A composite inner conductor for a superconducting coaxial cable used in quantum computers and its applications.

By employing a composite structure of a copper-nickel alloy core and a niobium-titanium superconducting layer in the inner conductor of a superconducting coaxial cable, the problem of easy breakage when the inner conductor is bent in quantum computers has been solved, enabling reliable wiring in a confined space while maintaining superconducting performance.

CN123072840APending Publication Date: 2026-11-10XIAN SUPERCONDUCTING WIRE TECHNOLOGIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611552018.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The inner conductor of conventional superconducting coaxial cables is prone to breakage when bent in quantum computers, resulting in poor mechanical reliability and making it difficult to lay cables in confined spaces.

Method used

Using a copper-nickel alloy core as a carrier, a composite structure of TiN or NbN transition layer and niobium-titanium superconducting layer is formed to create a concentric layered inner conductor. This is prepared by chemical vapor deposition, reducing the minimum bending radius of the inner conductor to 5D.

Benefits of technology

While ensuring superconducting performance, the minimum bending radius of the inner conductor is significantly reduced, improving mechanical reliability and adapting to the wiring requirements of quantum computers in confined spaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123072840A_ABST
    Figure CN123072840A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of superconducting coaxial cables, and particularly relates to a composite inner conductor for superconducting coaxial cables used in quantum computers and its applications. This invention provides a composite inner conductor for superconducting coaxial cables used in quantum computers. The composite inner conductor has a concentric layered structure, comprising a copper-nickel alloy core, a transition layer, and a niobium-titanium superconducting layer arranged sequentially from the inside out. This invention utilizes the copper-nickel alloy core as a carrier, combined with the transition layer and the outer niobium-titanium superconducting layer, to ensure extremely low signal attenuation in the superconducting coaxial cable while reducing the minimum bending radius of the composite inner conductor to 5D, thus solving the mechanical reliability problem of superconducting coaxial cables in confined spaces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of superconducting coaxial cables, and particularly relates to a composite inner conductor for a superconducting coaxial cable used in quantum computers and its applications. Background Technology

[0002] Superconducting coaxial cables, due to their near-zero-loss signal transmission and excellent fidelity, are widely used in the qubit readout and control systems of quantum computers, becoming a crucial guarantee for achieving high-precision quantum operations. Conventional superconducting coaxial cables often use superconducting niobium-titanium alloys for their inner and outer conductors. However, due to the limited space inside quantum computers, superconducting coaxial cables often need to be bent during wiring. The inner conductor of conventional superconducting coaxial cables, i.e., pure niobium-titanium alloy wire, frequently breaks during bending (minimum bending radius greater than 20D, where D is the outer diameter of the inner conductor), severely affecting its mechanical reliability.

[0003] Therefore, in the field of superconducting coaxial cables, it is particularly important to develop an inner conductor for superconducting coaxial cables used in quantum computers that combines superconductivity with excellent bendability. Summary of the Invention

[0004] The purpose of this invention is to provide a composite inner conductor for a superconducting coaxial cable used in quantum computers. This invention utilizes a copper-nickel alloy core as a carrier, combined with a transition layer and an outer niobium-titanium superconducting layer. While ensuring extremely low signal attenuation in the superconducting coaxial cable, it reduces the minimum bending radius of the inner conductor to 5D, thus solving the mechanical reliability problem of wiring superconducting coaxial cables in confined spaces.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows: On the one hand, the present invention provides a composite inner conductor for a superconducting coaxial cable for quantum computers. The composite inner conductor is a concentric layered structure, comprising a copper-nickel alloy core (1), a transition layer (2), and a niobium-titanium superconducting layer (3) arranged sequentially from the inside to the outside.

[0006] In this invention, the copper-nickel alloy core (1) is located in the innermost layer of the composite inner conductor and is the central matrix of the entire inner conductor. Its outer surface is a continuous and smooth cylindrical surface, providing a supporting carrier for the outer layer structure. The transition layer (2) covers the outer surface of the copper-nickel alloy core (1). Its inner side is in complete contact with the outer surface of the copper-nickel alloy core, and its outer side is a continuous cylindrical surface, serving as a transition connecting the copper-nickel alloy core and the niobium-titanium superconducting layer. The niobium-titanium superconducting layer (3) is the outermost layer of the composite inner conductor. Its inner side is tightly covered with the outer surface of the transition layer. There are no gaps between the layers, which together form an integral concentric cylindrical inner conductor structure.

[0007] Preferably, the nickel content in the copper-nickel alloy core (1) is 25-50 wt%.

[0008] Preferably, the roundness of the copper-nickel alloy core (1) is ±0.02 mm.

[0009] Preferably, the outer surface roughness (Ra) of the copper-nickel alloy core (1) is 0.2-1.0.

[0010] Preferably, the transition layer (2) is composed of TiN or NbN.

[0011] Preferably, the thickness of the transition layer (2) is 300-500 nm.

[0012] Preferably, the Nb content in the niobium-titanium superconducting layer (3) is 40-60 wt%, and the Ti content is 40-60 wt%.

[0013] Preferably, the thickness of the niobium-titanium superconducting layer (3) is 3-7 μm.

[0014] It should be noted that the copper-nickel alloy core can be obtained using conventional drawing processes in this field; the preparation of the transition layer and the niobium-titanium superconducting layer can be carried out by methods such as physical vapor deposition, chemical vapor deposition, and electroplating, and those skilled in the art can apply the corresponding coatings using these methods.

[0015] On the other hand, a method for preparing the composite internal conductor according to the present invention is provided, comprising the following steps: 1. Substrate preparation: The copper-nickel alloy core wire that has been drawn is subjected to surface pretreatment. It is then ultrasonically cleaned with organic solvents (such as acetone and anhydrous ethanol) to remove surface oil stains, then rinsed and activated with dilute acid solution (such as 5-10% dilute nitric acid), and finally cleaned and dried with deionized water to obtain a clean copper-nickel alloy core substrate.

[0016] 2. Deposition of transition layer (NbN): A niobium nitride (NbN) transition layer is deposited on the clean copper-nickel alloy core substrate using chemical vapor deposition (CVD) process.

[0017] Example of process parameters: Niobium pentachloride (NbCl5) and ammonia (NH3) are used as precursor reactant gases, and hydrogen (H2) is used as both carrier and reducing gas; the reaction temperature is controlled at 800℃-1100℃, and the reaction chamber pressure is maintained at 100-500 Pa. The gas flow ratio is NbCl5:H2:NH3≈1:20:10 (volume ratio or molar ratio). The deposition time is adjusted according to the required transition layer thickness (e.g., 1-5 micrometers), typically 30-120 minutes. After deposition, the mixture is slowly cooled to room temperature under an inert atmosphere (e.g., argon).

[0018] 3. Deposition of niobium-titanium (NbTi) superconducting layer: On the surface of the NbN transition layer, a niobium-titanium (NbTi) superconducting layer is further deposited using chemical vapor deposition (CVD).

[0019] Example of process parameters: Niobium pentachloride (NbCl5) and titanium tetrachloride (TiCl4) are used as niobium and titanium sources, respectively, and hydrogen (H2) is used as the carrier gas and reducing gas. The reaction temperature is controlled at 1000℃-1300℃, and the reaction chamber pressure is maintained at 200-1000 Pa. The vapor flow rate ratio of NbCl5 to TiCl4 is precisely controlled (e.g., the molar ratio is adjusted to around 1:1 to obtain a near-equiatomic NbTi alloy), and reacted with excess H2. The total gas flow rate and deposition time are determined according to the desired superconducting layer thickness (e.g., 5-20 μm), typically 1-4 hours. After deposition, annealing is performed under an inert atmosphere (e.g., holding at 800-1000℃ for 30-60 minutes) to optimize the lattice structure of the superconducting phase, followed by slow cooling.

[0020] 4. Post-processing: The composite wire with deposited NbN transition layer and NbTi superconducting layer is subjected to necessary post-processing, such as homogenization annealing in an inert atmosphere or vacuum, to further improve the uniformity of the superconducting layer and the critical current performance.

[0021] In another aspect, a superconducting coaxial cable is provided, wherein the superconducting coaxial cable includes the composite inner conductor described in this invention.

[0022] On another front, the present invention provides the application of the composite inner conductor described herein in the preparation of superconducting coaxial cables.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention utilizes a copper-nickel alloy core as a carrier, combined with a transition layer and an outer niobium-titanium superconducting layer. While ensuring extremely low signal attenuation in the superconducting coaxial cable, it reduces the minimum bending radius of the inner conductor to 5D (D is the outer diameter of the inner conductor), thus solving the mechanical reliability problem of superconducting coaxial cable wiring in confined spaces.

[0024] Specifically, the composite inner conductor of this invention can achieve a minimum bending radius of less than 5D while ensuring superconducting performance.

[0025] This invention uses a copper-nickel alloy-niobium-titanium composite material as the inner conductor of a superconducting coaxial cable, instead of the conventional pure niobium-titanium alloy wire, which effectively improves the problem of easy breakage of the inner conductor when the superconducting coaxial cable is bent.

[0026] The copper-nickel alloy used as the core material in this invention can release the stress generated during bending and reduce the minimum bending radius. The TiN or NbN transition layer in this invention helps improve the stability of the interfacial bonding of the film layers. The niobium-titanium superconducting layer, as the outermost layer, can utilize the skin effect (i.e., transmission on the outermost side of the inner conductor) during signal transmission to ensure the superconducting performance of the inner conductor. Attached Figure Description

[0027] Figure 1 A schematic cross-sectional view of a composite inner conductor in a superconducting coaxial cable for quantum computers, provided as an embodiment of the present invention; Figure reference numerals: 1-Copper-nickel alloy core; 2-Transition layer; 3-Niobium-titanium superconducting layer. Detailed Implementation

[0028] The technical solution of the present invention will be described below with reference to embodiments. However, the present invention is not limited to the following embodiments. Unless otherwise specified, the experimental methods and detection methods described in each embodiment are conventional methods; unless otherwise specified, the reagents and materials can be purchased commercially.

[0029] Example 1 This embodiment provides a composite inner conductor for a superconducting coaxial cable used in quantum computers.

[0030] like Figure 1 As shown, this embodiment provides a composite inner conductor for a superconducting coaxial cable used in quantum computers. The overall outer diameter of the composite inner conductor is 0.2 mm, and it includes: Copper-nickel alloy core 1, the nickel content in copper-nickel alloy core 1 is 25% (wt%), the roundness of copper-nickel alloy core 1 is +0.01mm, and the surface roughness (Ra) of copper-nickel alloy core 1 is 0.2.

[0031] The transition layer 2 is composed of TiN and has a thickness of 300 nm.

[0032] The niobium-titanium superconducting layer 3 contains 40 wt% Nb and 60 wt% Ti, and has a thickness of 3 μm.

[0033] Bending test method: Bend the material sample along the mold (usually 90 degrees or 180 degrees), and then carefully examine the bent outer surface with a magnifying glass for cracks. Find the smallest radius that allows multiple samples to be bent without producing cracks; this is the minimum bending radius of the material.

[0034] The bending test results show that its minimum bending radius is 0.9 mm, which is less than 5D (D is the outer diameter of the inner conductor). The bending radius of a conventional pure niobium titanium inner conductor of this size is 4.3 mm, which is greater than 20D (D is the outer diameter of the inner conductor).

[0035] After assembling the composite inner conductor provided in this embodiment of the invention and the conventional pure niobium-titanium inner conductor into superconducting coaxial cables using conventional processes, the signal attenuation at 5GHz at 4K was measured to be 0.48dB / m and 0.49dB / m, respectively, indicating that the composite inner conductor provided in this embodiment of the invention does not affect the overall superconducting performance of the superconducting coaxial cable.

[0036] Conventional process: The outer side of the inner conductor is insulated with PTFE (polytetrafluoroethylene), and then inserted into the outer conductor (capillary) of the coaxial cable to form a superconducting coaxial cable.

[0037] Example 2 This embodiment provides another composite inner conductor for superconducting coaxial cables used in quantum computers.

[0038] This embodiment provides another type of composite inner conductor for superconducting coaxial cables used in quantum computers. The overall outer diameter of the composite inner conductor is 0.51 mm, and it includes: Copper-nickel alloy core 1, the nickel content in copper-nickel alloy core 1 is 50% (wt%), the roundness of copper-nickel alloy core 1 is +0.02mm, and the surface roughness (Ra) of copper-nickel alloy core 1 is 1.0.

[0039] The composition of transition layer 2 is NbN, and the thickness of transition layer 2 is 500 nm.

[0040] The niobium-titanium superconducting layer 3 contains 60 wt% Nb and 40 wt% Ti, and has a thickness of 7 μm.

[0041] Bending tests (using the same method as in Example 1) showed that its minimum bending radius was 1.5 mm, which is less than 5D (where D is the outer diameter of the inner conductor). The bending radius of a conventional pure niobium-titanium inner conductor of this size is 11 mm, which is greater than 20D (where D is the outer diameter of the inner conductor). After assembling the composite inner conductor provided in this embodiment of the invention and the conventional pure niobium-titanium inner conductor into a superconducting coaxial cable using conventional processes (using the same method as in Example 1), the signal attenuation at 5 GHz at 4 K was measured to be 0.34 dB / m and 0.33 dB / m, respectively. This indicates that the composite inner conductor provided in this embodiment of the invention does not affect the overall superconducting performance of the superconducting coaxial cable.

[0042] The embodiments described above are some, but not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but rather to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art through related deductions and substitutions based on the inventive concept, without inventive effort, are within the scope of protection of the present invention.

Claims

1. A composite inner conductor for a superconducting coaxial cable used in quantum computers, characterized in that, The composite inner conductor has a concentric layered structure, including a copper-nickel alloy core (1), a transition layer (2), and a niobium-titanium superconducting layer (3) arranged sequentially from the inside to the outside.

2. The composite inner conductor according to claim 1, characterized in that, The nickel content in the copper-nickel alloy core (1) is 25-50 wt%.

3. The composite inner conductor according to claim 1, characterized in that, The roundness of the copper-nickel alloy core (1) is ±0.02 mm.

4. The composite inner conductor according to claim 1, characterized in that, The outer surface roughness of the copper-nickel alloy core (1) is 0.2-1.

0.

5. The composite inner conductor according to claim 1, characterized in that, The transition layer (2) is composed of TiN or NbN.

6. The composite inner conductor according to claim 1, characterized in that, The thickness of the transition layer (2) is 300-500 nm.

7. The composite inner conductor according to claim 1, characterized in that, The niobium-titanium superconducting layer (3) contains 40-60 wt% Nb and 40-60 wt% Ti.

8. The composite inner conductor according to claim 1, characterized in that, The thickness of the niobium-titanium superconducting layer (3) is 3-7 μm.

9. A superconducting coaxial cable, characterized in that, The superconducting coaxial cable includes the composite inner conductor as described in any one of claims 1-8.

10. The application of the composite inner conductor according to any one of claims 1-8 in the preparation of superconducting coaxial cables.