A surface micro-arc treatment process for aluminum alloy automobile parts

By using three-stage gradient current density and variable frequency pulse power supply control, dual-stage temperature regulation, and rare earth oxide graphene additives, the problems of high film porosity, edge effect, and high energy consumption in micro-arc oxidation technology on aluminum alloy automotive parts have been solved, achieving efficient and environmentally friendly ceramic layer treatment that meets the salt spray resistance test requirements of automotive parts.

CN123063831APending Publication Date: 2026-11-10NANTONG CHAYO ELECTROCHEMICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611334509.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing micro-arc oxidation technology for the surface treatment of aluminum alloy automotive parts suffers from problems such as high film porosity, severe edge and corner effects on complex-shaped parts, high energy consumption, poor electrolyte stability, and insufficient adhesion between the film and subsequent coatings, making it difficult to meet the stringent requirements of automotive parts.

Method used

A dense and uniform ceramic layer is formed by using a three-stage gradient current density combined with a variable frequency pulse power supply, a two-stage electrolyte temperature control, rare earth and graphene oxide composite additives, and vacuum impregnation sealing technology, along with edge suppression current regulation.

Benefits of technology

It significantly improves the density and uniformity of the film, reduces energy consumption, extends electrolyte life, enhances corrosion resistance and film uniformity of complex curved parts, and meets the salt spray resistance test requirements of automotive parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application discloses a surface micro-arc treatment process for aluminum alloy automobile parts, which comprises the following steps: S1, pretreatment: sequentially performing degreasing cleaning, alkali corrosion roughening, pickling and descaling, and deionized water cleaning on the aluminum alloy automobile parts; S2, electrolyte preparation: preparing a water-based composite electrolyte; S3, micro-arc oxidation treatment: placing the pretreated aluminum alloy automobile parts as an anode in the electrolyte, taking a stainless steel plate as a cathode, and adopting a three-stage gradient current density combined with a variable-frequency pulse power source to perform micro-arc oxidation treatment; and S4, post-treatment and sealing: after the micro-arc oxidation treatment, the aluminum alloy automobile parts are washed with hot water, rinsed with deionized water, and then subjected to vacuum immersion sealing treatment, and then taken out, drained and solidified. The application has the advantages that a uniform and dense ceramic layer with excellent performance is obtained on the surface of the aluminum alloy automobile parts, meanwhile, energy consumption is remarkably reduced, the service life of the electrolyte is prolonged, the application is green and environment-friendly, and is suitable for large-scale production of automobile parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal surface treatment technology, and in particular to a micro-arc surface treatment process for aluminum alloy automotive parts. Background Technology

[0002] Aluminum alloys, due to their high specific strength, light weight, and excellent thermal and electrical conductivity, occupy a core position in the automotive lightweighting process. With the rapid development of new energy vehicles and lightweight body technologies, the application ratio of aluminum alloys in automotive powertrains, chassis, and body structural components continues to rise. However, the low hardness, poor wear resistance, and insufficient corrosion resistance of aluminum alloys directly limit their service life under harsh conditions such as friction, corrosion, and high temperatures. Therefore, surface strengthening treatment is necessary.

[0003] Currently, the mainstream surface treatment technologies for aluminum alloys include: anodizing, chemical conversion treatment (such as chromate passivation), electroplating, spraying, and micro-arc oxidation (also known as plasma electrolytic oxidation, PEO).

[0004] Micro-arc oxidation technology is a high-voltage plasma discharge surface treatment technology developed based on anodic oxidation. Its principle is as follows: An aluminum alloy workpiece is placed in an electrolyte, and a voltage higher than the anodic breakdown voltage is applied, causing micro-discharge on the workpiece surface. Under the action of high-temperature and high-pressure micro-plasma, a ceramic layer mainly composed of α-Al₂O₃ and γ-Al₂O₃ is generated in situ. Compared with anodic oxidation, micro-arc oxidation films have significant advantages such as high hardness (up to 1000~2000 HV), large thickness (up to tens to hundreds of micrometers), high bonding strength with the substrate (metallurgical bonding), and excellent wear and corrosion resistance, making it considered one of the most promising aluminum alloy surface treatment technologies.

[0005] However, existing micro-arc oxidation technology still faces a series of technical bottlenecks that urgently need to be addressed when it is applied to the mass production of automotive parts:

[0006] 1. The film layer has high porosity and insufficient density. During micro-arc oxidation, plasma discharge inevitably forms micropores and discharge channels. The porosity of the porous layer on the surface of ceramic layers prepared by existing technologies is generally between 5% and 15%, and the porous structure easily becomes a corrosive medium (Cl). - The porous structure allows for the penetration of substances such as water vapor and salt spray, resulting in insufficient corrosion resistance and making it difficult to meet the stringent requirements of the neutral salt spray test (NSS) for automotive components, which must be ≥336 hours. This porosity issue is particularly prominent for chassis and wheel hub components that are exposed to road salt spray environments for extended periods.

[0007] 2. Complex-shaped parts suffer from severe edge and corner effects, resulting in uneven film thickness and performance. Automotive parts often have complex three-dimensional curved surfaces with numerous edges, sharp corners, holes, and depressions. Micro-arc oxidation discharge concentrates current density at sharp corners and edges, leading to excessively strong local discharge, causing abnormally thick film, increased roughness, and even defects such as "scarring" and "ablation." Conversely, current density is lower in internal holes, deep grooves, and depressions, resulting in thinner films or even failure to form a film. This unevenness—"overburning at edges and underburning in depressions"—is one of the main obstacles hindering the mass application of micro-arc oxidation technology in automotive parts.

[0008] 3. High energy consumption and low current efficiency result in high production costs. Existing micro-arc oxidation processes typically employ constant current density or a single voltage mode. The current density fluctuates greatly throughout the process, and a large amount of electrical energy is lost as heat, resulting in a specific energy consumption as high as 2~4 kWh / m²·μm. The electrolyte temperature rises rapidly, requiring a high-power cooling system, which leads to high energy and equipment costs and limits the economic viability of large-scale production.

[0009] 4. Poor electrolyte stability, short service life, and pollution issues. Traditional micro-arc oxidation electrolytes often use high-concentration silicates. After prolonged operation, the number of suspended particles in the electrolyte increases, pH drifts, and conductivity fluctuates, leading to unstable membrane quality and requiring frequent replacement. Furthermore, some processes use formulations with high chromium and phosphorus content, posing environmental risks and failing to meet the increasingly stringent environmental requirements of the automotive industry.

[0010] 5. Insufficient adhesion and functional integration between the film layer and subsequent coatings. For components that require further coating or to be endowed with self-lubricating, antibacterial, or other functions, the existing single micro-arc oxidation film layer is insufficient to meet the synergistic requirements of the ceramic hard layer and the functional surface layer. Summary of the Invention

[0011] The purpose of this invention is to provide a surface micro-arc treatment process for aluminum alloy automotive parts, which obtains a high-performance, uniform, and dense ceramic layer on the surface of aluminum alloy automotive parts, while significantly reducing energy consumption, improving electrolyte life, being environmentally friendly, and suitable for the large-scale production of automotive parts.

[0012] The above-mentioned technical objective of the present invention is achieved through the following technical solution: A surface micro-arc treatment process for aluminum alloy automotive parts includes the following steps: S1, Pretreatment: The aluminum alloy automotive parts are sequentially degreased and cleaned, subjected to alkaline corrosion roughening, pickled to remove ash, and cleaned with deionized water. S2, Electrolyte preparation: Prepare a water-based composite electrolyte. Based on one liter of deionized water, the water-based composite electrolyte consists of the following components: sodium silicate 8~20 g / L, sodium aluminate 2~8 g / L, sodium pyrophosphate 1~6 g / L, potassium hydroxide 0.5~3 g / L, rare earth composite additive 0.2~1.5 g / L, graphene oxide-silane coupling agent composite dispersant 0.05~0.5 g / L, and sodium citrate 0.5~2 g / L. S3, Micro-arc oxidation treatment: The pre-treated aluminum alloy automotive parts are placed in the electrolyte as the anode, and a stainless steel plate is used as the cathode. Micro-arc oxidation treatment is carried out by using a three-stage gradient current density combined with a frequency conversion pulse power supply. S4, Post-treatment sealing: After the micro-arc oxidation treatment, the aluminum alloy automotive parts are washed with hot water and rinsed with deionized water, then vacuum impregnated and sealed, and then taken out, drained and cured. S5, Drying and Performance Inspection: Dry the sealed parts and inspect them.

[0013] Preferably, the alkaline solution used in step S1 for alkaline corrosion roughening is a mixed solution of NaOH 30~60g / L and Na2CO3 10~20g / L, the treatment temperature is 50~70℃, and the treatment time is 2~5min; Pickling and ash removal uses a mixed acid solution of 150~300g / L HNO3 and 20~50g / L HF, treated at room temperature for 30~90s.

[0014] Preferably, the rare earth composite additive in step S2 is a mixture of cerium nitrate and terbium nitrate in a mass ratio of 1:0.3 to 1:1.

[0015] Preferably, the graphene oxide-silane composite dispersant in step S2 is prepared by mixing graphene oxide and γ-aminopropyltriethoxysilane in a mass ratio of 1:2 to 1:5. The preparation method is to disperse graphene oxide in deionized water and sonicate it for 30 to 60 minutes, then add silane coupling agent and stir the mixture at 60 to 80°C for 1 to 2 hours.

[0016] Preferably, in step S2, the pH value of the water-based composite electrolyte is 10.5~12.5, and the conductivity is 25~45 mS / cm.

[0017] Preferably, the three-stage gradient current density combined with the frequency conversion pulse power supply for micro-arc oxidation treatment in step S3 specifically includes: the first stage, with a current density J1 = 2~4A / dm 2 Frequency 600~1000Hz, duty cycle 15%~25%, processing time 3~8min; The second stage uses a constant current-constant voltage composite mode to increase the current density to J2=5~8A / dm. 2The frequency varies in a decreasing pattern within the range of 200~600Hz, with a duty cycle of 35%~50%, and the processing time is 15~40 minutes. The third stage reduces the current density to J3 = 3~5 A / dm. 2 The process involves using a high-frequency refined pulse of 1000~2000Hz with a duty cycle of 10%~20% for 5~15 minutes. During the first and second stages, the electrolyte temperature is 15~25℃, and during the third stage, the electrolyte temperature rises to 30~40℃.

[0018] Preferably, in the second stage, during the process of the current density linearly increasing from J1 to J2, the frequency gradually decreases from 600~1000Hz to 300~500Hz; then, while keeping J2 constant, the frequency decreases in a stepwise manner of 50~100Hz every 1~3 minutes to 200~300Hz.

[0019] Preferably, in step S3, the micro-arc oxidation treatment employs corner suppression current control, applying a current density 10% to 25% lower than that in the central region to the discharge circuit corresponding to the corner and edge areas of the workpiece.

[0020] Preferably, the ratio of the cathode area to the anode area in the micro-arc oxidation treatment in step S3 is 2:1 to 4:1.

[0021] Preferably, the sealing agent used for vacuum impregnation sealing in step S4 is a nano-zirconia-organic silicon composite sealing liquid, with a vacuum degree ≤2kPa, impregnation for 10~30min, and then curing at 120~180℃ for 30~60min; The nano-zirconia-organosilicon composite sealing solution comprises the following weight groups: 30-50 parts of nano-zirconia sol with a solid content of 10%-20%, 10-20 parts of methyltrimethoxysilane, 5-15 parts of γ-glycidyl etheroxypropyltrimethoxysilane, 30-50 parts of anhydrous ethanol, and 5-15 parts of water.

[0022] In summary, the present invention has the following beneficial effects: 1. Significantly improved film density: Through three-stage current density gradient and frequency conversion pulse control, combined with two-stage temperature regulation, the porosity of the loose layer on the surface of the micro-arc oxidation ceramic layer obtained by this invention can be controlled at 1%~4%, which is significantly lower than the 5%~15% of the existing technology.

[0023] 2. Excellent comprehensive mechanical properties: The film thickness can reach 40~80μm, the microhardness reaches 1200~1800HV, the bonding strength with the substrate is high (0 grade in cross-cut test, bonding strength in tensile test >30MPa), and the wear resistance is excellent.

[0024] 3. Outstanding corrosion resistance: Aluminum alloy automotive parts treated with this invention can withstand more than 720~1000h of neutral salt spray test without matrix corrosion, which is significantly better than existing micro-arc oxidation process (usually 336~500h) and anodizing process.

[0025] 4. Good uniformity of complex curved surfaces: By controlling the current at the edges and corners, the thickness difference of the film in various parts of complex shaped components is controlled within ±15%, eliminating overburning at the edges and corners and underburning in the concave areas.

[0026] 5. Significantly reduced energy consumption: Three-stage gradient control avoids ineffective high-current discharge, reducing specific energy consumption to 1.2~1.8kWh / m²·μm, which is about 30%~50% lower than traditional processes.

[0027] 6. Green and environmentally friendly: The electrolyte is free of chromium and high concentration of phosphorus, and uses rare earth and graphene oxide green additives, making wastewater treatment simple; the electrolyte has a long service life, can operate stably and sustainably, and reduces emissions. Detailed Implementation

[0028] The specific embodiments of the present invention will be further described below. These embodiments do not constitute a limitation on the present invention.

[0029] Example 1 Taking a certain type of aluminum alloy automobile engine cylinder head (material: ZL105 cast aluminum alloy, chemical composition: Si 4.5%~5.5%, Cu 1.0%~1.5%, Mg 0.4%~0.6%, the remainder being Al) as an example, the process of this invention is used for surface micro-arc treatment.

[0030] S1, Preprocessing The aluminum alloy cylinder head was subjected to the following steps: degreasing and cleaning (using an industrial alkaline degreasing agent containing 20g / L NaOH, 15g / L Na2SiO3, and 3g / L surfactant, soaked at 60℃ for 10min with ultrasonic assistance); alkaline corrosion roughening (using a mixed alkaline solution of 45g / L NaOH and 15g / L Na2CO3, treated at 60℃ for 4min); acid pickling and descaling (using a mixed acid solution of 200g / L HNO3 and 35g / L HF, treated at room temperature for 60s); and two-stage countercurrent rinsing with deionized water. A clean and activated substrate was obtained.

[0031] S2, Electrolyte preparation Prepare the electrolyte (per 1L) according to the following ratio: sodium silicate 14g / L; sodium aluminate 5g / L; sodium pyrophosphate 3g / L; potassium hydroxide 1.5g / L; rare earth composite additive 1.0g / L (cerium nitrate:terbium nitrate = 1:0.6); graphene oxide-silane composite dispersant 0.2g / L (graphene oxide:KH-550 = 1:3); sodium citrate 1g / L; the remainder is deionized water. Adjust the pH to 11.5 with KOH to control the conductivity at 35mS / cm.

[0032] Preparation of graphene oxide-silane composite dispersant: 0.05 g of graphene oxide was ultrasonically dispersed in 50 mL of deionized water for 60 min, 0.15 g of KH-550 was added, and the mixture was stirred at 70 °C for 1.5 h to obtain the composite dispersant.

[0033] S3, Micro-arc oxidation treatment The pretreated cylinder head (approximately 0.5 m²) was immersed in the electrolyte as the anode, and a stainless steel cathode was used with a cathode / anode area ratio of 3:1. A three-stage gradient current density combined with a variable frequency pulse power supply is adopted: Stage 1: Current density J1 = 3 A / dm², frequency f = 800 Hz, duty cycle D = 20%, processing time t1 = 5 min, electrolyte temperature controlled at 15℃; Stage 2: Current density linearly increases from 3 A / dm² to 6 A / dm² over 8 min, frequency linearly decreases from 800 Hz to 300 Hz; then J = 6 A / dm² is maintained, frequency decreases from 300 Hz to 200 Hz in a stepwise manner of 80 Hz every 2 min, duty cycle D = 45%, total processing time t2 = 28 min, electrolyte temperature controlled at 20℃; Stage 3: Current density J3 = 4 A / dm², high-frequency refined pulse f = 1500 Hz, duty cycle D = 15%, processing time t3 = 10 min, electrolyte temperature rises to 35℃.

[0034] The entire micro-arc oxidation process employs edge and corner suppression current control: applying a current density 15% lower than that in the central region to the discharge circuit corresponding to the edge and ridge areas of the cylinder head valve seat ring.

[0035] S4, Post-processing closed After micro-arc oxidation, the workpiece is washed with hot water (60℃), rinsed with deionized water, and then vacuum impregnated and sealed. The sealing solution consists of 40 parts of nano-zirconia sol (15% solid content), 15 parts of MTMS, 10 parts of KH-560, 40 parts of anhydrous ethanol, and 10 parts of water. The vacuum degree is 1.5 kPa, and the impregnation time is 20 min. After being removed and drained, the workpiece is cured at 150℃ for 45 min.

[0036] S5, Drying and Inspection Samples were taken for testing after drying at 80℃.

[0037] Example 2 Taking a certain type of aluminum alloy automobile wheel (material: A356 cast aluminum alloy) as an example, the process parameters are adjusted as follows: pretreatment alkaline solution NaOH 35g / L, Na2CO3 12g / L, 60℃ treatment for 5min; electrolyte: sodium silicate 12g / L, sodium aluminate 6g / L, sodium pyrophosphate 4g / L, KOH 1.8 g / L, rare earth composite additive (Ce:Tb=1:0.5) 1.2 g / L, graphene oxide composite dispersant 0.3 g / L, sodium citrate 1.5 g / L; three-stage treatment: t1=6 min (J1=3.5 A / dm², f=700 Hz, D=20%, 18℃); t2=35 min (J increases to 6.5 A / dm², frequency decreases stepwise from 700 to 250 Hz, D=40%, 22℃); t3=12 min (J3=4.5 A / dm², f=1600 Hz, D=15%, 38℃); edge and corner suppression: the current in the rim edge area is 20% lower than that in the center; sealing: vacuum degree 1.2 kPa, impregnation for 25 min, curing at 160℃ for 40 min.

[0038] Example 3 Taking a certain type of aluminum alloy automotive chassis subframe (material: 6005-T5 wrought aluminum alloy) as an example, the process parameters are adjusted as follows: pretreatment alkaline solution NaOH 50g / L, Na2CO3 18g / L, 65℃ treatment for 3min; electrolyte: sodium silicate 16g / L, sodium aluminate 4g / L, sodium pyrophosphate 2.5g / L, KOH 1.0 g / L, rare earth composite additive 0.8 g / L, graphene oxide composite dispersant 0.15 g / L, sodium citrate 1 g / L; three-stage treatment: t1=4 min (J1=2.5 A / dm², f=900 Hz, D=18%, 15℃); t2=20 min (J increases to 5.5 A / dm², frequency 900→300 Hz, D=35%, 18℃); t3=8 min (J3=3.5 A / dm², f=1800 Hz, D=12%, 30℃); edge and corner suppression: the current in the weld protrusion and edge area is 18% lower than that in the center; sealing: vacuum degree 1.8 kPa, impregnation for 18 min, curing at 140℃ for 50 min.

[0039] Comparative Example The comparative example used a conventional micro-arc oxidation process (constant current density 6A / dm², constant frequency 500Hz, duty cycle 40%, constant electrolyte temperature 20℃, conventional silicate electrolyte, hot water sealing), with the remaining conditions being the same as in Example 1, as a performance comparison benchmark.

[0040] To verify the technical effects of the present invention, the following testing methods were used to systematically test the film layers of the embodiments and comparative examples.

[0041]

[0042] Comparison of film thickness and hardness

[0043] Conclusion: The film thickness uniformity (range ±8%~14%) of the embodiments of the present invention is significantly better than that of the comparative example (±28%), indicating that the edge suppression current regulation effectively solves the problems of overburning at the edges and underburning at the concave surfaces of complex curved parts. The surface hardness (1420~1650HV) is improved by about 45%~68% compared with the comparative example (980HV), and the roughness is significantly reduced.

[0044] Comparison of membrane porosity and compactness

[0045] Conclusion: Through the synergistic effect of three-stage gradient control, frequency conversion pulse, and dual-stage temperature regulation, the porosity of the surface loose layer of this invention is reduced to 2.9%~3.8%, which is about 70% lower than that of the comparative example (12.6%); the porosity of the intermediate dense layer is as low as 0.9%~1.5%, and the film density is greatly improved.

[0046] Comparison of corrosion resistance performance (neutral salt spray NSS test)

[0047] Conclusion: The neutral salt spray corrosion resistance time of the film layer of the present invention reaches 760~940h, which is about 1~1.5 times higher than that of the comparative example (380h). Moreover, the rust area ratio is extremely low after 200h of salt spray, which meets the stringent corrosion resistance requirements of ≥720h for components such as automobile chassis and wheel hubs.

[0048] Comparison of bond strength and wear resistance

[0049] Conclusion: The membrane of this invention achieved grade 0 in the cross-cut test, with a tensile bond strength of 32~37MPa, which is about 43%~64% higher than that of the comparative example (22.4MPa). The wear amount was reduced by about 67%~77%, the coefficient of friction was reduced, and the wear resistance was significantly better than that of the comparative example.

[0050] Comparison of energy consumption and electrolyte lifespan

[0051] Conclusion: The energy consumption of this invention is 1.3~1.6 kWh / m²·μm, which is about 43%~54% lower than that of the comparative example (2.8 kWh / m²·μm); the continuous operating life of the electrolyte reaches 300~340h, which is about 2.5 times higher than that of the comparative example (120h); and the pH drift is small (≤0.4) after 100h of operation, indicating excellent electrolyte stability, effectively reducing production costs and environmental pressure.

[0052] Film phase composition (XRD analysis, Example 1) XRD analysis showed that the main phase composition of the film in Example 1 was: α-Al2O3 (approximately 35%), γ-Al2O3 (approximately 48%), mullite-like amorphous phase, and Ce / Tb-doped oxide (approximately 17%). Among them, the content of α-Al2O3 was significantly increased compared with the comparative example (approximately 18%), which is the key to high hardness and wear resistance.

[0053] Comparison of film thickness in corner / recessed areas (Example 1: Cylinder head, μm)

[0054] Conclusion: By controlling the current of edge suppression, this invention can obtain a uniform film layer of more than 50μm on difficult-to-process parts such as cylinder head edges, inner cavities, and bolt holes, without overburning or underburning defects. In contrast, the comparative model shows overburning of edges (72μm and ablation) and severe underburning of inner cavities and bolt holes (20~26μm), verifying the outstanding effect of edge suppression control on uniform film formation of complex curved parts.

[0055] Overall performance summary

[0056] The core technical difference between this invention and existing micro-arc oxidation technology lies in: 1. Three-stage gradient current density combined with variable frequency pulse power supply control strategy: Existing technologies mostly adopt constant current or single pulse mode. This invention realizes the gradient structure construction of film layer from the process dynamics level through three-stage control of "low current arc initiation - medium current rapid growth (variable frequency reduction) - high frequency fine pulse densification".

[0057] 2. Two-stage electrolyte temperature control: During the film growth stage, the low temperature (15~25℃) inhibits discharge scaling and pore coarsening, while during the densification stage, the temperature is increased (30~40℃) to accelerate reaction kinetics and pore healing. The temperature time gradient is coupled with the current density gradient, and the two work synergistically.

[0058] 3. Synergistic electrolyte system of "pyrophosphate + rare earth composite additive (Ce / Tb) + graphene oxide composite dispersant": rare earth element Ce³ + / Tb³ + The process involves the formation of doped oxides to refine grains and fill pores during discharge; graphene oxide is reduced and embedded in the film layer in the discharge region, bridging micropores and improving conductivity uniformity; pyrophosphate complexes metal ions to stabilize the electrolyte, and the three work together to achieve low porosity and high density.

[0059] 4. Vacuum impregnation of nano-zirconia-organic silicon composite sealing: Unlike conventional hot water sealing or single organic silicon sealing, vacuum assistance is used to allow nano-zirconia particles to penetrate into the micropores of the film layer, and the organic silicon hydrolysis and condensation form a double sealing structure, which further improves corrosion resistance and sealing density.

[0060] 5. Corner Suppression Current Regulation Module: For complex curved automotive parts, this module uses independent rectification in different areas to achieve differentiated current density regulation between corners and recessed regions, solving the problem of unevenness in corner overheating and recessed underheating.

[0061] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art can make various modifications or equivalent substitutions to the present invention within the scope of its essence and protection. Such modifications or equivalent substitutions should also be considered to fall within the protection scope of the present invention.

Claims

1. A surface micro-arc treatment process for aluminum alloy automotive parts, characterized in that, Includes the following steps: S1, Pretreatment: The aluminum alloy automotive parts are sequentially degreased and cleaned, subjected to alkaline corrosion roughening, pickled to remove ash, and cleaned with deionized water. S2, Electrolyte preparation: Prepare a water-based composite electrolyte. Based on one liter of deionized water, the water-based composite electrolyte consists of the following components: sodium silicate 8~20 g / L, sodium aluminate 2~8 g / L, sodium pyrophosphate 1~6 g / L, potassium hydroxide 0.5~3 g / L, rare earth composite additive 0.2~1.5 g / L, graphene oxide-silane coupling agent composite dispersant 0.05~0.5 g / L, and sodium citrate 0.5~2 g / L. S3, Micro-arc oxidation treatment: The pre-treated aluminum alloy automotive parts are placed in the electrolyte as the anode, and a stainless steel plate is used as the cathode. Micro-arc oxidation treatment is carried out by using a three-stage gradient current density combined with a frequency conversion pulse power supply. S4, Post-treatment sealing: After the micro-arc oxidation treatment, the aluminum alloy automotive parts are washed with hot water and rinsed with deionized water, then vacuum impregnated and sealed, and then taken out, drained and cured. S5, Drying and Performance Inspection: Dry the sealed parts and inspect them.

2. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: In step S1, the alkaline corrosion roughening uses a mixed solution of NaOH 30~60g / L and Na2CO3 10~20g / L, the treatment temperature is 50~70℃, and the treatment time is 2~5min. Pickling and ash removal uses a mixed acid solution of 150~300g / L HNO3 and 20~50g / L HF, treated at room temperature for 30~90s.

3. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: In step S2, the rare earth composite additive is a mixture of cerium nitrate and terbium nitrate in a mass ratio of 1:0.3 to 1:

1.

4. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: In step S2, the graphene oxide-silane composite dispersant is prepared by mixing graphene oxide and γ-aminopropyltriethoxysilane in a mass ratio of 1:2 to 1:

5. The preparation method is to disperse graphene oxide in deionized water and sonicate it for 30 to 60 minutes, then add silane coupling agent and stir and react at 60 to 80°C for 1 to 2 hours.

5. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: In step S2, the pH value of the water-based composite electrolyte is 10.5~12.5, and the conductivity is 25~45 mS / cm.

6. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: The micro-arc oxidation process in step S3, which combines a three-stage gradient current density with a frequency conversion pulse power supply, specifically involves the following: The first stage uses a current density J1 = 2~4 A / dm². 2 Frequency 600~1000Hz, duty cycle 15%~25%, processing time 3~8min; The second stage uses a constant current-constant voltage composite mode to increase the current density to J2=5~8A / dm. 2 The frequency varies in a decreasing pattern within the range of 200~600Hz, with a duty cycle of 35%~50%, and the processing time is 15~40 minutes. The third stage reduces the current density to J3 = 3~5 A / dm. 2 The process involves using a high-frequency refined pulse of 1000~2000Hz with a duty cycle of 10%~20% for 5~15 minutes. During the first and second stages, the electrolyte temperature is 15~25℃, and during the third stage, the electrolyte temperature rises to 30~40℃.

7. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 6, characterized in that: In the second segment, as the current density linearly increases from J1 to J2, the frequency gradually decreases from 600~1000Hz to 300~500Hz; then, while keeping J2 constant, the frequency decreases in a stepwise manner of 50~100Hz every 1~3 minutes to 200~300Hz.

8. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: In step S3, the micro-arc oxidation process employs edge and corner suppression current control, applying a current density 10% to 25% lower than that in the central region to the discharge circuit corresponding to the workpiece's edges and corners.

9. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: In step S3, the ratio of cathode to anode area in the micro-arc oxidation treatment is 2:1 to 4:

1.

10. The surface micro-arc treatment process for aluminum alloy automotive parts according to claim 1, characterized in that: In step S4, the sealing agent for vacuum impregnation is a nano-zirconia-organic silicon composite sealing liquid with a vacuum degree ≤2kPa, impregnation for 10~30min, and then curing at 120~180℃ for 30~60min. The nano-zirconia-organosilicon composite sealing solution comprises the following weight groups: 30-50 parts of nano-zirconia sol with a solid content of 10%-20%, 10-20 parts of methyltrimethoxysilane, 5-15 parts of γ-glycidyl etheroxypropyltrimethoxysilane, 30-50 parts of anhydrous ethanol, and 5-15 parts of water.