A heat-resistant anticorrosive coating containing a modified terpene resin and a method for preparing the same

By modifying terpene resin through a combination of grafting and crosslinking modification, and optimizing the coating preparation process, a multi-component synergistic protection system was constructed. This solved the problems of poor heat resistance and uneven coating of terpene resin, and achieved high-efficiency heat resistance, corrosion resistance and weather resistance of the coating.

CN122326080APending Publication Date: 2026-07-03LUODING XINGGUANG CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610682985.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-18
Publication Date
2026-07-03

AI Technical Summary

Technical Problem

Existing terpene resins have poor heat resistance, lack anti-corrosion functional groups, have limited modification effects, poor synergy of coating components, and unoptimized preparation processes, resulting in uneven coating performance and insufficient protective effect.

Method used

Terpene resin was modified by combining grafting and crosslinking modification to construct a multi-component synergistic protection system. The preparation process was optimized, and a dense protective layer was formed by the rational combination of modified terpene resin with epoxy resin, anti-corrosion filler, and weather-resistant additives. This improved the heat resistance, corrosion resistance, and weather resistance of the coating. The components were uniformly dispersed by stepwise dispersion and precise control of stirring speed and temperature.

Benefits of technology

It significantly improves the heat resistance, corrosion resistance and weather resistance of the coating, improves the adhesion and hardness of the coating, forms a stable physical protective layer, and achieves an overall performance improvement of the coating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of coating technology, specifically to a heat-resistant and corrosion-resistant coating containing modified terpene resin and its preparation method. By weight, it comprises the following components: 15-40 parts modified terpene resin, 30-50 parts epoxy resin, 10-20 parts silica, 5-12 parts zinc phosphate, 0.5-1.5 parts antioxidant 1010, 0.3-1.2 parts ultraviolet absorber 1130, 12-22 parts curing agent, 20-30 parts solvent, 0.2-0.6 parts leveling agent, and 0.1-0.5 parts defoamer. The modified terpene resin is obtained by grafting and crosslinking modification of natural terpene resin. The leveling agent is a polyether-modified polyorganosiloxane, and the defoamer is tributyl phosphate. The heat-resistant and corrosion-resistant coating containing modified terpene resin and its preparation method provided by this invention innovate from multiple dimensions, including resin modification, component design, and process optimization, effectively solving many technical defects of existing technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, specifically to a heat-resistant and corrosion-resistant coating containing modified terpene resin and its preparation method. Background Technology

[0002] Heat-resistant and corrosion-resistant coatings are key materials in the field of industrial protection and are widely used to protect various substrates affected by high temperature and corrosive media. Their heat resistance, corrosion resistance and comprehensive mechanical properties directly determine the protective effect and service life.

[0003] Terpene resins are often incorporated into coating systems due to their readily available raw materials and good compatibility. However, natural terpene resins have poor heat resistance and lack anti-corrosion functional groups, making direct use unsuitable for high-temperature and corrosive environments. Existing technologies for modifying terpene resins mostly employ single grafting or single crosslinking methods, resulting in limited modification effects and an inability to effectively introduce functional groups, thus failing to fundamentally improve their heat resistance and corrosion resistance.

[0004] Meanwhile, the existing heat-resistant and corrosion-resistant coatings mostly use a single filler combination, which makes it difficult to form a dense protective layer. Corrosive media can easily penetrate, resulting in insufficient long-term protection. Although some coatings take into account the improvement of individual performance, they ignore the synergistic effect between components, which leads to an imbalance between the coating's weather resistance, hydrophobicity and mechanical properties, resulting in problems such as poor adhesion, insufficient hardness and rapid weather resistance decay.

[0005] Furthermore, existing coating preparation processes lack targeted optimization, and problems such as uneven filler dispersion and insufficient component mixing are common, further affecting the structural stability and overall performance of the coating. Currently, there is no coating solution that combines dual modification of terpene resin with synergistic design of multiple components and optimized preparation processes, making it difficult to meet the high requirements of industrial scenarios for comprehensive protective performance. Therefore, there is an urgent need to develop a heat-resistant and corrosion-resistant coating containing modified terpene resin with excellent comprehensive performance and its preparation method. Summary of the Invention

[0006] The primary objective of this invention is to provide a heat-resistant and corrosion-resistant coating containing modified terpene resin and a method for preparing the same.

[0007] A further objective of this invention is to provide a heat-resistant and corrosion-resistant coating containing modified terpene resin, comprising, by weight, the following components: 15-40 parts modified terpene resin, 30-50 parts epoxy resin, 10-20 parts silica, 5-12 parts zinc phosphate, 0.5-1.5 parts antioxidant 1010, 0.3-1.2 parts ultraviolet absorber 1130, 12-22 parts curing agent, 20-30 parts solvent, 0.2-0.6 parts leveling agent, and 0.1-0.5 parts defoamer; wherein the modified terpene resin is obtained by grafting modification and crosslinking modification of natural terpene resin, the leveling agent is polyether-modified polyorganosiloxane, and the defoamer is tributyl phosphate.

[0008] Preferably, by weight, it also contains 0-12 parts of quaternary ammonium salt modified montmorillonite and 0-3 parts of fluorine-containing additive FC1402.

[0009] Preferably, the curing agent is a phenolic amine curing agent, or a mixture of phenolic amine and isooctyl ether amine in a 3:2 ratio, or a mixture of phenolic amine, isooctyl ether amine and butanol in a 3:2:1 ratio; the solvent is toluene, or a mixture of toluene and xylene in a 1:1 ratio, or a mixture of toluene and ethylene glycol ethyl ether in a 2:1 ratio, or a mixture of toluene, xylene and ethylene glycol ethyl ether in a 2:1:1 ratio.

[0010] A method for preparing a heat-resistant and corrosion-resistant coating containing modified terpene resin includes the following steps:

[0011] Step 1: Add the modified terpene resin and epoxy resin to the stirred tank, add half of the total amount of solvent, heat to 60-80℃ and stir to obtain the resin mixture.

[0012] Step 2: Add silica and zinc phosphate to the resin mixture and stir. Then add antioxidant 1010, UV absorber 1130, leveling agent, and defoamer and continue stirring. If the coating contains quaternary ammonium salt modified montmorillonite and fluorine-containing additive FC1402, add quaternary ammonium salt modified montmorillonite and fluorine-containing additive FC1402 in sequence after stirring silica and zinc phosphate and stir them separately.

[0013] Step 3: Cool down to 40℃, add curing agent and stir, then add the remaining half of the solvent to adjust the viscosity of the system to 200-300 mPa·s, continue stirring and filter through a 200-mesh filter to obtain a heat-resistant and corrosion-resistant coating.

[0014] Preferably, the preparation of the modified terpene resin includes the following steps: using 100 parts by weight of natural terpene resin as a basis, the natural terpene resin is mixed with solvent, modifier and initiator, and then subjected to dissolution, reaction and neutralization treatment in sequence. After distillation under reduced pressure at a distillation temperature of 90°C, a distillation pressure of 0.06 MPa and a distillation time of 1.5 hours, the mixture is dried and then pulverized to 90 mesh.

[0015] Preferably, based on 100 parts by weight of natural terpene resin, the solvent content is 50-150 parts by weight, the modifier content is 10-40 parts by weight, the initiator content is 0.5-5 parts by weight, and the neutralizer content is 1-8 parts by weight; the modifier is maleic anhydride, or a mixture of maleic anhydride and hydroxypropyl acrylate in a 3:2 ratio, or a mixture of maleic anhydride, hydroxypropyl acrylate, and styrene in a 3:2:2 ratio, or a combination of any of the above mixtures with a fluorinated monomer; the initiator is benzoyl peroxide, or a mixture of benzoyl peroxide and azobisisobutyronitrile in a 1:1 ratio; the neutralizer is triethanolamine, or a mixture of triethanolamine and diethanolamine in a 2:1 ratio.

[0016] Preferably, the temperature of the dissolution process is 80-120℃, the dissolution holding time is 10-20 minutes, and the dissolution stirring speed is 300-600 r / min; the temperature of the reaction process is 130-180℃, the reaction time is 2-6 hours, and the reaction stirring speed is 400-800 r / min; the system is cooled to 60-80℃ before neutralization, and the stirring time after neutralization is 30 minutes.

[0017] Preferably, the stirring speed in step one is 500-800 r / min, and the stirring time is 30-50 minutes.

[0018] Preferably, in step two, the stirring speed after adding silica and zinc phosphate is 800-1100 r / min, and the stirring time is 60-90 minutes; after adding antioxidant 1010, ultraviolet absorber 1130, leveling agent, and defoamer, the stirring speed is 600 r / min, and the stirring time is 30 minutes; if quaternary ammonium salt modified montmorillonite or fluorine-containing additive FC1402 is added, the stirring time is 20-40 minutes after each component is added.

[0019] Preferably, in step three, the stirring speed after adding the curing agent is 400 r / min, and the stirring time is 20-30 minutes; after adjusting the viscosity of the system, the stirring time is continued for 10-15 minutes.

[0020] Compared with the prior art, the beneficial effects of the present invention are:

[0021] 1. The heat-resistant and corrosion-resistant coating containing modified terpene resin and its preparation method provided by the present invention innovate from multiple dimensions such as resin modification, component design and process optimization, and effectively solve many technical defects of the prior art.

[0022] 2. This invention uses a combination of grafting modification and crosslinking modification to modify terpene resin, which can effectively introduce heat-resistant and corrosion-resistant functional groups, optimize the molecular structure of terpene resin, and significantly improve its heat resistance and chemical stability, laying a core foundation for the heat resistance and corrosion resistance of coatings.

[0023] 3. This invention constructs a multi-component synergistic protection system by rationally combining modified terpene resin with epoxy resin, anti-corrosion filler, and weather-resistant additives. The components complement each other and enhance each other's effects. This not only forms a dense physical protective layer to block the penetration of corrosive media, but also improves the chemical stability of the coating through the synergistic effect of functional groups. At the same time, it endows the coating with excellent weather resistance and hydrophobicity, achieving simultaneous improvement in heat resistance, corrosion resistance, and weather resistance.

[0024] 4. This invention optimizes the preparation process parameters based on the characteristics of the coating system. By stepwise dispersion and precise control of stirring speed and temperature, it ensures uniform dispersion of each component, effectively improving the mechanical properties of the coating such as adhesion and hardness, and solving the problems of high brittleness and unstable structure of existing coatings. Detailed Implementation

[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] Preparation of modified terpene resin:

[0027] The modified terpene resins used in each embodiment were prepared by a combination of grafting modification and crosslinking modification. The amount of natural terpene resin used was 100 parts. The specific preparation parameters were gradually optimized with each embodiment to form a performance gradient. The modified terpene resins prepared in the corresponding embodiment were used in the subsequent coating preparation to ensure the continuity and technical progress between each embodiment.

[0028] The vacuum distillation process is uniformly controlled as follows: distillation temperature 90℃, distillation pressure 0.06MPa, distillation time 1.5 hours, and after drying, the product is pulverized to 90 mesh.

[0029] Example 1:

[0030] Preparation parameters of modified terpene resin: solvent is toluene, amount 50 parts; modifier is maleic anhydride, amount 10 parts; initiator is benzoyl peroxide, amount 0.5 parts; neutralizer is triethanolamine, amount 1 part; dissolution temperature is 80℃, dissolution holding time is 10 minutes, stirring speed is 300 r / min; reaction temperature is 130℃, reaction time is 2 hours, reaction stirring speed is 400 r / min; cooling temperature is 60℃, stirring time after neutralization is 30 minutes.

[0031] Coating raw material proportions by weight: 15 parts modified terpene resin, 30 parts epoxy resin, 10 parts silica, 5 parts zinc phosphate, 0.5 parts antioxidant 1010, 0.3 parts ultraviolet absorber 1130, 12 parts curing agent, 20 parts solvent, 0.2 parts leveling agent, and 0.1 parts defoamer.

[0032] The curing agent is a phenolic amine curing agent, the solvent is a 1:1 mixture of toluene and xylene, the leveling agent is a polyether-modified polysiloxane, and the defoamer is tributyl phosphate.

[0033] Coating preparation method:

[0034] The first step involves adding the modified terpene resin and epoxy resin to a stirred tank, adding 10 parts of solvent, heating to 60°C, stirring for 30 minutes at a speed of 500 r / min, to obtain a resin mixture.

[0035] The second step is to add silica and zinc phosphate to the resin mixture, adjust the speed to 800 r / min, stir for 60 minutes, then add antioxidant 1010, ultraviolet absorber 1130, leveling agent and defoamer, and continue stirring for 30 minutes at 600 r / min.

[0036] The third step is to cool the temperature to 40°C, add the curing agent, stir for 20 minutes at a speed of 400 r / min, then add 10 parts of the remaining solvent, adjust the viscosity of the system to 200 mPa·s, continue stirring for 10 minutes, filter with a 200-mesh filter to remove impurities, and obtain a heat-resistant and corrosion-resistant coating.

[0037] Example 2:

[0038] Preparation parameters of modified terpene resin: Optimized based on Example 1. The solvent is a mixture of toluene and ethylene glycol ethyl ether in a 2:1 ratio, used in an amount of 80 parts; the modifier is a mixture of maleic anhydride and hydroxypropyl acrylate in a 3:2 ratio, used in a total amount of 18 parts; the initiator is a mixture of benzoyl peroxide and azobisisobutyl cyanide in a 1:1 ratio, used in an amount of 1.5 parts; the neutralizing agent is a mixture of triethanolamine and diethanolamine in a 2:1 ratio, used in an amount of 3 parts; the dissolution temperature is 90℃, the dissolution holding time is 15 minutes, and the stirring speed is 400 r / min; the reaction temperature is 145℃, the reaction time is 3 hours, and the reaction stirring speed is 500 r / min; the cooling temperature is 70℃, and the stirring time after neutralization is 30 minutes.

[0039] Coating raw material proportions by weight: 22 parts modified terpene resin, 35 parts epoxy resin, 12 parts silica, 6 parts zinc phosphate, 0.8 parts antioxidant 1010, 0.5 parts ultraviolet absorber 1130, 15 parts curing agent, 22 parts solvent, 0.3 parts leveling agent, and 0.2 parts defoamer.

[0040] The types of curing agent, solvent, leveling agent, and defoamer are the same as in Example 1.

[0041] Coating preparation method: Based on Example 1, the process parameters were adjusted. In the first step, the stirring temperature was increased to 70°C, the stirring time was extended to 40 minutes, and the stirring speed was 600 r / min. In the second step, the stirring speed was increased to 900 r / min and the stirring time was extended to 70 minutes. In the third step, after the curing agent was added, the stirring time was extended to 25 minutes. The remaining steps were the same as in Example 1.

[0042] Example 3:

[0043] Preparation parameters of modified terpene resin: Based on Example 2, further optimization was performed. The solvent was a mixture of toluene, xylene, and ethylene glycol ethyl ether in a ratio of 2:1:1, with a dosage of 110 parts. The modifier was a mixture of maleic anhydride, hydroxypropyl acrylate, and styrene in a ratio of 3:2:2, with a total dosage of 25 parts. The initiator dosage was 2.5 parts. The neutralizer dosage was 5 parts. The dissolution temperature was 100℃, the dissolution holding time was 15 minutes, and the stirring speed was 500 r / min. The reaction temperature was 160℃, the reaction time was 4 hours, and the reaction stirring speed was 600 r / min. The cooling temperature was 75℃, and the stirring time after neutralization was 30 minutes.

[0044] Coating raw material proportions by weight: 30 parts modified terpene resin, 40 parts epoxy resin, 15 parts silica, 8 parts zinc phosphate, 1.0 parts antioxidant, 0.7 parts ultraviolet absorber, 7 parts quaternary ammonium salt modified montmorillonite, 18 parts curing agent, 25 parts solvent, 0.4 parts leveling agent, and 0.3 parts defoamer.

[0045] The curing agent is a mixture of phenolic amine and isooctyl ether amine in a 3:2 ratio, and the other additives are the same as in Example 1.

[0046] Coating preparation method: Based on Example 2, in the second step, after adding silica and zinc phosphate, stir for 30 minutes, then add quaternary ammonium salt modified montmorillonite and continue stirring for 40 minutes; the stirring speed in the first step is increased to 700 r / min, and the stirring speed in the second step is increased to 1000 r / min. The remaining process parameters are the same as in Example 2.

[0047] Example 4:

[0048] Preparation parameters of modified terpene resin: optimized based on Example 3, with solvent amount of 130 parts; modifier amount of 32 parts, and 0.8 parts of fluorinated monomer added for modification; initiator amount of 3.5 parts; neutralizer amount of 6 parts; dissolution temperature of 110℃, dissolution holding time of 20 minutes, stirring speed of 550 r / min; reaction temperature of 170℃, reaction time of 5 hours, stirring speed of 700 r / min; cooling temperature of 80℃, and stirring time after neutralization of 30 minutes.

[0049] Coating raw material proportions by weight: 35 parts modified terpene resin, 45 parts epoxy resin, 18 parts silica, 10 parts zinc phosphate, 1.2 parts antioxidant 1010, 0.9 parts ultraviolet absorber 1130, 9 parts quaternary ammonium salt modified montmorillonite, 22 parts fluorine-containing additive FC140, 20 parts curing agent, 28 parts solvent, 0.5 parts leveling agent, and 0.4 parts defoamer.

[0050] The other types of additives are the same as in the previous examples.

[0051] Coating preparation method: Based on Example 3, in the second step, after adding quaternary ammonium salt modified montmorillonite, stir for 30 minutes, then add fluorine-containing additive FC1402 and continue stirring for 30 minutes; in the third step, adjust the viscosity of the system to 250 mPa·s, and at the same time extend the stirring time to 15 minutes. The remaining process parameters are the same as in Example 3.

[0052] Example 5:

[0053] Preparation parameters of modified terpene resin: Further optimized based on Example 4, with solvent amount of 150 parts; modifier amount of 40 parts, fluorinated monomer amount increased to 1.2 parts; initiator amount of 5 parts; neutralizer amount of 8 parts; dissolution temperature of 120℃, dissolution holding time of 20 minutes, stirring speed of 600 r / min; reaction temperature of 180℃, reaction time of 6 hours, stirring speed of 800 r / min; cooling temperature of 80℃, stirring time after neutralization of 30 minutes.

[0054] Coating raw material proportions by weight: 40 parts modified terpene resin, 50 parts epoxy resin, 20 parts silica, 12 parts zinc phosphate, 1.5 parts antioxidant 1010, 1.2 parts ultraviolet absorber 1130, 12 parts quaternary ammonium salt modified montmorillonite, 3 parts fluorine-containing additive FC1402, 22 parts curing agent, 30 parts solvent, 0.6 parts leveling agent, and 0.5 parts defoamer.

[0055] The curing agent is a mixture of phenolic amine, isooctyl ether amine and butanol in a ratio of 3:2:1, and the other additives are the same as those in the previous examples.

[0056] Coating preparation method: Based on Example 4, the stirring temperature in the first step is increased to 80°C, the stirring time is extended to 50 minutes, and the stirring speed is 800 r / min; in the second step, the stirring speed is increased to 1100 r / min, and the stirring time is extended to 90 minutes; in the third step, after the curing agent is added, the stirring time is extended to 30 minutes, and the viscosity of the system is adjusted to 300 mPa·s. The remaining steps are the same as in Example 4.

[0057] Example 6:

[0058] Preparation parameters of modified terpene resin: The modifier compound system of Example 3 was used, that is, maleic anhydride, hydroxypropyl acrylate and styrene were mixed in a ratio of 3:2:2, with a dosage of 22 parts; solvent dosage of 100 parts; initiator dosage of 2.0 parts; neutralizer dosage of 4 parts; fluorinated monomer dosage of 0.6 parts; dissolution temperature of 95℃, dissolution holding time of 15 minutes, stirring speed of 450 r / min; reaction temperature of 150℃, reaction time of 3.5 hours, stirring speed of 550 r / min; cooling temperature of 75℃, stirring time after neutralization of 30 minutes.

[0059] Coating raw material proportions by weight: 28 parts modified terpene resin, 38 parts epoxy resin, 16 parts silica, 7 parts zinc phosphate, 0.9 parts antioxidant 1010, 0.6 parts ultraviolet absorber 1130, 8 parts quaternary ammonium salt modified montmorillonite, 1.5 parts fluorine-containing additive FC1402, 16 parts curing agent, 24 parts solvent, 0.35 parts leveling agent, and 0.25 parts defoamer.

[0060] The curing agent is a mixture of phenolic amine and isooctyl ether amine in a 3:2 ratio, and the other additives are the same as those in the previous examples.

[0061] Coating preparation method: Integrating the process advantages of Examples 2 to 4, the first step is to stir at a temperature of 75°C for 45 minutes and a speed of 650 r / min; the second step is to stir at a speed of 950 r / min for 80 minutes, adding fillers and additives in the following order: silica, zinc phosphate, quaternary ammonium salt modified montmorillonite, fluorine-containing additives, and other auxiliary additives, stirring for 20 minutes after each addition; the third step is to adjust the system viscosity to 280 mPa·s and stir for 12 minutes, with the remaining steps being the same as in the previous examples.

[0062] Comparative Example 1:

[0063] Instead of using modified terpene resin, 15 parts of natural terpene resin were used, and the remaining raw material ratios and preparation processes were the same as in Example 1.

[0064] This comparative example corresponds to the existing technology of directly using natural terpene resin to prepare coatings. However, the terpene resin is not modified, resulting in poor heat resistance and corrosion resistance. In stark contrast to the modified terpene resin of this invention, its performance is far inferior to all embodiments of this invention.

[0065] Comparative Example 2:

[0066] In the preparation of the modified terpene resin, no modifier was added. 100 parts of natural terpene resin were mixed with 50 parts of toluene, 0.5 parts of benzoyl peroxide, and 1 part of triethanolamine for reaction. The remaining raw material ratios and preparation process were the same as in Example 1.

[0067] This comparative example corresponds to the existing single crosslinking modification scheme without the addition of grafting modifier, which cannot effectively introduce corrosion-resistant and heat-resistant functional groups, resulting in poor modification effect. In contrast to the dual modification method of the present invention, its performance is inferior to that of Example 1.

[0068] Comparative Example 3:

[0069] Zinc phosphate was not added, and the proportions of the remaining raw materials and the preparation process were the same as in Example 1.

[0070] This comparative example corresponds to a solution in the prior art where the coating system lacks anti-corrosion fillers, thus failing to form effective anti-corrosion protection. In contrast to the synergistic anti-corrosion system of the present invention, its anti-corrosion performance is far inferior to all embodiments of the present invention.

[0071] Comparative Example 4:

[0072] The amount of modified terpene resin was reduced to 5 parts, while the proportions of the remaining raw materials and the preparation process were the same as in Example 1.

[0073] This comparative example corresponds to the existing technology where the amount of modified terpene resin is insufficient, failing to fully utilize its heat resistance and corrosion resistance. Compared with the reasonable range of modified terpene resin dosage in this invention, its performance is inferior to that of Example 1.

[0074] Comparative Example 5:

[0075] In the preparation method, the stirring speed in the second step is reduced to 300 r / min, the stirring time is shortened to 20 minutes, and the remaining raw material ratios and preparation processes are the same as in Example 1.

[0076] This comparative example corresponds to an existing technology with an unreasonable preparation process and uneven filler dispersion. Compared with the optimized preparation process of this invention, its coating quality and performance are inferior to those of Example 1.

[0077] Comparative Example 6

[0078] Antioxidant 1010 and ultraviolet absorber 1130 were not added, and the remaining raw material ratios and preparation processes were the same as in Example 1.

[0079] This comparative example corresponds to existing technologies that lack weather-resistant additives and have poor weather resistance. In contrast to the weather-resistant protection system of the present invention, its weather resistance is far inferior to all embodiments of the present invention.

[0080] Comparative Example 7:

[0081] The single grafted modified terpene resin disclosed in the prior art was used, and maleic anhydride was used for graft modification. The preparation parameters were the same as in Example 1. Quaternary ammonium salt modified montmorillonite and fluorine-containing additives were not added to the coating formulation. The remaining raw material ratios and preparation processes were the same as in Example 1.

[0082] This comparative example directly corresponds to existing technologies with single modification methods and poor component synergy. It directly contrasts with the dual modification and composite protection system of this invention, highlighting the inventiveness of this invention. Its overall performance is far inferior to all embodiments of this invention.

[0083] Comparative Example 8:

[0084] The existing single crosslinked modified terpene resin is simply mixed with the existing anti-corrosion coating components. That is, the modified terpene resin is modified by single crosslinking, and the coating formulation is made up of a single anti-corrosion additive disclosed in the prior art. The proportions of the remaining raw materials and the preparation process are the same as in Example 1.

[0085] This comparative example corresponds to the combination scheme of the prior art, which does not form a synergistic protection system. In contrast to the dual modification and multiple synergistic system of the present invention, its performance is inferior to that of Example 1, further proving that the present invention is different from any combination of the prior art and has outstanding inventiveness.

[0086] Performance testing and results analysis:

[0087] Testing standards:

[0088] (1) The heat resistance test refers to GB / T1735-2009. The high temperature aging test chamber is used. The coating is placed at 300℃ for 72 hours. The appearance change of the coating is observed and the weight loss rate of the coating is tested.

[0089] (2) Corrosion resistance test: Refer to ASTM B117 standard, conduct neutral salt spray test, use 5% NaCl solution, temperature 35℃, test the time when the coating shows rust and blistering; Refer to GB / T1763-1989, conduct chemical corrosion resistance test, immerse in 5% hydrochloric acid and 5% sodium hydroxide solution respectively, place at room temperature for 72 hours, observe the changes in the appearance of the coating.

[0090] (3) Mechanical properties were tested according to GB / T1720-1979, using the pull-off method to test the coating adhesion; according to GB / T1730-2007, the coating pencil hardness was tested; according to GB / T1732-1993, the coating impact resistance was tested.

[0091] (4) Weather resistance test refers to GB / T1865-2009, using a xenon lamp aging test chamber, aging for 5000 hours, testing the coating gloss retention rate and color difference ΔE, and evaluating the anti-chalking grade;

[0092] (5) The hydrophobicity test was conducted using a contact angle measuring instrument to test the water contact angle of the coating.

[0093] The test results are shown in Table 1 below:

[0094] Test sample Heat resistance weight loss rate Heat resistance appearance Salt spray test corrosion time Chemically resistant appearance Adhesion MPa Pencil hardness Gloss retention Color difference ΔE Water contact angle Example 1 3.2 No bubbling or cracking 1500 No peeling or discoloration 7.5 2H 85 3.2 95 Example 2 2.8 No bubbling or cracking 1800 No peeling or discoloration 8.0 2H 88 2.8 98 Example 3 2.3 No bubbling or cracking 2200 No peeling or discoloration 8.5 3H 90 2.5 102 Example 4 1.9 No bubbling or cracking 2600 No peeling or discoloration 9.0 3H 92 2.1 110 Example 5 1.5 No bubbling or cracking 3000 No peeling or discoloration 9.5 4H 94 1.8 115 Example 6 2.5 No bubbling or cracking 2000 No peeling or discoloration 8.2 3H 89 2.6 105 Comparative Example 1 8.7 Severe bubbling and cracking 600 Partial peeling and slight discoloration 5.2 H 62 6.8 78 Comparative Example 2 7.9 Slight cracking of bubbles 750 Slight peeling and slight discoloration 5.8 H 68 6.2 82 Comparative Example 3 6.5 No bubbling, slight cracking 800 Partial peeling and obvious discoloration 6.0 H 70 5.9 85 Comparative Example 4 7.2 Slight cracking of bubbles 850 Slight peeling and slight discoloration 6.3 H 72 5.7 88 Comparative Example 5 7.5 Bubbling and cracking 700 Partial peeling and slight discoloration 5.5 H 65 6.5 80 Comparative Example 6 6.8 No bubbling or cracking 900 No peeling or obvious discoloration 6.8 2H 58 7.2 90 Comparative Example 7 6.2 Slight bubbling without cracking 1000 Slight peeling and slight discoloration 6.5 2H 75 5.5 89 Comparative Example 8 6.0 Slight bubbling without cracking 1100 Slight peeling and slight discoloration 6.7 2H 78 5.3 92

[0095] The results are analyzed as follows:

[0096] In terms of heat resistance, the weight loss rate of each embodiment was controlled below 3.2%. Furthermore, with optimization of the modification process, improvement of the modifier compounding, and adjustment of process parameters, the weight loss rate gradually decreased, with Example 5 exhibiting the lowest weight loss rate at only 1.5. All embodiments showed no blistering or cracking after being kept at 300℃ for 72 hours, demonstrating excellent high-temperature stability. In contrast, the weight loss rates of the comparative examples were all above 6.0, with Comparative Example 1 showing the highest weight loss rate at 8.7. Most comparative examples also exhibited blistering and cracking, especially Comparative Example 1 (which did not use modified terpene resin) and Comparative Example 2 (which only used single crosslinking modification), which showed extremely poor heat resistance. This difference fully demonstrates that the grafting and crosslinking dual modification method used in this invention can effectively improve the heat resistance of terpene resin. Combined with the optimized preparation process, the coating forms a stable three-dimensional network structure, thereby significantly enhancing the high-temperature stability of the coating and solving the technical defects of poor heat resistance of terpene resin and easy damage to the coating at high temperatures in the prior art.

[0097] In terms of corrosion resistance, the salt spray corrosion time of all embodiments exceeded 1500 hours, with Example 5 exhibiting the longest corrosion time at 3000 hours. Furthermore, all embodiments showed no peeling or discoloration in the chemical corrosion resistance test, demonstrating significant corrosion resistance. The salt spray corrosion time of all comparative examples was below 1100 hours, with Comparative Example 1 showing a corrosion time of only 600 hours. Some comparative examples showed peeling and discoloration. Comparative Example 3, without zinc phosphate, exhibited the worst corrosion resistance, with a salt spray corrosion time of only 800 hours, and also showed significant discoloration and partial peeling. This indicates that the synergistic anti-corrosion system constructed in this invention, consisting of modified terpene resin, zinc phosphate, and quaternary ammonium salt-modified montmorillonite, can form a dense protective layer, effectively blocking the penetration of corrosive media and significantly improving the coating's corrosion resistance and long-term protective capability. This overcomes the limitations of existing technologies with single anti-corrosion systems and poor protective effects.

[0098] In terms of mechanical properties, the adhesion of all embodiments was above 7.5 MPa, and the pencil hardness was 2H or higher. Embodiment 5 exhibited an adhesion of 9.5 MPa and a pencil hardness of 4H, demonstrating excellent adhesion and hardness, meeting the requirements of industrial applications. The adhesion of all comparative examples was below 6.8 MPa, and the pencil hardness was mostly H, indicating poor mechanical properties. Comparative Example 1, in particular, had an adhesion of only 5.2 MPa and a pencil hardness of only H, failing to meet the mechanical requirements for practical protection. This result demonstrates that the present invention, by optimizing the synergistic ratio of modified terpene resin and epoxy resin and adjusting the preparation process parameters to ensure uniform dispersion of all components, effectively improves the mechanical properties of the coating and addresses the problems of high brittleness and poor adhesion in existing technologies.

[0099] Regarding weather resistance and hydrophobic properties, the gloss retention rate of all embodiments was above 85%, the color difference ΔE was below 3.2%, and the water contact angle was above 95°. Example 5 achieved a gloss retention rate of 94%, a color difference ΔE of only 1.8%, and a water contact angle of 115°, demonstrating outstanding weather resistance and hydrophobicity. The gloss retention rates of all comparative examples were below 78%, the color difference ΔE was above 5.3%, and the water contact angle was below 92°. Comparative example 6, which did not contain antioxidants or UV absorbers, had a gloss retention rate of only 58% and a color difference ΔE of 7.2%, exhibiting extremely poor weather resistance. This indicates that the antioxidants and UV absorbers added in this invention, along with the fluorinated additives and fluorinated modified terpene resin, form a synergistic effect, not only improving the weather resistance of the coating but also endowing it with excellent hydrophobic properties, further enhancing the protective effect and service life of the coating.

[0100] Comparative examples and comparative examples demonstrate that the dual modification method, component synergistic system, and optimized preparation process of the present invention are key to improving the overall performance of the coating. Comparative Examples 7 and 8 correspond to typical and combined solutions of existing technologies, respectively, and their overall performance is far inferior to that of the embodiments of the present invention, further proving that the technical solution of the present invention differs from existing technologies and arbitrary combinations thereof, exhibiting outstanding inventiveness. Furthermore, the logical progression of performance among the embodiments also proves the rationality and scientific validity of the raw material ratios and process parameter adjustments of the present invention, enabling adaptation to different performance requirements, expanding the application scope of the present invention, and enhancing its practicality.

[0101] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention.

Claims

1. A heat-resistant and corrosion-resistant coating containing modified terpene resin, characterized in that, The product, by weight, comprises the following components: 15-40 parts modified terpene resin, 30-50 parts epoxy resin, 10-20 parts silica, 5-12 parts zinc phosphate, 0.5-1.5 parts antioxidant 1010, 0.3-1.2 parts ultraviolet absorber 1130, 12-22 parts curing agent, 20-30 parts solvent, 0.2-0.6 parts leveling agent, and 0.1-0.5 parts defoamer; wherein the modified terpene resin is obtained by grafting modification and crosslinking modification of natural terpene resin, the leveling agent is polyether-modified polyorganosiloxane, and the defoamer is tributyl phosphate.

2. The heat-resistant and corrosion-resistant coating containing modified terpene resin according to claim 1, characterized in that, By weight, it also contains 0-12 parts of quaternary ammonium salt modified montmorillonite and 0-3 parts of fluorine-containing additive FC1402.

3. The heat-resistant and corrosion-resistant coating containing modified terpene resin according to claim 1 or 2, characterized in that, The curing agent is a phenolic amine curing agent, or a mixture of phenolic amine and isooctyl ether amine in a 3:2 ratio, or a mixture of phenolic amine, isooctyl ether amine and butanol in a 3:2:1 ratio; the solvent is toluene, or a mixture of toluene and xylene in a 1:1 ratio, or a mixture of toluene and ethylene glycol ethyl ether in a 2:1 ratio, or a mixture of toluene, xylene and ethylene glycol ethyl ether in a 2:1:1 ratio.

4. A method for preparing a heat-resistant and corrosion-resistant coating containing modified terpene resin as described in any one of claims 1-3, characterized in that, Includes the following steps: Step 1: Add the modified terpene resin and epoxy resin to the stirred tank, add half of the total amount of solvent, heat to 60-80℃ and stir to obtain the resin mixture. Step 2: Add silica and zinc phosphate to the resin mixture and stir. Then add antioxidant 1010, UV absorber 1130, leveling agent, and defoamer and continue stirring. If the coating contains quaternary ammonium salt modified montmorillonite and fluorine-containing additive FC1402, add quaternary ammonium salt modified montmorillonite and fluorine-containing additive FC1402 in sequence after stirring silica and zinc phosphate and stir them separately. Step 3: Cool down to 40℃, add curing agent and stir, then add the remaining half of the solvent to adjust the viscosity of the system to 200-300 mPa·s, continue stirring and filter through a 200-mesh filter to obtain a heat-resistant and corrosion-resistant coating.

5. The preparation method according to claim 4, characterized in that, The preparation of the modified terpene resin includes the following steps: using 100 parts by weight of natural terpene resin as a basis, the natural terpene resin is mixed with solvent, modifier and initiator, and then subjected to dissolution, reaction and neutralization treatment in sequence. After distillation under reduced pressure at a distillation temperature of 90℃, a distillation pressure of 0.06MPa and a distillation time of 1.5 hours, the mixture is dried and then pulverized to 90 mesh.

6. The preparation method according to claim 5, characterized in that, Based on 100 parts by weight of natural terpene resin, the solvent dosage is 50-150 parts by weight, the modifier dosage is 10-40 parts by weight, the initiator dosage is 0.5-5 parts by weight, and the neutralizer dosage is 1-8 parts by weight; the modifier is maleic anhydride, or a mixture of maleic anhydride and hydroxypropyl acrylate in a 3:2 ratio, or a mixture of maleic anhydride, hydroxypropyl acrylate, and styrene in a 3:2:2 ratio, or a combination of any of the above mixtures with a fluorinated monomer; the initiator is benzoyl peroxide, or a mixture of benzoyl peroxide and azobisisobutyronitrile in a 1:1 ratio; the neutralizer is triethanolamine, or a mixture of triethanolamine and diethanolamine in a 2:1 ratio.

7. The preparation method according to claim 5, characterized in that, The dissolution process is carried out at a temperature of 80-120℃, with a holding time of 10-20 minutes and a stirring speed of 300-600 r / min. The reaction process is carried out at a temperature of 130-180℃, with a reaction time of 2-6 hours and a stirring speed of 400-800 r / min. Before neutralization, the system is cooled to 60-80℃, and after neutralization, the stirring time is 30 minutes.

8. The preparation method according to claim 4, characterized in that, The stirring speed in step one is 500-800 r / min, and the stirring time is 30-50 minutes.

9. The preparation method according to claim 4, characterized in that, In step two, after adding silica and zinc phosphate, the stirring speed is 800-1100 r / min and the stirring time is 60-90 minutes; after adding antioxidant 1010, ultraviolet absorber 1130, leveling agent and defoamer, the stirring speed is 600 r / min and the stirring time is 30 minutes; if quaternary ammonium salt modified montmorillonite or fluorine-containing additive FC1402 is added, stir for 20-40 minutes after each component is added.

10. The preparation method according to claim 4, characterized in that, In step three, after adding the curing agent, the stirring speed is 400 r / min and the stirring time is 20-30 minutes; after adjusting the viscosity of the system, the stirring time is continued for 10-15 minutes.