Carbon fiber reinforced antistatic flame-retardant polysulfide composite paper and preparation method thereof

By using a sandwich structure design, combining a surface layer and a middle core layer, the contradiction between flame retardancy, mechanical strength and functionality of aramid paper is resolved, achieving a synergistic improvement in antistatic and electromagnetic shielding performance, and expanding its application in the field of high-end composite materials.

CN122358545APending Publication Date: 2026-07-10SHANGHAI ARAMID VALLEY NEW MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610748774.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-02-09
Filing Date
2026-05-28
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

Existing aramid paper suffers from limitations in functionalization, including limited functionality, difficulty in achieving a balance between flame retardancy, mechanical strength, and electromagnetic shielding performance, and the tendency of traditional modification methods to cause electromagnetic wave reflection pollution, failing to meet the application requirements of modern electronic devices.

Method used

The product adopts a sandwich structure design. The outer layer is composed of aramid nanofibers and modified LDH-MXene composite flame retardant, while the middle core layer is formed by interwoven aramid short fibers and carbon fibers to form a robust skeleton. Through carbon fiber reinforcement and MXene to build a conductive network, the antistatic and electromagnetic shielding performance is synergistically improved.

Benefits of technology

It achieves a synergistic improvement in antistatic and electromagnetic shielding performance, stabilizes material properties, expands its application in the field of high-end composite materials, and maintains the high temperature resistance and flame retardant properties of aramid fiber.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a carbon fiber reinforced antistatic and flame-retardant aramid fiber composite paper and its preparation method. The antistatic and flame-retardant aramid fiber composite paper adopts a sandwich structure. The top and bottom layers are made of a slurry composed of aramid fiber nanofibers, LDH / MXene composite functional materials, and a dispersant, imparting electromagnetic wave absorption properties and surface flame-retardant protection. The middle core layer is made of a slurry composed of aramid fiber chopped strands, aramid precipitated strands, carbon fiber chopped strands, and a dispersant, forming a supporting framework and constructing a bulk conductive network to ensure the mechanical strength and overall conductivity of the composite paper. Through multi-channel gradient papermaking and programmed temperature-controlled hot pressing processes, interlayer bonding and structural stability are achieved, enabling the material to maintain the inherent high-temperature resistance and flame-retardant properties of aramid fiber while also possessing synergistic properties of antistatic properties, electromagnetic shielding absorption, and high mechanical strength. This effectively solves the technical challenge of traditional materials struggling to achieve multiple functions simultaneously.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-performance specialty paper technology and relates to a flame-retardant aramid composite paper. Specifically, it relates to an aramid composite paper with a "sandwich" structure that combines high conductivity, excellent mechanical strength, efficient electromagnetic shielding performance, and durable antistatic and flame-retardant properties. It is particularly suitable for fields with stringent requirements for electromagnetic compatibility and lightweighting, such as aerospace, high-end electronic equipment, flexible circuits, and special protection. Background Technology

[0002] Aryl sulfone fiber has excellent high temperature resistance, inherent flame retardancy and chemical corrosion resistance. Aryl sulfone paper made from it has been widely used in high-end industrial fields such as high temperature filtration, electrical insulation and aerospace. However, existing aramid paper and its modified products have significant defects in achieving functionalization: (1) Traditional aramid paper has a single function and is difficult to meet the requirements of modern industry for the comprehensive performance of materials. Adding functional components through blending can improve its specific properties to a certain extent, such as conductivity, but often at the cost of sacrificing its inherent mechanical strength, electrical insulation or flame retardancy, resulting in a decline in the comprehensive performance of the material. (2) Existing electromagnetic shielding aramid materials mostly adopt the modification method of blending with metal fibers. This technical route mainly relies on the electromagnetic wave reflection mechanism to achieve the shielding function, which is prone to secondary electromagnetic wave reflection pollution and cannot meet the urgent needs of modern electronic equipment for absorption electromagnetic shielding materials.

[0003] Therefore, there is an urgent need in this field for a new type of aramid paper that can combine multiple properties such as antistatic properties, electromagnetic shielding, mechanical strength, and lightweight, and whose performance is stable and durable. Summary of the Invention

[0004] In order to overcome the above-mentioned technical problems, the present invention aims to: (1) provide an aramid paper with antistatic properties, electromagnetic shielding, mechanical strength and lightweight properties; (2) provide a method for preparing an aramid paper with antistatic properties, electromagnetic shielding, mechanical strength and lightweight properties.

[0005] The inventive concept of this invention is to effectively solve the contradiction between flame retardancy, mechanical strength and functionality in traditional aramid paper. By designing a composite structure with clear functional zones, the invention achieves an organic combination of "surface flame retardancy and electromagnetic protection" and "core conductive reinforcement and mechanical support". While maintaining the inherent high temperature resistance and flame retardant properties of the material, it endows it with efficient and long-lasting antistatic properties and electromagnetic shielding function with absorption as the main function, thereby expanding its application in the field of high-end composite materials.

[0006] To achieve the aforementioned objectives, this invention provides a carbon fiber reinforced antistatic and flame-retardant aramid fiber composite paper, comprising a top layer, a middle core layer, and a bottom layer, sequentially laminated from top to bottom. The top layer, middle core layer, and bottom layer are formed by applying top layer slurry, middle core layer slurry, and bottom layer slurry through a three-channel slurry application system and then forming the paper. The top layer and bottom layer slurries mainly consist of aramid fiber nanofiber (PSA-NF) dispersion, modified LDH-MXene composite flame retardant, and dispersant. The middle core layer slurry mainly consists of aramid filament short fibers, aramid filament precipitated fibers, carbon fiber short fibers, and dispersant. The middle layer accounts for 60%–70%, and the top layer and bottom layer each account for 15%–20%. The antistatic and flame-retardant aramid fiber composite paper has a limiting oxygen index ≥35%, a smoke density reduction of 20–30%, a longitudinal tensile strength ≥22.0 MPa, and a surface resistivity <1.0 × 10⁻⁶. 9 Ω•cm, long-term operating temperature not lower than 250℃.

[0007] Furthermore, in the carbon fiber reinforced antistatic and flame-retardant aramid composite paper provided by the present invention, the solid content of the surface layer slurry and the bottom layer slurry used for papermaking is 0.05%~0.8%.

[0008] Furthermore, in the carbon fiber reinforced antistatic flame-retardant aramid composite paper provided by the present invention, in the surface and bottom slurries used for papermaking, before the required solid content dilution is carried out, the mass percentage of aramid nanofiber (PSA-NF) dispersion is 65%~75%, the mass percentage of modified LDH-MXene composite flame retardant is 20%~30%, and the mass percentage of dispersant is 1%~5%; the solid content of PSA-NF dispersion is 0.25%~5%.

[0009] Furthermore, in the carbon fiber reinforced antistatic flame-retardant aramid composite paper provided by the present invention, the modified LDH-MXene composite flame retardant is obtained by combining LDH and MXene at a mass ratio of 1:(0.8~1.2) and then modifying them with a silane coupling agent; MXene is prepared by in-situ HF generation method; and LDH is prepared by co-precipitation method.

[0010] Furthermore, in the carbon fiber reinforced antistatic and flame-retardant aramid composite paper provided by the present invention, the solid content of the intermediate core layer slurry used for papermaking is 0.05% to 0.5%; before the required solid content dilution, the mass percentage of aramid stub fibers is 28% to 35%, the mass percentage of aramid precipitated fibers is 25% to 35%, the mass percentage of carbon fiber stub fibers is 30% to 38%, and the mass percentage of dispersant is 1% to 5%.

[0011] Furthermore, in the carbon fiber reinforced antistatic and flame-retardant aramid composite paper provided by the present invention, in the intermediate core layer slurry, the average length of the aramid stub fiber is 2~10mm, the average length of the aramid precipitated fiber is 0.5~5mm, and the length of the carbon fiber stub filament is 2~10mm.

[0012] Furthermore, the present invention also provides a method for preparing any of the above-mentioned carbon fiber reinforced antistatic flame-retardant aramid composite paper, comprising the steps of:

[0013] S1. Preparation of aramid nanofiber (PSA-NF) dispersion: After drying the short-cut aramid fibers, add DMSO / KOH mixed solution and stir. After solvent replacement, washing and ultrasonic treatment, PSA-NF dispersion is obtained.

[0014] S2, LDH-MXene composite flame retardant preparation and modification: MXene was prepared by in-situ HF generation method and LDH was prepared by co-precipitation method. After mixing, silane coupling agent was added, and the mixture was dried after reflux reaction to obtain modified LDH-MXene composite flame retardant.

[0015] S3. Three-layer slurry preparation: Top layer slurry and bottom layer slurry: mainly composed of PSA-NF dispersion, modified LDH-MXene composite flame retardant, and dispersant. The mass percentage of aramid nanofiber (PSA-NF) dispersion is 65%~75%, the mass percentage of modified LDH-MXene composite flame retardant is 20%~30%, and the mass percentage of dispersant is 1%~5%. Take the PSA-NF dispersion, add it to the modified LDH-MXene composite flame retardant and PEO dispersant, ultrasonically disperse, and dilute to a solid content of 0.0%. 5%~0.8%; Intermediate core layer slurry: mainly composed of aramid sulfone short-cut fibers, aramid sulfone precipitated fibers, carbon fiber short-cut fibers, and dispersant, wherein the mass percentage of aramid sulfone short-cut fibers is 28%~35%, the mass percentage of aramid sulfone precipitated fibers is 25%~35%, the mass percentage of carbon fiber short-cut fibers is 30%~38%, and the mass percentage of dispersant is 1%~5%; First, the aramid sulfone short-cut fibers are loosened, then carbon fiber short-cut fibers are added for further loosening, then aramid sulfone precipitated fibers and dispersant are added for loosening, and diluted to a solid content of 0.05%~0.5%;

[0016] S4. Wet paper web obtained by papermaking: A three-channel pulping system is used to distribute pulp in the order of bottom layer, middle core layer and top layer. After natural dewatering and vacuum dewatering, a wet paper web with a dryness of 10% to 30% is obtained.

[0017] S5. Drying and heat setting: After the wet paper web is dehydrated by pressing, it undergoes multi-stage temperature-controlled drying and hot pressing to obtain a smooth multi-gradient aramid paper.

[0018] Furthermore, in the preparation method of carbon fiber reinforced antistatic flame-retardant aramid composite paper provided by the present invention, in step S1, a silane coupling agent is added to the PSA-NF dispersion obtained by ultrasonic treatment, and the amount of silane coupling agent added is 2% of the mass of the PSA-NF dispersion.

[0019] Furthermore, in the preparation method of carbon fiber reinforced antistatic flame-retardant aramid composite paper provided by the present invention, in step S5, the hot pressing temperature is 150~350℃, the hot pressing pressure is 2~20MPa, the heating rate is 1~10℃ / min, and the cooling rate is 1~5℃ / min.

[0020] Furthermore, in the preparation method of carbon fiber reinforced antistatic flame-retardant aramid composite paper provided by the present invention, in step S5, the hot pressing adopts a four-stage process procedure of "preheating → heating up → holding up → cooling". The four-stage process procedure is: preheating at 150°C for 5 min → heating up to 300°C (rate 6°C / min) → holding up at 15MPa at 300°C for 20 min → cooling to room temperature (rate 4°C / min).

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) It achieves a synergistic improvement in antistatic, absorption-type electromagnetic shielding performance and mechanical properties. The high-efficiency two-dimensional conductive network constructed by MXene in the surface layer provides durable antistatic properties and forms a synergistic system with the carbon fiber network in the middle layer. Through multiple electromagnetic loss mechanisms, it constructs an electromagnetic shielding function dominated by absorption, which significantly suppresses the secondary reflection of electromagnetic waves. The carbon fiber introduced in the middle core layer interweaves with the aramid fiber to form a strong support skeleton, which greatly improves the tensile strength and tear resistance of the material. Moreover, both MXene and carbon fiber are firmly fixed in the fiber network through nanofiber anchoring and hot pressing processes, avoiding migration or detachment, so that the performance remains stable for a long time, which is far superior to the traditional solution that relies on surface coating or small molecule antistatic agents. (2) It expands the application field. Since the final product not only maintains the inherent high temperature resistance, flame retardancy and low smoke toxicity of aramid, but also has good antistatic function and electromagnetic shielding performance, it expands the application field and improves its application value in high-end fields such as high temperature filtration, electrical insulation, rail transit interior and aerospace equipment protection. Detailed Implementation

[0022] The inventive concept is to organically combine "surface flame retardancy and electromagnetic protection" with "core conductive reinforcement and mechanical support" by designing a "sandwich" structure with clearly defined functional layers. This effectively solves the contradiction between flame retardancy, mechanical strength, and functionality that is difficult to achieve simultaneously in traditional aramid paper. While maintaining the material's inherent high-temperature resistance and flame retardant properties, it further endows it with highly efficient and durable antistatic properties and absorption-based electromagnetic shielding, thereby expanding its application value in the field of high-end composite materials.

[0023] The core innovation of this invention lies in the adoption of a three-layer structure design consisting of a "surface flame-retardant functional layer + intermediate core structural support layer".

[0024] To achieve a unified function of "providing flame retardancy and electromagnetic protection in the surface layer" and "providing electrical conductivity enhancement and mechanical support in the core layer," the inventors designed a sandwich structure. The surface layer is formed by papermaking a slurry mainly composed of aramid nanofiber (PSA-NF) dispersion and MXene nanosheets. The middle core layer is formed by uniformly dispersing aramid short fibers, aramid precipitated fibers, and short carbon fibers in a dispersion solution. By using carbon fiber to reinforce the middle layer and adding MXene to the surface layer, the shortcomings of existing technologies in terms of functional integration and performance synergy are overcome.

[0025] Regarding the modified LDH-MXene composite flame retardant added to the top and bottom layer slurries: In this invention, the modified LDH-MXene composite flame retardant was prepared by the inventors themselves. It was obtained by compounding LDH and MXene at a mass ratio of 1:(0.8~1.2) and then modifying it with a silane coupling agent. The inventors discovered that the mass ratio of LDH to MXene is crucial. If the mass ratio of LDH to MXene is lower than 1:0.8 (i.e., too much MXene), the two-dimensional MXene sheets will easily stack and agglomerate, failing to fully compound with LDH, resulting in limited improvement in electromagnetic absorption performance. Furthermore, due to insufficient LDH content, the smoke density reduction is <20%. If the mass ratio of LDH to MXene is higher than 1:1.2 (i.e., too much LDH), the excessive LDH particles will disrupt the continuity of the MXene conductive network, resulting in a surface resistivity >10. 9 Ω•cm, antistatic failure, and LDH is prone to sedimentation, resulting in uneven distribution of surface components.

[0026] Regarding MXene: MXene is prepared using the HF in-situ generation method. This method preserves the complete two-dimensional sheet structure of MXene, resulting in a large specific surface area, which is beneficial for constructing a continuous conductive network and is suitable for antistatic and electromagnetic shielding functions. The surface is rich in -OH and -F functional groups, facilitating chemical bonding with LDH and silane coupling agents, and allowing for uniform mixing with PSA-NF, avoiding MXene agglomeration during preparation. The method is simple to operate, low in cost, and produces a high-purity product with no impurities affecting the flame retardancy and mechanical properties of aramid paper. If mechanical peeling / melting methods are used, the MXene sheets are easily damaged and uneven in size, failing to form an effective conductive network. Furthermore, the surface has fewer functional groups, resulting in poor composite effect with LDH and failing to achieve the smoke density reduction and electromagnetic shielding performance described in the examples.

[0027] Regarding LDH: LDH is prepared using a co-precipitation method. This method allows for precise control of the LDH interlayer spacing and metal element ratio, resulting in a large specific surface area and numerous flame-retardant and smoke-suppressing active sites. The surface is rich in hydroxyl groups, readily forming hydrogen / covalent bonds with MXene functional groups and silane coupling agents, achieving uniform composite formation and preventing LDH sedimentation in the slurry. The reaction conditions are mild (60~80℃), requiring no high temperature or high pressure. Using hydrothermal / sol-gel methods would result in excessively large and unevenly distributed LDH particles, leading to easy phase separation during MXene composite formation, resulting in uneven surface flame retardancy and insufficient reduction in smoke density.

[0028] Regarding the components, proportions, and solid content of the intermediate slurry, the inventors discovered that when the mass percentage of aramid filament short-cut fibers in the intermediate slurry is 28%–35%, the mass percentage of aramid filament precipitated fibers is 25%–35%, and the mass percentage of carbon fiber short-cut fibers is 30%–38%, the optimal synergistic effect of core layer mechanical strength and electrical conductivity can be achieved. This is achieved by forming a stable mechanical support framework through the interweaving of aramid filament fibers and by constructing a continuous three-dimensional conductive network with the help of carbon fibers.

[0029] The inventors discovered that a pulp solids content of 0.05% to 0.5% in the intermediate core layer achieves good results in uniform fiber dispersion, stable wet paper web formation, and a dense and uniform core layer structure. If the content is below 0.05%, the pulp concentration is too low, resulting in sparse fiber dispersion and an inability to form a dense and continuous fiber-interwoven skeleton. This leads to a loose structure after wet paper web formation, a significant decrease in the mechanical strength of the core layer after drying, and excessively dispersed carbon fiber distribution, preventing the construction of a continuous three-dimensional conductive network and causing electromagnetic shielding and antistatic performance failure. Conversely, if the content is above 0.5%, the pulp concentration is too high, causing aramid filament short-cut fibers, precipitated fibers, and short-cut carbon fibers to easily agglomerate and entangle. This results in extremely poor wet paper web uniformity during papermaking, with localized fiber aggregation and uneven thickness. Agglomerated carbon fiber areas exhibit excessive conductivity, while the conductive network breaks in non-agglomerated areas. Furthermore, fiber entanglement leads to uneven stress within the core layer, making it prone to warping and cracking after drying, and significantly reducing mechanical properties.

[0030] The inventors discovered that the average length of chopped aramid fibers should be within the range of 2-10 mm. This range balances fiber entanglement and dispersion. Lengths below 2 mm result in excessively short fibers, significantly weakening the physical entanglement between fibers and failing to provide effective mechanical support. This leads to a significant decrease in the tensile strength and tear resistance of the core layer, resulting in substandard overall mechanical properties of the composite paper. Lengths above 10 mm result in excessively long fibers, which easily entangle during unwinding and papermaking, forming fiber bundles. This causes uneven pulp dispersion, poor wet paper web uniformity, and stress concentration at localized fiber aggregation points. After drying, the composite paper cracks and delaminates, while also hindering the uniform distribution of carbon fibers and disrupting the continuity of the conductive network.

[0031] The inventors discovered that the average length of aramid precipitated fibers should be within the range of 0.5~5mm. The core function of precipitated fibers is bonding and filling, and this length balances bonding strength and dispersive filling properties. If it is less than 0.5mm, the fiber size will be too fine, resulting in insufficient strength and an inability to effectively bond chopped fibers and carbon fibers. The bonding force between core layer fibers will be weak, making interlayer separation and fiber shedding likely, and significantly reducing tear resistance. If it is greater than 5mm, the fiber flexibility will decrease, making it difficult to fill the fiber gaps, the bonding effect will fail, and it will easily entangle and aggregate with other fibers, leading to a loose core layer structure and a simultaneous decrease in uniformity and mechanical properties.

[0032] The inventors discovered that the length of chopped carbon fiber filaments should be 2-10 mm. This range is a core parameter for constructing a continuous conductive network and achieving mechanical reinforcement. The inventors found that if the length of the chopped carbon fiber filaments is less than 2 mm, the fibers are too short to overlap and form a continuous conductive path, resulting in substandard electromagnetic shielding and antistatic properties. Furthermore, the short carbon fibers cannot participate in the construction of the mechanical framework, leading to ineffective reinforcement. If the length of the chopped carbon fiber filaments is greater than 10 mm, the carbon fibers become rigid and prone to tangling and agglomeration. Uneven dispersion in the slurry leads to the formation of carbon fiber bundles, causing localized abnormalities in the conductivity and mechanical properties of the core layer. Agglomerated bundles become stress concentration points, making the composite paper prone to breakage under stress. Simultaneously, it damages the interwoven structure of the aramid fibers, reducing the overall stability of the core layer.

[0033] The method for preparing any of the above-mentioned carbon fiber reinforced antistatic flame-retardant aramid composite papers includes the following steps:

[0034] S1. Preparation of aramid nanofiber (PSA-NF) dispersion: After drying the short-cut aramid fibers, add DMSO / KOH mixed solution and stir. After solvent replacement, washing and ultrasonic treatment, PSA-NF dispersion is obtained.

[0035] S2, LDH-MXene composite flame retardant preparation and modification: MXene was prepared by in-situ HF generation method and LDH was prepared by co-precipitation method. After mixing, silane coupling agent was added, and the mixture was dried after reflux reaction to obtain modified LDH-MXene composite flame retardant.

[0036] S3. Preparation of three-layer slurry: Prepare the surface slurry, bottom slurry and intermediate core slurry separately.

[0037] Top and bottom layer slurry preparation: The top and bottom layer slurries mainly consist of PSA-NF dispersion, modified LDH-MXene composite flame retardant, and dispersant. The mass percentage of the aramid nanofiber (PSA-NF) dispersion is 65%–75%, the mass percentage of the modified LDH-MXene composite flame retardant is 20%–30%, and the mass percentage of the dispersant is 1%–5%. The specific preparation steps are as follows: Take the PSA-NF dispersion, add it to the modified LDH-MXene composite flame retardant and PEO dispersant, ultrasonically disperse, and dilute to a solid content of 0.05%–0.8%.

[0038] Intermediate core layer slurry preparation: The intermediate core layer slurry is mainly composed of aramid sulfone short-cut fibers, aramid sulfone precipitated fibers, carbon fiber short-cut fibers, and dispersant. The mass percentage of aramid sulfone short-cut fibers is 28%~35%, the mass percentage of aramid sulfone precipitated fibers is 25%~35%, the mass percentage of carbon fiber short-cut fibers is 30%~38%, and the mass percentage of dispersant is 1%~5%. The solid content of the intermediate core layer slurry is 0.05%~0.5%. The specific preparation steps are as follows: The intermediate core layer slurry is prepared by a stepwise decomposition process. After the aramid sulfone short-cut fibers are decomposed, carbon fiber short-cut fibers are added for further decomposition, and then aramid sulfone precipitated fibers and dispersant are added.

[0039] S4. Wet paper web production: A three-channel pulping system is used to distribute pulp in the order of bottom layer, middle core layer and top layer. After natural dewatering and vacuum dewatering, a wet paper web with a dryness of 10% to 30% is obtained.

[0040] S5. Drying and heat setting: After the wet paper web is dehydrated by pressing, it undergoes multi-stage temperature-controlled drying and hot pressing to obtain a smooth multi-gradient aramid paper.

[0041] Besides the solid content, component selection, and component ratio of the slurry affecting the performance of the final product, the preparation steps of "preparation of arylsulfonyl fibrous nanofiber (PSA-NF) dispersion," "preparation and modification of LDH-MXene composite flame retardant," and heat setting process conditions all have a significant impact on the performance of the final product. The inventors discovered that the following process parameters can achieve the intended results: hot pressing temperature 150~350℃, hot pressing pressure 2~20MPa, total hot pressing time 2~30 minutes, heating rate 1~10℃ / min, and cooling rate 1~5℃ / min. More preferably, the hot pressing adopts a four-stage process procedure of "preheating → heating → holding → cooling," which is: preheating at 150℃ for 5 minutes → heating to 300℃ (rate 6℃ / min) → holding at 300℃ and 15MPa for 20 minutes → cooling to room temperature (rate 4℃ / min).

[0042] The composite paper prepared by the above method has a limiting oxygen index (LOI) ≥35%, a smoke density reduction of 20-30%, a longitudinal tensile strength ≥22.0 MPa, and a surface resistivity <1.0×10⁻⁶. 9 Ω•cm, long-term operating temperature not lower than 250℃.

[0043] Example 1

[0044] In this embodiment, DMSO, KOH, silane coupling agent, and PEO dispersant were all commercially available; aramid filament short-cut fibers and aramid filament precipitated fibers were self-made.

[0045] This embodiment prepares antistatic flame-retardant aramid composite paper according to the following steps:

[0046] (1) Preparation of PSA-NF dispersion: After drying the short-cut aramid fibers, add DMSO / KOH mixed solution (mass ratio 10:1) and stir for 24h. After replacement with deionized water solvent and washing until neutral, ultrasonic treatment and dilution are performed to obtain PSA-NF dispersion with a solid content of 0.25%.

[0047] (2) Preparation of modified LDH-MXene composite flame retardant: MXene was prepared by in-situ HF generation method and LDH was prepared by co-precipitation method. They were mixed at a mass ratio of 1:0.8, and a silane coupling agent was added. The silane coupling agent accounted for 3% of the mass of the composite flame retardant. The reaction was carried out at 80℃ for 4 hours. After drying, the mixture was pulverized to a particle size ≤5μm to obtain the modified LDH-MXene composite flame retardant.

[0048] (3) Preparation of three-layer slurry: ① Top layer / bottom layer slurry: Take PSA-NF dispersion, add modified LDH-MXene composite flame retardant and PEO dispersant, ultrasonically disperse for 20 min, and dilute to a papermaking solids content of 0.05%; ② Intermediate core layer slurry: First, loosen 2mm aramid filament short-cut fibers for 30 min, add 2mm short-cut carbon fibers and continue loosening for 20 min, then add 0.5mm aramid filament precipitated fibers and PEO dispersant, loosen for 10 min, and dilute to a papermaking solids content of 0.05%;

[0049] (4) Wet paper web is obtained by papermaking: using a slanted wire paper forming machine, the pulp is spread in the order of bottom layer → middle core layer → surface layer. After natural dewatering for 1 hour, vacuum dewatering is performed for 30 minutes to obtain wet paper web.

[0050] (5) Drying and heat setting: After the wet paper web is dehydrated by pressing, it is dried in sections (60℃→80℃→100℃, 1h each), and then placed in a hot press and hot-pressed according to the following parameters: hot pressing temperature 150℃, hot pressing pressure 2MPa, total hot pressing time 2min, heating rate 1℃ / min, cooling rate 1℃ / min; after hot pressing, it is cooled to room temperature to obtain composite paper samples.

[0051] Tests showed that the aramid fiber paper had a LOI of 35.0%, a smoke density reduction of 20.0%, a longitudinal tensile strength of 22.3 MPa, and a surface resistivity of 1.0 × 10⁻⁶. 8 Ω•cm, with a heat shrinkage rate of 1.2% at a long-term operating temperature of 250℃.

[0052] Example 2

[0053] In this embodiment, DMSO, KOH, silane coupling agent, and PEO dispersant were all commercially available; aramid filament short-cut fibers and aramid filament precipitated fibers were self-made.

[0054] The process is basically the same as in Example 1, except that the following parameters are adjusted: (1) The solid content of the PSA-NF dispersion is adjusted to 2.5%, and the ultrasonic treatment time is 40 min; (2) LDH and MXene are mixed at a mass ratio of 1:1, the amount of silane coupling agent added is 4%, and the reaction time is 5 h; (3) The intermediate core layer pulp is loosened: 6 mm aramid short-cut fibers are loosened for 30 min, 6 mm short-cut carbon fibers are added and loosened for 25 min, and then 2.5 mm aramid precipitated fibers are added and loosened for 15 min; (4) The hot pressing parameters are adjusted to 250℃, 10 MPa, 15 min, heating rate of 5℃ / min, cooling rate of 3℃ / min; the wet paper web dryness is increased to 20%, and the segmented drying temperature is 60℃→90℃→110℃, each for 1 h.

[0055] Tests showed that the aramid fiber paper had a LOI of 37.5%, a smoke density reduction of 26.5%, a longitudinal tensile strength of 28.5 MPa, and a surface resistivity of 5.0 × 10⁻⁶. 7 Ω·cm, with a heat shrinkage rate of 0.8% at a long-term operating temperature of 260℃.

[0056] Example 3

[0057] In this embodiment, DMSO, KOH, silane coupling agent, and PEO dispersant were all commercially available; aramid filament short-cut fibers and aramid filament precipitated fibers were self-made.

[0058] The process is basically the same as in Example 1, except for the following parameters: (1) The solid content of the PSA-NF dispersion is adjusted to 5.0%, and the ultrasonic treatment time is 50 min (power 400W) to avoid agglomeration; (2) LDH and MXene are mixed at a mass ratio of 1:1.2, the amount of silane coupling agent added is 5%, and the reflux reaction is carried out for 6 h to ensure uniform composite; (3) The pulp of the intermediate core layer is loosened: 10 mm aramid short-cut fiber is loosened for 40 min, 10 mm short-cut carbon fiber is added and loosened for 30 min, and then 5 mm aramid precipitated fiber is added and loosened for 20 min to increase the loosening time and avoid fiber entanglement; (4) The hot pressing parameters are adjusted to 350℃, 20MPa, 30 min, the heating rate is 10℃ / min, and the cooling rate is 5℃ / min; the wet paper web dryness is increased to 30%, and the segmented drying temperature is 70℃→100℃→120℃, each for 1.5 h; the pressing pressure is increased to 2MPa to ensure sufficient dehydration.

[0059] Tests showed that the aramid fiber paper had a LOI of 38.2%, a smoke density reduction of 29.8%, a longitudinal tensile strength of 32.1 MPa, and a surface resistivity of 8.0 × 10⁻⁶. 7 Ω•cm, with a heat shrinkage rate of 0.6% at a long-term operating temperature of 270℃.

[0060] Example 4

[0061] In this embodiment, DMSO, KOH, silane coupling agent, and PEO dispersant were all commercially available; aramid filament short-cut fibers and aramid filament precipitated fibers were self-made.

[0062] Combining the advantages of the processes in Examples 2 and 3, the dissolution and hot pressing steps were optimized: (1) PSA-NF dispersion was ultrasonically treated for 45 minutes, and a small amount of silane coupling agent (accounting for 2% of the mass of PSA-NF) was added to enhance the bonding force with MXene; (2) Modified LDH-MXene composite flame retardant was ball-milled for 30 minutes, and the particle size was controlled at 2~3μm to ensure uniform dispersion; (3) The intermediate core layer slurry adopted the "step dissolution + segmented dispersion" process, 5mm aramid short-cut fiber was dissoluted for 35 minutes, 5mm short-cut carbon fiber was added and dissoluted for 25 minutes, and then 2mm aramid precipitated fiber was added, while dissolution was carried out and dispersant was added; (4) Hot pressing adopted the four-stage procedure of "preheating → heating → heat preservation → cooling": 150℃ preheating for 5 minutes → heating to 300℃ (rate 6℃ / min) → heat preservation at 300℃ and 15MPa for 20 minutes → cooling to room temperature (rate 4℃ / min) to ensure strong interlayer bonding.

[0063] Tests showed that the aramid fiber paper had a LOI of 38.0%, a smoke density reduction of 28.2%, a longitudinal tensile strength of 30.8 MPa, and a surface resistivity of 4.2 × 10⁻⁶. 7Ω·cm, with a heat shrinkage rate of 0.7% at a long-term operating temperature of 262℃.

Claims

1. A carbon fiber reinforced antistatic flame-retardant aramid fiber composite paper, characterized in that, The paper comprises, from top to bottom, a top layer, an intermediate core layer, and a bottom layer. The top layer, intermediate core layer, and bottom layer are formed by applying top layer slurry, intermediate core layer slurry, and bottom layer slurry through a three-channel slurry application system and then forming the final product. The top layer and bottom layer slurries mainly consist of a dispersion of aramid nanofibers (PSA-NF), a modified LDH-MXene composite flame retardant, and a dispersant. The intermediate core layer slurry mainly consists of aramid short-cut fibers, aramid precipitated fibers, carbon fiber short-cut fibers, and a dispersant. The intermediate layer accounts for 60%–70% of the total mass, while the top layer and bottom layer each account for 15%–20%. The antistatic and flame-retardant aramid composite paper has a limiting oxygen index ≥35%, a smoke density reduction of 20–30%, a longitudinal tensile strength ≥22.0 MPa, and a surface resistivity <1.0 × 10⁻⁶. 9 Ω•cm, long-term operating temperature not lower than 250℃.

2. The carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 1, characterized in that... In the surface layer and the bottom layer slurry used for papermaking, the solid content of the surface layer slurry and the bottom layer slurry is 0.05% to 0.8%.

3. The carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 1, characterized in that... In the surface layer and the bottom layer slurry used for papermaking, before the required solid content dilution, the mass percentage of the aramid nanofiber (PSA-NF) dispersion is 65%~75%, the mass percentage of the modified LDH-MXene composite flame retardant is 20%~30%, and the mass percentage of the dispersant is 1%~5%; the solid content of the PSA-NF dispersion is 0.25%~5%.

4. The carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 1, characterized in that... The modified LDH-MXene composite flame retardant is obtained by combining LDH and MXene at a mass ratio of 1:(0.8~1.2) and then modifying them with a silane coupling agent; the MXene is prepared by in-situ HF generation; and the LDH is prepared by co-precipitation.

5. The carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 1, characterized in that... In the intermediate core layer slurry used for papermaking, the solid content of the intermediate core layer slurry is 0.05% to 0.5%; before the required solid content dilution, the mass percentage of the aramid sulfone short-cut fibers is 28% to 35%, the mass percentage of the aramid sulfone precipitated fibers is 25% to 35%, the mass percentage of the carbon fiber short-cut fibers is 30% to 38%, and the mass percentage of the dispersant is 1% to 5%.

6. The carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 1, characterized in that... In the intermediate core layer slurry, the average length of the aramid filament short-cut fibers is 2~10mm, the average length of the aramid filament precipitated fibers is 0.5~5mm, and the length of the carbon fiber short-cut filaments is 2~10mm.

7. A method for preparing carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in any one of claims 1 to 6, characterized in that, Including the following steps: S1. Preparation of aramid nanofiber (PSA-NF) dispersion: After drying the aramid short-cut fibers, add DMSO / KOH mixed solution and stir. After solvent replacement, washing and ultrasonic treatment, PSA-NF dispersion is obtained. S2, LDH-MXene composite flame retardant preparation and modification: MXene was prepared by in-situ HF generation method and LDH was prepared by co-precipitation method. After mixing, silane coupling agent was added, and the mixture was dried after reflux reaction to obtain modified LDH-MXene composite flame retardant. S3. Three-layer slurry preparation: Top layer slurry and bottom layer slurry: mainly composed of PSA-NF dispersion, modified LDH-MXene composite flame retardant, and dispersant. The mass percentage of aramid nanofiber (PSA-NF) dispersion is 65%~75%, the mass percentage of modified LDH-MXene composite flame retardant is 20%~30%, and the mass percentage of dispersant is 1%~5%. Take the PSA-NF dispersion, add it to the modified LDH-MXene composite flame retardant and PEO dispersant, ultrasonically disperse, and dilute to a solid content of 0.0%. 5%~0.8%; Intermediate core layer slurry: mainly composed of aramid sulfone short-cut fibers, aramid sulfone precipitated fibers, carbon fiber short-cut fibers, and dispersant, wherein the mass percentage of aramid sulfone short-cut fibers is 28%~35%, the mass percentage of aramid sulfone precipitated fibers is 25%~35%, the mass percentage of carbon fiber short-cut fibers is 30%~38%, and the mass percentage of dispersant is 1%~5%; First, the aramid sulfone short-cut fibers are loosened, then carbon fiber short-cut fibers are added for further loosening, then aramid sulfone precipitated fibers and dispersant are added for loosening, and diluted to a solid content of 0.05%~0.5%; S4. Wet paper web obtained by papermaking: A three-channel pulping system is used to distribute pulp in the order of bottom layer, middle core layer and top layer. After natural dewatering and vacuum dewatering, a wet paper web with a dryness of 10% to 30% is obtained. S5. Drying and heat setting: After the wet paper web is dehydrated by pressing, it undergoes multi-stage temperature-controlled drying and hot pressing to obtain a smooth multi-gradient aramid paper.

8. The method for preparing a carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 7, characterized in that... In step S1, a silane coupling agent is added to the PSA-NF dispersion obtained by ultrasonic treatment, and the amount of the silane coupling agent added is 2% of the mass of the PSA-NF dispersion.

9. The method for preparing a carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 7, characterized in that... In step S5, the hot pressing temperature is 150~350℃, the hot pressing pressure is 2~20MPa, the heating rate is 1~10℃ / min, and the cooling rate is 1~5℃ / min.

10. The method for preparing a carbon fiber reinforced antistatic flame-retardant aramid composite paper as described in claim 9, characterized in that... In step S5, the hot pressing adopts a four-stage process procedure of "preheating → heating up → holding → cooling". The four-stage process procedure is: preheating at 150℃ for 5 min → heating up to 300℃ (rate 6℃ / min) → holding at 15MPa at 300℃ for 20 min → cooling to room temperature (rate 4℃ / min).