A gel composite electrolyte based on metal complexes and its preparation method, and a potassium-ion battery
By preparing a metal complex-anchored gel composite electrolyte in potassium-ion batteries, the problems of low ionic conductivity and mechanical property imbalance of solid electrolytes in potassium-ion batteries are solved, achieving high mechanical strength and long cycle life electrochemical performance stability, which is suitable for solid electrolyte applications in potassium-ion batteries.
Patent Information
- Application Number
- CN202611430243.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-10
AI Technical Summary
Existing potassium-ion batteries have problems with solid electrolytes, such as low ionic conductivity, poor electrode/electrolyte interface stability, and unbalanced mechanical properties, which limit the battery's cycle life and safety.
A gel composite electrolyte was prepared by anchoring a metal complex in a semi-interpenetrating three-dimensional polymer network formed by PVDF-HFP and acrylate monomers and immersing it in an electrolyte solution. The metal complex plays an adsorption role in the polymer backbone, restricting the movement of anions and improving mechanical strength and the stability of ion migration channels.
This technology improves the long-cycle performance and electrochemical stability of potassium-ion batteries, enhances mechanical strength, reduces manufacturing costs, expands application conditions, and enables the application of highly safe solid-state potassium-ion batteries.
Smart Images

Figure CN123073137A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery materials, specifically to a gel composite electrolyte based on metal complexes and its preparation method, and a potassium-ion battery. Background Technology
[0002] Fossil fuels such as oil, coal, and natural gas are non-renewable resources. Over-exploitation and utilization of these resources will accelerate depletion, directly threatening the long-term survival and development of human society. Furthermore, the environmental pollution caused by large-scale use will further damage the ecosystem and human living environment. Against the backdrop of rapid economic development, human society's energy demand continues to rise, and the consumption of fossil fuels is increasing year by year. In this context, developing alternative energy sources to non-renewable resources has become a crucial technology urgently needed to achieve sustainable social development.
[0003] Currently, humans have developed various energy storage technologies, mainly including flywheel energy storage, compressed air energy storage, pumped hydro storage, supercapacitor energy storage, and battery energy storage. Among them, battery energy storage relies on the redox reaction of positive and negative electrode materials to achieve the mutual conversion of chemical energy and electrical energy. Due to its high energy conversion efficiency and adaptability to different application environments and size requirements, it has become a research and application hotspot in the field of energy storage. The main types of energy storage batteries include nickel-metal hydride batteries, lead-acid batteries, flow batteries, and alkali metal-ion batteries. Alkali metal-ion batteries, represented by lithium-ion batteries, sodium-ion batteries, and potassium-ion batteries, have shown significant application potential among various energy storage batteries due to their advantages such as high energy density, excellent cycle performance, no memory effect, and good environmental compatibility.
[0004] Electrolytes, as the ion transport medium between the positive and negative electrodes, are a core component of alkali metal ion battery systems, undertaking the crucial function of ion conduction and directly determining the battery's ion transport efficiency and electrochemical performance. Currently, liquid electrolytes are the main application system in alkali metal ion batteries. Among them, non-aqueous liquid electrolytes are usually prepared by combining organic solvents with alkali metal salts. Although these electrolytes have high ionic conductivity, their organic solvents have inherent defects such as volatility and flammability, which can easily lead to safety accidents such as fires and explosions under charge-discharge cycles, overcharge, or high-temperature conditions, becoming a key bottleneck restricting the large-scale application of alkali metal ion batteries. Therefore, developing novel solid-state electrolytes with high safety has become an important research direction and urgent need in this field.
[0005] An ideal solid-state electrolyte must simultaneously meet multiple performance requirements: high room-temperature ionic conductivity, a wide electrochemical stability window, and excellent chemical / electrochemical stability and mechanical properties to adapt to the actual working environment and assembly needs of the battery. As the core functional material of solid-state alkali metal ion batteries, the performance of the solid-state electrolyte directly determines the overall electrochemical performance and safety characteristics of the solid-state battery. Therefore, recent research on solid-state batteries has mainly focused on the design, preparation, and performance optimization of high-performance solid-state electrolytes.
[0006] Potassium-ion batteries possess significant advantages such as abundant potassium resources and low cost. Solid-state potassium-ion batteries further enhance safety and are currently in the early stages of research and commercialization, showing great development potential. However, solid-state electrolytes for potassium-ion batteries present several research challenges: 1. Ionic conductivity needs improvement. Potassium ions have a large radius, making migration difficult in solid materials, especially resulting in low ionic conductivity at room temperature. 2. Low electrode / electrolyte interface stability. Poor solid-solid contact between the solid electrolyte and electrode materials leads to high interfacial impedance, and some potassium-based solid electrolytes exhibit severe side reactions with the cathode material, significantly affecting battery cycle life and safety. 3. Imbalance between mechanical properties and processability. Solid electrolytes with good flexibility and ease of processing often have lower mechanical strength; conversely, solid electrolytes with high rigidity and mechanical strength are often difficult to process into thin and flexible films. Summary of the Invention
[0007] In view of the problems existing in the prior art, this application provides a gel composite electrolyte based on metal complexes and its preparation method, as well as a potassium-ion battery. The gel composite electrolyte based on metal complexes described in this application has the advantages of wide application conditions, high mechanical strength, long cycle life and stable electrochemical performance.
[0008] To achieve this objective, the following technical solution is adopted in this application: One of the objectives of this application is to provide a method for preparing a gel composite electrolyte based on a metal complex, characterized in that the preparation method includes the following: The metal complex was immersed in an electrolyte, and then subjected to solid-liquid separation to obtain the immersed metal complex. The soaked metal complex is anchored in a semi-interpenetrating three-dimensional polymer network formed by in-situ polymerization of PVDF-HFP and acrylate monomers to obtain a polymer film. The polymer film is immersed in the electrolyte to obtain a gel composite electrolyte based on metal complexes.
[0009] In the preparation method described in this application, the metal complex is anchored in the three-dimensional polymer network of PVDF-HFP by in-situ photopolymer crosslinking monomers, and the gel composite electrolyte is obtained by soaking in electrolyte, for example, by soaking in potassium ion battery electrolyte to obtain solid potassium ion battery gel composite electrolyte. The metal-complex-based gel composite electrolyte prepared in this application, in which the metal complex is doped into a dual polymer backbone and the electrolyte is adsorbed within the metal-complex-doped dual polymer backbone, has the following advantages: The metal complex, doped into the three-dimensional network structure of the polymer, effectively adsorbs organic molecules in the electrolyte, restricts the movement of anionic groups in the electrolyte, and reduces interference with alkali metal ion migration, such as reducing the negative impact on potassium ion migration and increasing the potassium ion transference number. The addition of the metal complex to the polymer increases the mechanical strength of the polymer matrix, making the ion migration channels in the electrolyte more stable, thereby improving the long-cycle performance of solid-state alkali metal ion batteries, such as improving the long-cycle performance of solid-state potassium ion batteries. The embedding of the metal complex increases the amorphous region of the polymer, increases the mobility of polymer chain segments, and promotes ion transport. The metal-complex-based gel composite electrolyte prepared in this application uses readily available raw materials with low toxicity and also has advantages such as wide applicability, high mechanical strength, good cycle performance, and stable electrochemical performance. Furthermore, the preparation process of this application is simple, low-cost, and easy to implement.
[0010] It should be noted that the PVDF-HFP described in this application is a polyvinylidene fluoride-hexafluoropropylene copolymer, which is a conventional polymer material in the art.
[0011] As one technical solution of this application, the metal complex is prepared by the following method: an aqueous solution A of NaN(CN)2 is heated, an aqueous solution B of metal nitrate is added dropwise under stirring, the mixture is cooled to room temperature, allowed to stand, and then subjected to solid-liquid separation, washing, and drying to obtain the metal complex.
[0012] As a technical solution of this application, it satisfies at least one of the following (1) to (6): (1) The metal nitrate includes at least one of Co(NO3)2, Zn(NO3)2 and Cu(NO3)2; (2) The NaN(CN)2 concentration of the aqueous solution A is the same as the metal nitrate concentration of the aqueous solution B, which is 1.3~1.7 mol / L, for example 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L or 1.7 mol / L, but is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0013] (3) Assuming that the weight of aqueous solution A is 100, the weight of aqueous solution B is 40 to 60, such as 40, 43, 45, 47, 50, 52, 55, 57 or 60, but not limited to the listed values. Other unlisted values within the above range are also applicable.
[0014] (4) The target heating temperature is 50~70℃, such as 50℃, 52℃, 55℃, 57℃, 60℃, 63℃, 65℃, 68℃ or 70℃, but is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0015] (5) The settling time is more than 5 days.
[0016] (6) The drying process includes drying in a vacuum drying oven for more than 24 hours.
[0017] As one technical solution of this application, the metal complex is immersed in the electrolyte for more than 10 hours.
[0018] And / or, based on 100 parts by weight of the metal complex, the electrolyte is 100 to 150 parts by weight, such as 100, 110, 120, 130, 140 or 150, but not limited to the listed values. Other unlisted values within the above range also apply.
[0019] As one technical solution of this application, the anchoring includes the following: the soaked metal complex is mixed evenly with PVDF-HFP solution, acrylate monomers and photoinitiator, and then polymerized in situ using ultraviolet light, coated on a glass plate, and freeze-dried to obtain the polymer film.
[0020] As one technical solution of this application, the solvent of the PVDF-HFP solution includes at least one of N-methylpyrrolidone, N,N-dimethylformamide and dimethyl sulfoxide.
[0021] And / or, in the PVDF-HFP solution, the weight ratio of PVDF-HFP to solvent is 1:(10~20), for example, 1:10, 1:11, 1:13, 1:15, 1:17, 1:19, or 1:20, but not limited to the listed values; other unlisted values within the above range are also applicable. For example, in the preparation of the PVDF-HFP solution, 100 parts by weight of PVDF-HFP are dissolved in 1000~2000 parts by weight of solvent.
[0022] And / or, based on 100 parts by weight of acrylate monomers, the PVDF-HFP in the PVDF-HFP solution is 100 to 200 parts by weight, such as 100, 110, 130, 150, 160, 180 or 200, etc.; the photoinitiator is 1 to 3 parts by weight, such as 1, 1.5, 2, 2.5 or 3, etc.; and the metal complex is 10 to 100 parts by weight, such as 10, 30, 50, 60, 80 or 100, etc., but not limited to the listed values. Other unlisted values within the above range also apply.
[0023] And / or, the acrylate monomers include at least one of ethoxylated trimethylolpropane triacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipropylene glycol diacrylate.
[0024] And / or, the photoinitiator includes HMPP. HMPP, chemically named 2-hydroxy-2-methyl-1-phenyl-1-propanone, commonly known in the industry as photoinitiator 1173, is a highly efficient, liquid ultraviolet photoinitiator widely used in UV curing.
[0025] As a technical solution of this application, it satisfies at least one of the following (7) to (12): (7) The uniform mixing includes: stirring at a speed of 500~600 r / min for 2~5 h at room temperature, such as 500 r / min, 510 r / min, 530 r / min, 550 r / min, 560 r / min, 580 r / min or 600 r / min, etc., and stirring time such as 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, etc., but not limited to the listed values. Other unlisted values within the above range are also applicable.
[0026] (8) The wavelength range of the ultraviolet light is 365nm~400nm.
[0027] (9) The in-situ polymerization process is accompanied by stirring, and the stirring speed is 100~200r / min, such as 100r / min, 110r / min, 130r / min, 150r / min, 160r / min, 180r / min or 200r / min, but it is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0028] (10) The in-situ polymerization time is 1 to 2 hours, such as 1 hour, 1.1 hours, 1.3 hours, 1.5 hours, 1.6 hours, 1.8 hours or 2 hours, but is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0029] (11) The thickness of the coating on the glass plate is 100~300μm, such as 100μm, 130μm, 150μm, 180μm, 200μm, 210μm, 230μm, 250μm, 260μm, 280μm or 300μm, but is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0030] (12) The freeze-drying temperature is -60℃, the vacuum degree is -0.1MPa, and the time is 7~10 days.
[0031] As one technical solution of this application, based on 100 parts by weight of polymer film, the amount of electrolyte required for immersion is 200 to 300 parts by weight, such as 200 parts, 210 parts, 230 parts, 250 parts, 260 parts, 280 parts or 300 parts, etc., but is not limited to the listed values. Other unlisted values within the above range are also applicable.
[0032] And / or, the polymer film is immersed in the electrolyte for more than 12 hours.
[0033] The second objective of this application is to provide a metal complex-based gel composite electrolyte, prepared by the preparation method described in the first objective; wherein, in the metal complex-based gel composite electrolyte, the weight parts of the semi-interpenetrating three-dimensional polymer network formed by in-situ polymerization of PVDF-HFP and acrylate monomers are 100-300 based on 100 parts by weight of the metal complex, and the weight parts of the electrolyte adsorbed after soaking are 100-500.
[0034] As one technical solution of this application, the gel composite electrolyte based on metal complexes comprises 100 parts by weight of metal complexes, 100-300 parts by weight of polymer backbones, and 100-500 parts by weight of electrolyte; wherein, the electrolyte is adsorbed in a dual polymer backbone doped with metal complexes; the ligand of the metal complex is a dicyanamide ligand, and the metal salt is selected from cobalt nitrate, zinc nitrate, and copper nitrate; the dual polymer backbone is a composite polymer backbone formed by in-situ polymerization of PVDF-HFP and acrylate crosslinking monomers, and the acrylate crosslinking monomers are selected from ethoxylated trimethylolpropane triacrylate (ETPTA), trimethylolpropane triacrylate (TMPTA), pentaerythritol tetraacrylate (PETEA), and tripropylene glycol diacrylate (TPGDA); the average thickness of the gel composite polymer film is 100-300 μm.
[0035] The third objective of this application is to provide an application of a metal complex-based gel composite electrolyte, wherein the metal complex-based gel composite electrolyte is prepared by the preparation method described in the first objective, and the electrolyte used in the preparation method is a potassium-ion battery electrolyte, which is used as a solid electrolyte for potassium-ion batteries.
[0036] Compared with existing technical solutions, this application has at least the following beneficial effects: (1) In the preparation method described in this application, the metal complex is anchored in the three-dimensional polymer network of PVDF-HFP by in-situ photopolymer crosslinking monomers, and the gel composite electrolyte is obtained by soaking in electrolyte.
[0037] (2) The gel composite electrolyte based on metal complex prepared in this application has metal complex doped in the three-dimensional network structure of polymer, which effectively plays the role of adsorption of organic molecules in electrolyte, restricts the movement of anionic groups in electrolyte, and reduces the interference on the migration of alkali metal ions. For example, it reduces the negative impact of interfering with potassium ion migration and increases the potassium ion transference number.
[0038] (3) The gel composite electrolyte based on metal complexes prepared in this application improves the mechanical strength of the polymer matrix by adding metal complexes to the polymer, making the migration channels of ions in the electrolyte more stable, thereby improving the long cycle performance of solid alkali metal ion batteries, such as improving the long cycle performance of solid potassium ion batteries.
[0039] (4) The gel composite electrolyte based on metal complex prepared in this application has increased the amorphous region of the polymer by the insertion of the metal complex, which increases the mobility of polymer chain segments and promotes ion transport.
[0040] (5) The metal complex-based gel composite electrolyte prepared in this application has readily available raw materials, low toxicity, and also has the advantages of wide application conditions, high mechanical strength, good cycle performance, and stable electrochemical performance. Moreover, the preparation process of this application is simple, low in cost, and easy to implement. Attached Figure Description
[0041] Figure 1 This is a schematic diagram of the microstructure of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 1 of this application.
[0042] Figure 2 This is a linear voltammetric scan result of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 1 of this application.
[0043] Figure 3 This is a graph showing the cycle performance test results of the potassium-ion battery gel composite electrolyte based on metal complexes obtained in Example 1 of this application.
[0044] Figure 4 This is a graph showing the constant current charge-discharge test results of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 1 of this application.
[0045] Figure 5 This is a schematic diagram of the microstructure of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 2 of this application.
[0046] Figure 6 This is a linear voltammetric scan result of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 2 of this application.
[0047] Figure 7 This is a graph showing the cycle performance test results of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 2 of this application.
[0048] Figure 8 This is a schematic diagram of the microstructure of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 3 of this application.
[0049] Figure 9 This is a linear voltammetric scan result of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 3 of this application.
[0050] Figure 10 This is a graph showing the cycle performance test results of the potassium-ion battery gel composite electrolyte based on metal complexes obtained in Example 3 of this application.
[0051] Figure 11 This is a schematic diagram of the microstructure of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 4 of this application.
[0052] Figure 12 This is a linear voltammetric scan result of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Example 5 of this application.
[0053] Figure 13 This is a graph showing the cycle performance test results of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Comparative Example 1 of this application.
[0054] Figure 14 This is a graph showing the cycle performance test results of the potassium-ion battery gel composite electrolyte based on metal complex obtained in Comparative Example 2 of this application. Detailed Implementation
[0055] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments.
[0056] To better illustrate this application and facilitate understanding of its technical solutions, typical but non-limiting embodiments of this application are as follows: Example 1 This embodiment provides a method for preparing a gel composite electrolyte based on a metal complex, the method comprising the following steps: 20 mL of a 1.5 mol / L NaN(CN)₂ aqueous solution A was heated to 60 °C in a water bath. 10 mL of a 1.5 mol / L Cu(NO₃)₂ aqueous solution B was added dropwise to A while continuously stirring for 2 hours. After the reaction was complete, the mixture was cooled to room temperature and left undisturbed for five days. After filtration, the solution was washed with deionized water, and then the entire product was dried in a vacuum drying oven for 24 hours to obtain the Cu metal complex.
[0057] 0.5 g of Cu metal complex was soaked in 1 g of potassium-ion battery electrolyte (0.8 M KPF6 in DEC:EC = 1:1 Vol %, Suzhou Duoduo Chemical Technology Co., Ltd., trade name KP-001) for more than 10 h. Then, the soaked Cu metal complex was placed in a PVDF-HFP solution, which was prepared by dissolving 0.5 g of PVDF-HFP in 10 g of N-methylpyrrolidone. Then, 0.5 g of ETPTA monomer and 0.005 g of photoinitiator HMPP were added. The solution was stirred at 500 r / min for 5 h at room temperature to make it homogeneous. In-situ polymerization was carried out using ultraviolet light with a wavelength range of 365 nm to 400 nm, while the solution was stirred at 100 r / min for 2 h.
[0058] The mixed slurry after UV polymerization was coated onto a glass plate using a doctor blade with a thickness of 300 μm. It was then freeze-dried for 7 days at a temperature below -60℃ and a vacuum of -0.1 MPa. The resulting polymer film was then immersed in a potassium-ion battery electrolyte (0.8 M KPF6 in DEC:EC = 1:1 Vol %, Suzhou Duoduo Chemical Technology Co., Ltd., trade name KP-001) for 12 hours to obtain a potassium-ion battery gel composite electrolyte based on metal complexes.
[0059] The microstructure of the potassium-ion battery gel composite electrolyte is as follows: Figure 1 As shown, a test cell with stainless steel as the working electrode was assembled using this gel composite electrolyte. Cyclic voltammetry (CV) scans of the cell were performed at room temperature using a CHI600E electrochemical workstation. The results are as follows: Figure 2As shown, a solid-state potassium-ion CR2032 coin cell assembled using this gel composite electrolyte was subjected to cycle performance testing at room temperature using a LAND battery testing system. The test results are shown in [Figure number missing]. Figure 3 The battery was subjected to constant current charge-discharge testing at room temperature using the LAND battery testing system. The test results are shown in [Figure number missing]. Figure 4 .
[0060] Depend on Figure 1 It can be seen that the prepared gel composite electrolyte has a porous structure, and the metal complex is uniformly and stably doped in the polymer three-dimensional network structure, which can improve the mechanical strength of the electrolyte. This structure can effectively play the role of the composite polymer network in adsorbing organic molecules in the electrolyte, restricting the movement of anionic groups in the electrolyte, and reducing the negative impact of interfering with potassium ion migration.
[0061] Depend on Figure 2 The CV curve shows that there is no oxidation peak before 4V, indicating that the prepared potassium-ion battery gel composite electrolyte has good electrochemical stability and can be matched with cathode materials with charging voltage below 4V.
[0062] Depend on Figure 3 It can be seen that the solid potassium-ion secondary battery assembled based on the potassium-ion battery gel composite electrolyte prepared in Example 1 has good cycle stability and can effectively improve the cycle life of the solid potassium-ion battery.
[0063] Depend on Figure 4 The charge-discharge voltage-specific capacity curves of the solid-state potassium-ion battery at cycles 1, 10, 100, and 500 are shown. A high discharge specific capacity is achieved in the first discharge cycle, with the discharge plateau located at 2.2-2.3 V. Although the discharge specific capacity decreases with each cycle, and the charge-discharge voltage gap widens, exacerbating polarization, the discharge specific capacity only decreases by about 20 mAh / g after 500 cycles, indicating good stability of the battery during long-term cycling.
[0064] Example 2 This embodiment provides a method for preparing a gel composite electrolyte based on a metal complex, the method comprising the following steps: 20 mL of a 1.5 mol / L NaN(CN)₂ aqueous solution A was heated to 60 °C in a water bath. 10 mL of a 1.5 mol / L Co(NO₃)₂ aqueous solution B was added dropwise to A while continuously stirring for 2 hours. After the reaction was complete, the mixture was cooled to room temperature and left undisturbed for five days. After filtration, the solution was washed with deionized water, and then the entire product was dried in a vacuum drying oven for 24 hours to obtain the Co metal complex.
[0065] 0.5 g of Co metal complex was soaked in 1.5 g of potassium-ion battery electrolyte (0.8 M KPF6 in DEC:EC = 1:1 Vol %, Suzhou Duoduo Chemical Technology Co., Ltd., trade name KP-001) for more than 10 h. Then, the soaked Co metal complex was placed in a PVDF-HFP solution, which was prepared by dissolving 0.5 g of PVDF-HFP in 10 g of N,N-dimethylformamide. Then, 0.5 g of PETEA monomer and 0.005 g of photoinitiator HMPP were added. The solution was stirred at 500 r / min for 5 h at room temperature to make it homogeneous. In-situ polymerization was carried out using ultraviolet light with a wavelength range of 365 nm to 400 nm, while the solution was stirred at 100 r / min for 2 h.
[0066] The mixed slurry after UV polymerization was coated onto a glass plate using a doctor blade with a thickness of 300 μm. It was then freeze-dried for 7 days at a temperature below -60℃ and a vacuum of -0.1 MPa. The resulting polymer film was then immersed in a potassium-ion battery electrolyte (0.8 M KPF6 in DEC:EC = 1:1 Vol %, Suzhou Duoduo Chemical Technology Co., Ltd., trade name KP-001) for 12 hours to obtain a potassium-ion battery gel composite electrolyte based on metal complexes.
[0067] The microstructure of the potassium-ion battery gel composite electrolyte is as follows: Figure 5 As shown, a test cell with stainless steel as the working electrode was assembled using this gel composite electrolyte. Cyclic voltammetry (CV) scans of the cell were performed at room temperature using a CHI600E electrochemical workstation. The results are as follows: Figure 6 As shown, a solid-state potassium-ion CR2032 coin cell assembled using this gel composite electrolyte was subjected to cycle performance testing at room temperature using a LAND battery testing system. The test results are shown in [Figure number missing]. Figure 7 .
[0068] Depend on Figure 5 It can be seen that the prepared gel composite electrolyte has a porous structure, and the metal complex is uniformly and stably doped in the polymer three-dimensional network structure, which can improve the mechanical strength of the electrolyte. This structure can effectively play the role of the composite polymer network in adsorbing organic molecules in the electrolyte, restricting the movement of anionic groups in the electrolyte, and reducing the negative impact of interfering with potassium ion migration.
[0069] Depend on Figure 6 The CV curve shows that there is no oxidation peak before 4V, indicating that the prepared potassium-ion battery gel composite electrolyte has good electrochemical stability and can be matched with cathode materials with charging voltage below 4V.
[0070] Depend on Figure 7 It can be seen that the solid potassium-ion secondary battery assembled based on the potassium-ion battery gel composite electrolyte prepared in Example 2 has good cycle stability and can effectively improve the cycle life of the solid potassium-ion battery.
[0071] Example 3 This embodiment provides a method for preparing a gel composite electrolyte based on a metal complex, the method comprising the following steps: 20 mL of a 1.5 mol / L NaN(CN)₂ aqueous solution A was heated to 60 °C in a water bath. 10 mL of a 1.5 mol / L Cu(NO₃)₂ aqueous solution B was added dropwise to A while continuously stirring for 2 h. After the reaction was complete, the mixture was cooled to room temperature and left undisturbed for five days. After filtration, the solution was washed with deionized water, and then the entire product was dried in a vacuum drying oven for 24 h to obtain the Cu metal complex.
[0072] 0.5 g of Cu metal complex was soaked in 1 g of potassium-ion battery electrolyte (1 M KFSI in DEC:EC = 1:1 Vol%, Suzhou Duoduo Chemical Technology Co., Ltd., trade name KP-044) for more than 10 h. Then, the soaked Cu metal complex was placed in a PVDF-HFP solution, which was prepared by dissolving 0.5 g of PVDF-HFP in 10 g of N-methylpyrrolidone. Then, 0.5 g of PETEA monomer and 0.005 g of photoinitiator HMPP were added. The solution was stirred at 500 r / min for 5 h at room temperature to make it homogeneous. In-situ polymerization was carried out using ultraviolet light with a wavelength range of 365 nm to 400 nm, while the solution was stirred at 100 r / min for 2 h.
[0073] The mixed slurry after UV polymerization was coated onto a glass plate using a doctor blade with a thickness of 300 μm. It was then freeze-dried for 7 days at a temperature below -60℃ and a vacuum of -0.1 MPa. The resulting polymer film was then immersed in a potassium-ion battery electrolyte (1M KFSI in DEC:EC=1:1 Vol %, Suzhou Duoduo Chemical Technology Co., Ltd., trade name KP-044) for 12 hours to obtain a potassium-ion battery gel composite electrolyte based on metal complexes.
[0074] The microstructure of the potassium-ion battery gel composite electrolyte is as follows: Figure 8As shown, a test cell with stainless steel as the working electrode was assembled using this gel composite electrolyte. Cyclic voltammetry (CV) scans of the cell were performed at room temperature using a CHI600E electrochemical workstation. The results are as follows: Figure 9 As shown, a solid-state potassium-ion CR2032 coin cell assembled using this gel composite electrolyte was subjected to cycle performance testing at room temperature using a LAND battery testing system. The test results are shown in [Figure number missing]. Figure 10 .
[0075] Depend on Figure 8 It can be seen that the prepared gel composite electrolyte has a porous structure, and the metal complex is uniformly and stably doped in the polymer three-dimensional network structure, which can improve the mechanical strength of the electrolyte. This structure can effectively play the role of the composite polymer network in adsorbing organic molecules in the electrolyte, restricting the movement of anionic groups in the electrolyte, and reducing the negative impact of interfering with potassium ion migration.
[0076] Depend on Figure 9 The CV curve shows that there is no oxidation peak before 4V, indicating that the prepared potassium-ion battery gel composite electrolyte has good electrochemical stability and can be matched with cathode materials with charging voltage below 4V.
[0077] Depend on Figure 10 It can be seen that the solid potassium-ion secondary battery assembled based on the potassium-ion battery gel composite electrolyte prepared in Example 3 has good cycle stability and can effectively improve the cycle life of the solid potassium-ion battery.
[0078] Example 4 This embodiment provides a method for preparing a gel composite electrolyte based on metal complexes. Compared with Example 1, the only difference is that freeze drying is replaced by vacuum drying. Specifically, vacuum drying is performed at 60°C for 12 hours under a vacuum with an absolute pressure of 180 Pa.
[0079] The microstructure of the potassium-ion battery gel composite electrolyte is as follows: Figure 11 As shown. By Figure 11 It can be seen that the porous structure of the obtained gel composite electrolyte is significantly reduced, which is not conducive to the movement of anionic groups in the electrolyte and is not conducive to the optimization of cycle performance and electrochemical performance.
[0080] Example 5 This embodiment provides a method for preparing a gel composite electrolyte based on metal complexes. Compared with Example 1, the only difference is that the mass of the Cu metal complex used for anchoring is reduced from 0.5g to 0.05g.
[0081] A test cell with a stainless steel working electrode was assembled using this gel composite electrolyte. Cyclic voltammetry (CV) scans of the cell were performed at room temperature using a CHI600E electrochemical workstation. The results are as follows: Figure 12 As shown. Figure 12 The middle image shows the CV curve of the battery during the first three cycles of testing, with a test voltage range of -1. 4V. During the negative scan, a significant reduction current was observed below 0V, corresponding to the potassium deposition process, with the highest reduction current amplitude in the first scan. During the positive scan, an oxidation peak appeared near 0V, representing the potassium stripping process. No significant oxidation current was observed within the 4V voltage range. The CV curves of the second and third cycles largely overlapped, indicating that the battery reaction exhibited good cycle reversibility after the initial activation cycle.
[0082] Comparative Example 1 This comparative example provides a method for preparing a gel composite electrolyte. Compared with Example 1, the only difference is that the metal complex is completely omitted. That is, the PVDF-HFP solution, ETPTA monomer and photoinitiator HMPP are directly mixed evenly, and in-situ polymerization is carried out using ultraviolet light. The mixture is then coated on a glass plate, freeze-dried to obtain a polymer film, and then immersed in potassium ion battery electrolyte again to obtain a gel composite electrolyte.
[0083] A solid-state potassium-ion CR2032 coin cell assembled using this gel composite electrolyte was subjected to cycle performance testing at room temperature using a LAND battery testing system. The test results are shown below. Figure 13 .Depend on Figure 13 It can be seen that the cycle stability of the solid potassium-ion secondary battery assembled based on the potassium-ion battery gel composite electrolyte prepared in Comparative Example 1 is significantly reduced.
[0084] Comparative Example 2 This comparative example provides a method for preparing a gel composite electrolyte. The only difference from Example 1 is that the prepared metal complex is directly anchored without being pre-soaked in potassium-ion battery electrolyte.
[0085] A solid-state potassium-ion CR2032 coin cell assembled using this gel composite electrolyte was subjected to cycle performance testing at room temperature using a LAND battery testing system. The test results are shown below. Figure 14 .Depend on Figure 14 It can be seen that the cycle stability of the solid potassium-ion secondary battery assembled based on the potassium-ion battery gel composite electrolyte prepared in Comparative Example 2 is significantly reduced, especially in the first 50 cycles. Although the coulombic efficiency remains good, the charge specific capacity and discharge specific capacity show a significant downward trend.
[0086] In summary, the alkali metal ion battery gel composite electrolyte based on metal complexes prepared in this application uses readily available raw materials with low toxicity. Furthermore, the preparation process is simple, low-cost, and easy to implement. The alkali metal ion battery gel composite electrolyte based on metal complexes prepared in this application has advantages such as wide applicability, high mechanical strength, long cycle life, and stable electrochemical performance, making it suitable for application in secondary solid-state alkali metal ion batteries.
[0087] This application illustrates its detailed structural features through the above embodiments, but it is not limited to these detailed structural features, meaning that this application does not necessarily rely on them for implementation. Those skilled in the art should understand that any improvements to this application, equivalent substitutions of selected components, additions of auxiliary components, and selection of specific methods all fall within the protection and disclosure scope of this application.
[0088] The preferred embodiments of this application have been described in detail above. However, this application is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this application, various simple modifications can be made to the technical solution of this application, and these simple modifications all fall within the protection scope of this application.
[0089] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this application will not describe the various possible combinations separately.
[0090] Furthermore, various different implementations of this application can be combined in any way, as long as they do not violate the spirit of this application, they should also be regarded as the content disclosed in this application.
Claims
1. A method for preparing a gel composite electrolyte based on a metal complex, characterized in that, The preparation method includes the following: The metal complex was immersed in an electrolyte, and then subjected to solid-liquid separation to obtain the immersed metal complex. The soaked metal complex is anchored in a semi-interpenetrating three-dimensional polymer network formed by in-situ polymerization of PVDF-HFP and acrylate monomers to obtain a polymer film. The polymer film is immersed in the electrolyte to obtain a gel composite electrolyte based on metal complexes.
2. The preparation method according to claim 1, characterized in that, The metal complex was prepared by the following method: an aqueous solution A of NaN(CN)2 was heated, and an aqueous solution B of a metal nitrate was added dropwise while stirring. The mixture was cooled to room temperature, allowed to stand, and then subjected to solid-liquid separation, washing, and drying to obtain the metal complex.
3. The preparation method according to claim 2, characterized in that, Satisfy at least one of the following (1) to (6): (1) The metal nitrate includes at least one of Co(NO3)2, Zn(NO3)2 and Cu(NO3)2; (2) The NaN(CN)2 concentration of the aqueous solution A is the same as the metal nitrate concentration of the aqueous solution B, which is 1.3~1.7 mol / L; (3) Based on the fact that the weight of aqueous solution A is 100, the weight of aqueous solution B is 40~60. (4) The target temperature for heating is 50~70℃; (5) The settling time is more than 5 days; (6) The drying process includes drying in a vacuum drying oven for more than 24 hours.
4. The preparation method according to claim 1, characterized in that, The metal complex is immersed in the electrolyte for more than 10 hours; And / or, based on 100 parts by weight of the metal complex, the electrolyte is 100 to 150 parts by weight.
5. The preparation method according to claim 1, characterized in that, The anchoring process includes the following steps: uniformly mixing the soaked metal complex with PVDF-HFP solution, acrylate monomers, and photoinitiator, performing in-situ polymerization using ultraviolet light, coating it onto a glass plate, and freeze-drying it to obtain the polymer film.
6. The preparation method according to claim 5, characterized in that, The solvent of the PVDF-HFP solution includes at least one of N-methylpyrrolidone, N,N-dimethylformamide and dimethyl sulfoxide; And / or, in the PVDF-HFP solution, the weight ratio of PVDF-HFP to solvent is 1:(10~20); And / or, based on 100 parts by weight of acrylate monomers, the PVDF-HFP in the PVDF-HFP solution is 100-200 parts by weight, the photoinitiator is 1-3 parts by weight, and the metal complex is 10-100 parts by weight. And / or, the acrylate monomers include at least one of ethoxylated trimethylolpropane triacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipropylene glycol diacrylate; And / or, the photoinitiator includes HMPP.
7. The preparation method according to claim 5, characterized in that, Satisfy at least one of the following (7) to (12): (7) The uniform mixing includes: stirring at a speed of 500~600r / min for 2~5h at room temperature; (8) The wavelength range of the ultraviolet light is 365nm~400nm; (9) The in-situ polymerization process is accompanied by stirring, and the stirring speed is 100~200 r / min; (10) The in-situ polymerization time is 1~2 hours; (11) The coating thickness on the glass plate is 100~300μm; (12) The freeze-drying temperature is -60℃, the vacuum degree is -0.1Mpa, and the time is 7~10 days.
8. The preparation method according to claim 1, characterized in that, Based on 100 parts by weight of polymer film, the amount of electrolyte required for immersion is 200-300 parts by weight. And / or, the polymer film is immersed in the electrolyte for more than 12 hours.
9. A gel composite electrolyte based on a metal complex, characterized in that, The preparation method described in any one of claims 1 to 8 is used; wherein, in the metal complex-based gel composite electrolyte, the weight parts of the semi-interpenetrating three-dimensional polymer network formed by in-situ polymerization of PVDF-HFP and acrylate monomers are 100 to 300, and the weight parts of the electrolyte adsorbed by soaking are 100 to 500, based on the weight parts of the metal complex being 100.
10. An application of a gel composite electrolyte based on a metal complex, characterized in that, A gel composite electrolyte based on a metal complex is prepared by any one of the preparation methods described in claims 1 to 8, wherein the electrolyte used in the preparation method is a potassium-ion battery electrolyte and is used as a solid electrolyte for potassium-ion batteries.