device height and good adaptability.

[0057] Preferably, the outer shell 100 of the reactor is made of glass; the support 200 and the tray 300 are made of polytetrafluoroethylene.

[0058] Example 1:

[0059] This embodiment provides a method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials, the specific steps of which are as follows:

[0060] (1) Weigh 2.5 g of amine-cured epoxy resin-based carbon fiber reinforced composite material (prepreg cured) as the sample to be recycled, and put it into the container. Figure 1 In the device shown;

[0061] (2) Add 50 mL of DMF to the apparatus, ensuring the solution completely submerges the sample. Perform a reflux stirring reaction at 160°C. In this embodiment, magnetic stirring is used; specifically, a magnetic stirring rotor is placed inside. Install a reflux condenser at the opening of the apparatus. Place the reaction apparatus on the magnetic stirrer, turn on the stirring, and simultaneously start heating to raise the temperature of the reaction system to 160°C. Turn on the cooling water to perform a constant-temperature reaction. The reaction continues for 3 hours, and the following can be observed: Figure 2 The composite material shown exhibits obvious delamination;

[0062] (3) Cool the reaction vessel to room temperature, remove the sample, rinse and dry it for later use. Add acetic acid and 30% hydrogen peroxide solution to the dried sample to form an in-situ peracetic acid generation system. The volume of hydrogen peroxide is 20 mL, and the volume ratio of acetic acid to hydrogen peroxide solution is 5:1.

[0063] (4) Turn on the stirrer and raise the temperature of the reaction system to 80°C. At this temperature, turn on the reflux condenser and maintain the temperature for 5 hours. During this period, peracetic acid will effectively break the crosslinking network of the epoxy resin, causing it to dissolve and separate from the carbon fibers. After the reaction is complete, the original composite material sample can be observed to disintegrate, yielding a solution and clustered carbon fibers;

[0064] (5) After the reaction is completed, the reaction mixture is separated into solid and liquid by using a Buchner funnel and a vacuum filtration device to collect the solid product (i.e. the recovered carbon fiber).

[0065] (6) Wash the carbon fiber repeatedly with sufficient deionized water until the filtrate is neutral; transfer the washed carbon fiber to a vacuum drying oven and dry it at 100°C for 12 hours to obtain the following result. Figure 3 The dried recycled carbon fiber shown is weighed.

[0066] Figure 4 This is a scanning electron microscope image of the recycled carbon fiber obtained in Example 1. From... Figure 4 It can be seen that the surface of the recycled fibers is clean and the morphology is not damaged. Thermogravimetric analysis and calculation show that the resin removal rate reaches 98%; the tensile strength of 20 carbon fibers was measured, and the average tensile strength is 91% of the original fiber strength.

[0067] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention. The above embodiments are provided only for the purpose of describing the present invention and are not intended to limit the present invention. Parts not described in detail in this specification are well-known in the art and are not intended to limit the scope of the present invention. The scope of the present invention is defined by the appended claims. All equivalent substitutions and modifications made without departing from the spirit and principle of the present invention should be covered within the scope of the present invention.

Claims

1. A method of recycling an amine cured epoxy resin carbon fiber reinforced composite material, characterized by, The composite material sample was pretreated with an organic solvent to induce solvent swelling, and then the epoxy resin matrix was degraded using an in-situ peracetic acid generation system, thereby achieving the recycling of carbon fiber.

2. The method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 1, characterized in that, The method specifically includes the following steps: S1: Immerse the amine-cured epoxy resin carbon fiber reinforced composite material in an organic solvent; S2: Stir and heat the mixture obtained in step S1 to cause the amine-cured epoxy resin carbon fiber reinforced composite material to swell; S3: After cooling the product of step S2 to room temperature, take out the swollen amine-cured epoxy resin carbon fiber reinforced composite material and dry it. S4: Immerse the dried amine-cured epoxy resin carbon fiber reinforced composite material obtained in step S3 into an in-situ reaction system, wherein the in-situ reaction system is a mixed solution of acetic acid and hydrogen peroxide; S5: Stir and heat the mixture obtained in step S4; in this step, peracetic acid will effectively break the cross-linking network of epoxy resin, causing it to dissolve and separate from the carbon fiber. S6: Perform solid-liquid separation on the product obtained in step S5 and collect the solid product; S7: Wash and dry the solid product obtained in step S6.

3. The method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 2, characterized in that, The organic solvent in step S1 is a polar solvent containing strongly polar functional groups, electron-donating atoms, and no active hydrogen.

4. The method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 3, characterized in that, The organic solvent in step S1 is one or a mixture of several of N,N-dimethylformamide, dimethyl sulfoxide, N,N-dimethylacetamide, N-methylpyrrolidone or γ-valerolactone.

5. The method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 2, characterized in that, The temperature of the heat treatment in step S2 is 100℃~160℃, and the heat treatment time is 2~10 hours.

6. The method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 2, characterized in that, In step S4, the volume ratio of hydrogen peroxide to sample mass is 2 mL:1 g to 10 mL:1 g, and the volume ratio of acetic acid to hydrogen peroxide is 3:1 to 20:1, ensuring that the mixed solution completely submerges the sample.

7. The method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 2, characterized in that, The temperature of the heat treatment in step S5 is 50℃~100℃, and the heat treatment time is 1~24 hours; The drying temperature in step S7 is 80℃~120℃, and the drying time is more than 12 hours.

8. The method for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 2, characterized in that, The stirring in step S2 is magnetic stirring or mechanical stirring; the condenser reflux device is turned on simultaneously with the heating treatment in steps S2 and S5.

9. An apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite materials, characterized in that, The device includes a reactor shell, a support frame, and several layers of trays; the support frame and several layers of trays are all located inside the reactor shell. The brackets are multiple, and multiple support structures for supporting the tray are provided on the brackets; the tray is fixed in the support structures of the brackets.

10. The apparatus for recycling amine-cured epoxy resin carbon fiber reinforced composite materials according to claim 9, characterized in that, The tray has multiple hollow structures and multiple circumferentially distributed opening structures, with the support located in the opening structures; The support structure is a groove structure, and the opening structure corresponds to and cooperates with the bracket, so that the tray can move along the axial direction of the bracket; when the tray moves to the groove structure position of the bracket, the non-opening part of the tray engages with the groove structure, thereby fixing the tray to the bracket.