A shuttle-resistant dendrite-inhibiting composite gel electrolyte and zinc-ion battery

By introducing PDAC-modified PAM gel electrolyte into zinc-iodine batteries, the problems of polyiodine ion shuttle and zinc dendrite growth are solved, achieving high cycle stability and safety of zinc-ion batteries, which are suitable for wearable devices and flexible electronic devices.

CN123073162APending Publication Date: 2026-11-10CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611344383.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing zinc-iodine batteries suffer from problems such as polyiodine ion shuttle and zinc dendrite growth, leading to short circuits and reduced cycle life. Existing technologies also suffer from the problem of small molecule additives being prone to ionization and loss, and the complex and costly processes involving zwitterionic and deep eutectic solvent systems.

Method used

By introducing the quaternary ammonium salt polymer polydimethyldiallylammonium chloride (PDAC) into polyacrylamide (PAM) gel, an anti-shuttle dendrite-inhibiting composite gel electrolyte is formed. This optimizes the three-dimensional network structure of the gel and the electrode interface environment. The long-chain structure of PDAC and the electrostatic interaction with the quaternary ammonium cations inhibit polyiodide ion shuttle and zinc dendrite growth.

Benefits of technology

It improves the cycle stability, safety, and rate performance of zinc-ion batteries, suppresses zinc dendrite growth and polyiodine ion shuttle effect, and enhances battery flexibility and ionic conductivity, making it suitable for wearable devices and flexible electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073162A_ABST
    Figure CN123073162A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of aqueous energy storage battery technology and discloses an anti-shutdown and dendrite-suppressing composite gel electrolyte and a zinc-ion battery. Addressing the problems of cycle life degradation caused by polyiodide ion shuttle and zinc dendrite growth in existing aqueous zinc-iodine batteries, as well as the complex modification process and easy loss, this invention provides a cross-linked gel electrolyte with polyacrylamide as the three-dimensional network framework and a trace amount of polydimethyldiallylammonium chloride (PDAC) composited in the form of acrylamide monomer to PDAC at a mass ratio of 1:0.001225–0.0049. This invention eliminates the need for complex eutectic solvents and utilizes the quaternary ammonium cations on the long chain of polymeric PDAC to both electrostatically anchor polyiodide anions in situ to suppress shuttle and adsorb onto the zinc anode surface to generate electrostatic shielding to suppress zinc dendrites. This battery has a simple fabrication process, high ionic conductivity, excellent flexibility, and ultra-long cycle life, making it highly promising for application in the field of flexible energy storage devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of energy storage technology, specifically to a zinc-ion battery based on an anti-shuttle dendrite-suppressing composite gel electrolyte. This battery not only possesses high safety, excellent rate performance, and ultra-long cycle life, but also achieves functional modification of the gel electrolyte and precise interface control, providing a new technical solution for flexible, highly stable, and long-life aqueous energy storage devices. Background Technology

[0002] In recent years, renewable energy and flexible electronics have developed rapidly, making high-safety, low-cost, and long-life energy storage technologies a key research focus. Aqueous zinc-ion batteries, due to their abundant resources, high safety, and environmental friendliness, have become a research hotspot for next-generation energy storage systems. Among them, zinc-iodine batteries possess advantages such as redox potential matching, stable capacity, and low cost, making them highly promising for application in the field of flexible energy storage.

[0003] However, zinc-iodine batteries face two major bottlenecks in practical applications: first, the zinc anode is prone to dendrite growth, hydrogen evolution, and corrosion side reactions, leading to short circuits and a significant decrease in cycle life; second, the iodine cathode generates polyiodide ions (I3+) during charging and discharging. - I5 - It is easy to dissolve and diffuse, causing a serious shuttle effect, resulting in loss of active materials, serious self-discharge, and reduced coulombic efficiency.

[0004] Gel electrolytes are an effective way to solve the above problems. Polyacrylamide (PAM)-based gels have good flexibility, strong ionic conductivity, and good compatibility with electrodes, but pure PAM gels are difficult to suppress polyiodide ion shuttle, provide insufficient protection for the zinc anode interface, and their ionic conductivity and mechanical properties still need to be improved. Currently, in order to improve the electrolyte's ability to resist shuttle and suppress dendrites, existing technologies mainly adopt the following methods: one is to introduce small molecule cationic additives with strong adsorption effects. For example, existing research, such as the literature "Cation Adsorption Engineering Enables Dual Stabilizations for Fast-Charging Zn-I2 Batteries", proposes a trimethylsulfonium cation (TMS) with strong adsorption effects. + Additives are used to stabilize the electrode. This technology utilizes TMS. + The strong interaction with polyiodides immobilizes a large amount of iodine in the form of oil-phase precipitation to avoid the shuttle effect, while TMS +Preferential adsorption on the zinc anode crystal surface generates electrostatic shielding to suppress dendrite formation. However, under long-term charge-discharge cycles and electric field effects, this small molecule additive is prone to free diffusion, migration, and eventual loss within the gel network, making it difficult to maintain long-term stability. Furthermore, the oil-phase precipitation mechanism of iodine may increase the ion transport resistance at the electrode or electrolyte interface, adversely affecting kinetics. Secondly, complex dual-network eutectic gel electrolyte systems are constructed. For example, the literature "Molecularly engineered dual-network eutectogel electrolytes for high-loading and stable zinc–iodine batteries" discloses a dual-network gel electrolyte prepared by in-situ polymerization of poly(N-hydroxyethylacrylamide) and zwitterionic polymers (PDMAPS) in a deep eutectic solvent. In this type of system, the deposition of zinc ions is regulated by the local electrostatic field generated by different groups in the zwitterionic polymer, which is controlled by quaternary ammonium salt groups (-NR). 4+ This type of system is responsible for anchoring polyiodide ions. However, it relies on complex deep eutectic solvents (DES), has a complicated and costly preparation process, and the synthesis of bifunctional groups is difficult, which hinders its large-scale application.

[0005] Based on the above background, the technical problem this invention aims to solve is how to address the issues of easy leaching and loss of small molecule additives, and the complex and costly processes of zwitterionic and deep eutectic solvent systems in existing technologies. This invention proposes a zinc-ion battery with an anti-shuttle dendrite-inhibiting composite gel electrolyte. By functionalizing the PAM gel with quaternary ammonium salt polymers, the three-dimensional network structure of the gel and the electrode interface environment are optimized, improving the battery's cycle stability, safety, and rate performance, thus providing a new path for the development of high-performance zinc-ion batteries. Summary of the Invention

[0006] To address the problems in the prior art, this invention provides a zinc-ion battery with an anti-shuttle and dendrite-suppressing composite gel electrolyte, aiming to overcome the technical challenges of polyiodine ion shuttle and zinc dendrite growth in existing zinc-iodine batteries. This invention utilizes an aqueous in-situ polymerization process, leveraging the functional groups of quaternary ammonium salt polymers to achieve anti-shuttle and dendrite-suppressing effects while maintaining excellent flexibility and ionic conductivity.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] A shuttle-resistant and dendrite-inhibiting composite gel electrolyte is disclosed. The composite gel electrolyte uses polyacrylamide (PAM) as a three-dimensional network hydrogel framework, in which a long-chain polymer containing quaternary ammonium cations, polydimethyldiallyl ammonium chloride (PDAC), is composited. Through a specific mass ratio and network structure, it achieves shuttle-resistant and dendrite-inhibiting functions. The composite gel electrolyte also contains an aqueous solution of zinc sulfate at a concentration of 1.5–2.5 mol / L.

[0009] Furthermore, in the composite gel electrolyte, the mass ratio of acrylamide monomer of polyacrylamide (PAM) to PDAC is 1:0.001 to 0.005. Preferably, it is 1:0.001225 to 0.0049.

[0010] As a preferred option, the PDAC used is a 30-35 wt.% aqueous solution with a molecular weight Mw < 100,000.

[0011] This invention also provides a method for preparing an anti-shuttle dendrite-inhibiting composite gel electrolyte, comprising the following steps:

[0012] (1) Raw material preparation: Weigh acrylamide monomer and PDAC at a mass ratio of 1:0.001225 to 0.0049, and prepare a zinc sulfate aqueous solution with a concentration of 1.5 to 2.5 mol / L as the electrolyte matrix;

[0013] (2) Add acrylamide monomer and PDAC to zinc sulfate aqueous solution and stir to form a homogeneous mixture; then add initiator and crosslinking agent in sequence; under constant temperature stirring conditions, allow the mixture to undergo in-situ free radical polymerization to form a semi-interpenetrating / crosslinked network composite gel;

[0014] The crosslinking agent is N,N'-methylenebisacrylamide, and the initiator is ammonium persulfate. The mass ratio of the crosslinking agent to the acrylamide monomer is 1:1000 to 1:3000; the mass ratio of the initiator to the acrylamide monomer is 0.005:1 to 0.015:1. The mass (g) ratio of the acrylamide monomer to the volume (mL) of the zinc sulfate aqueous solution is 1g:2.5 to 4.5mL.

[0015] (3) Post-treatment: The polymerized mixture is injected into a mold and placed in a drying oven at 55~75℃ for 3~4 hours to complete cross-linking and curing, thus obtaining the anti-shuttle dendrite composite gel electrolyte.

[0016] This invention modifies PAM electrolyte using PDAC, an interface modifier that can form a stable electrostatic interaction with zinc ions, thereby improving battery cycle life and inhibiting zinc dendrite growth. PDAC is preferentially adsorbed on the zinc anode surface to form an ordered ion-conducting interface layer, which effectively inhibits hydrogen evolution reaction and zinc corrosion.

[0017] A method for preparing a zinc-ion battery with a shuttle-resistant dendrite-suppressing composite gel electrolyte, wherein the battery is assembled as follows: a positive electrode material containing an iodine-carbon composite, zinc as a negative electrode material, and a composite gel electrolyte are sequentially assembled into a sandwich structure and encapsulated in a button cell or flexible cell.

[0018] Preferably, the active component of the positive electrode is an iodine-carbon composite (iodine to carbon in a mass ratio of 1:1, wherein the carbon is activated carbon AC); the positive electrode is composed of an iodine-carbon composite, a conductive agent (acetylene black), and a binder (polyvinylidene fluoride PVDF) mixed in a mass ratio of 8:1:1, with the addition of a solvent (N... - methyl - 2 - Pyrrolidone is thoroughly ground in a ceramic mortar to form a uniform slurry, then evenly coated onto the current collector, dried in a vacuum drying oven, and pressed into tablets to obtain the positive electrode.

[0019] Preferably, the battery is externally packaged as a button cell casing or a flexible aluminum-plastic film casing.

[0020] The beneficial effects of this invention are as follows:

[0021] (1) The PDAC selected in this invention has a long polymer chain structure. During polymerization, the PDAC long chains can be firmly inserted and anchored in the PAM gel backbone, avoiding loss during the recycling process. The quaternary ammonium cations on the PDAC chains interact electrostatically to hold polyiodide anions (I3) inside the gel. - I5 - It is firmly adsorbed, forming an ion sieving barrier, which effectively blocks the shuttle effect, reduces the self-discharge rate of the battery, and improves the utilization rate of iodine.

[0022] (2) The composite gel electrolyte prepared in this invention can improve the interfacial microenvironment of the zinc anode. The cationic groups in the PDAC can homogenize the concentration distribution of zinc ions at the anode interface through electrostatic adsorption, guiding the zinc ions to deposit smoothly and uniformly. This interface regulation effectively inhibits the nucleation and growth of zinc dendrites, significantly reduces the risk of internal short circuits in the battery, and improves cycle life.

[0023] (3) In the composite gel electrolyte prepared by this invention, hydrogen bonds and dipole interactions can be generated between the amide groups in the PAM molecular chain and PDAC, making the PAM three-dimensional network more compact and stable. This cross-linked network improves the water retention capacity of the gel on the one hand, and forms a continuous transport channel for zinc ions on the other. The two work together to reduce the resistance to ion transport, resulting in a higher ionic conductivity of the composite gel electrolyte.

[0024] (4) The hydrogel based on PAM in this invention produces an electrolyte with excellent mechanical properties and interfacial adhesion. Even when the battery is subjected to external forces and undergoes bending or deformation, the composite gel electrolyte can still maintain the integrity of its three-dimensional network structure and will not experience brittleness or leakage. This ensures the power supply stability of the battery in a flexible state. Combined with the high safety of the aqueous electrolyte itself, it is suitable for applications such as wearable devices and flexible electronic devices. Attached Figure Description

[0025] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein:

[0026] Figure 1 Electrochemical impedance spectroscopy for different electrolyte types;

[0027] Figure 2 A comparison chart of the ionic conductivity of different electrolytes;

[0028] Figure 3 Tafel corrosion curves for different electrolytes;

[0029] Figure 4 SEM and XRD patterns of zinc anode deposition morphology and crystal orientation for different electrolytes;

[0030] Figure 5 CA graph for different electrolyte addition amounts;

[0031] Figure 6 For iodine-carbon composite cathodes at 5 A·g -1 Cyclic performance graph;

[0032] Figure 7 The in-situ Raman spectroscopy characterization of polyiodide ion shuttle suppression diagram;

[0033] Figure 8 Self-discharge diagrams for different electrolytes;

[0034] Figure 9 Illustrations showing a small light bulb lit up by a PAM / PDAC electrolyte pouch battery at different folding angles;

[0035] Figure 10 A comparative CA graph showing the differences between different types of quaternary ammonium salt additives;

[0036] Figure 11 Comparative CA plots showing the evolution of electrochemical performance caused by excessive addition of high-concentration PDAC;

[0037] Figure 12 A comparison of the electrochemical stability window (LSV) of different types of gel substrates. Detailed Implementation

[0038] Example 1: Preparation of PAM / PDAC composite gel electrolyte and battery assembly

[0039] 1. Electrolyte preparation:

[0040] Raw material preparation: Weigh 3g of acrylamide monomer and 30 μL of PDAC as the main component of the electrolyte. The PDAC used is a 35wt.% aqueous solution with a molecular weight Mw<100000 and a density of about 1.05 g / mL.

[0041] Mixing and Polymerization: The above raw materials were added to a beaker, and 10 mL of 2 mol / L zinc sulfate electrolyte was added and stirred at high speed to form a homogeneous mixture. Then, under heating conditions of 65°C, 30 mg of ammonium persulfate initiator and 1.5 mg of N,N'-methylenebisacrylamide crosslinking agent were added and stirred continuously to allow the mixture to undergo in-situ free radical polymerization to form a three-dimensional network gel electrolyte. The mixture was then poured into a mold.

[0042] Post-processing: The obtained mold was placed in a forced-air drying oven (65℃) and dried at a constant temperature for 3.5 hours to complete the curing and obtain the anti-shuttle dendrite composite gel electrolyte.

[0043] The composite gel electrolyte prepared in Example 1 has an ionic conductivity of 25.51 mS / cm.

[0044] 2. Cathode preparation:

[0045] Raw material preparation: Iodine and carbon were mixed evenly at a mass ratio of 1:1, placed in a reaction vessel, and kept at 120℃ for 10 h. After cooling, iodine-carbon composite cathode material was obtained.

[0046] Positive electrode preparation: Iodine-carbon composite (320 mg), conductive agent acetylene black (40 mg), and binder PVDF (40 mg) were mixed in a mass ratio of 8:1:1, and an appropriate amount of N was added. - methyl - 2 - Pyrrolidone was thoroughly ground into a uniform slurry in a ceramic mortar, then evenly coated onto a carbon cloth current collector, and thoroughly dried in a vacuum drying oven to obtain a positive electrode sheet.

[0047] 3. Anode preparation:

[0048] Material selection: High-purity zinc sheets are selected as the negative electrode.

[0049] Post-processing: The zinc foil is ultrasonically cleaned with ethanol and dried to ensure that the surface is clean and free of impurities.

[0050] 4. Battery assembly:

[0051] Structure: The prepared positive electrode, negative electrode and gel electrolyte are assembled into a sandwich structure in sequence and then encapsulated in a button cell case.

[0052] Sealing: Mechanical stamping encapsulation ensures no internal leakage and good contact within the battery. For example... Figure 9 As shown, the PAM / PDAC gel electrolyte exhibits excellent flexibility and structural integrity. The assembled pouch battery can stably light up an LED bulb even when repeatedly folded and bent at angles from 0° to 180° without any internal open circuits or leakage.

[0053] 5. Performance Testing:

[0054] The assembled battery underwent zinc anode deposition and corrosion performance testing to observe the effect of the electrolyte on the zinc anode's regulation. The assembled battery then underwent zinc anode corrosion resistance testing. Figure 3 The Tafel polarization curves are shown. Compared with pure PAM gel electrolyte, the zinc anode using PAM / PDAC composite gel electrolyte exhibits a more positive corrosion potential and a lower corrosion current.

[0055] Figure 4 SEM and XRD patterns of zinc anode deposition morphology and crystal orientation for different electrolytes are shown. Figure 4 The modified composite electrolyte can guide the uniform deposition of zinc ions and effectively inhibit dendrite growth. Anti-shuttle performance testing: The assembled battery was tested using in-situ Raman spectroscopy to monitor the migration behavior of polyiodide ions during charging and discharging in real time, evaluating the electrolyte's suppression effect on the shuttle effect. Changes in the intensity of polyiodide ion characteristic peaks were recorded during the test to analyze the degree of diffusion. Figure 7 The in-situ Raman spectroscopy characterization of polyiodide ion shuttle inhibition shows that the composite gel can anchor polyiodide anions by electrostatic interaction, significantly reducing the loss of active substances.

[0056] Self-discharge test: such as Figure 8 As shown, after a fully charged battery is left to stand for 24 hours, the capacity retention rate of the pure PAM battery is only 87.27%, indicating severe self-discharge caused by shuttle. However, the capacity retention rate of the battery using PAM / PDAC composite gel electrolyte reaches 92% after 24 hours of standing, demonstrating its anti-shuttle capability.

[0057] Example 2: Preparation and battery performance optimization of composite gel electrolytes modified with different amounts of additives

[0058] 1. Electrolyte modification:

[0059] Raw material preparation: Based on Example 1, different volumes of PDAC solution were added to the electrolyte, and other operations were the same as in Example 1.

[0060] Mixing and Polymerization: Mixing and polymerization were carried out according to the steps of Example 1, but different amounts of PDAC needed to be uniformly dispersed in the raw materials before adding the initiator and crosslinking agent. Specifically, 3g of acrylamide monomer was added to a beaker, and 10mL of 2mol / L zinc sulfate electrolyte was added and stirred at high speed to form a homogeneous mixture. Then, 10 μL, 20 μL, 30 μL, and 40 μL of PDAC solution were added respectively. Under heating at 65°C, ammonium persulfate initiator and N,N'-methylenebisacrylamide crosslinking agent were added and stirred continuously to allow the mixture to undergo in-situ free radical polymerization to form a three-dimensional network gel electrolyte. The mixture was then poured into a mold.

[0061] Post-processing: Same as in Example 1, electrolytes modified with different amounts of PDAC were prepared.

[0062] 2. Battery assembly:

[0063] Assembly: Assemble the battery according to the steps in Example 1.

[0064] 3. Performance Testing:

[0065] Electrochemical workstation testing: The effect of different PDAC addition amounts on zinc ion deposition behavior was tested using chronoamperometry (CA). From Figure 5 It can be seen that compared with pure PAM electrolyte without PDAC, the zinc deposition current decays faster after adding PDAC, indicating that the zinc ion deposition kinetics are improved. Among them, the electrolyte with 30 μL of PDAC shows the fastest current stabilization, indicating that it has the best effect on regulating the uniform deposition of zinc ions.

[0066] Example 3:

[0067] 1. Electrolyte modification:

[0068] Raw material preparation: The optimal formulation determined in Example 2 was used, namely, PAM / PDAC composite gel electrolyte with a PDAC addition amount of 30 μL.

[0069] Mixing and polymerization: Mixing and polymerization were carried out according to the steps of Example 1.

[0070] Post-processing: Same as in Example 1, 30 μL of PAM / PDAC composite gel electrolyte was prepared.

[0071] 2. Battery assembly and testing:

[0072] Assembly: The battery was assembled using different amounts of additives according to the steps of Example 1.

[0073] Cyclic testing: Long-term cycle performance testing was conducted on assembled zinc-iodine batteries with different gel electrolytes. Figure 6 For zinc-iodine batteries at 5A g -1 Cyclic performance at high current density. The graph shows that the battery using pure PAM electrolyte (orange curve) has a low initial specific capacity and exhibits significant capacity decay during cycling. In contrast, the battery using PAM / PDAC composite gel electrolyte (blue curve) demonstrates superior cycle stability, maintaining a high specific capacity even after 30,000 ultra-long cycles, while its coulombic efficiency remains close to 100%. This clearly demonstrates that the introduction of PDAC can improve the cycle life and reversibility of zinc-iodine batteries.

[0074] Example 4: Effect of Optimal Additive Content Composite Gel Electrolyte on Battery Interfacial Impedance

[0075] The electrolyte used in the battery in Example 4 is the modified electrolyte with the optimal addition amount determined in Example 3 (i.e., PAM / PDAC composite gel electrolyte with a PDAC addition amount of 30 μL).

[0076] 1. Cathode preparation:

[0077] Raw material preparation: Prepare according to the steps in Example 1.

[0078] Electrode preparation: The positive electrode was prepared according to the steps in Example 1.

[0079] 2. Negative electrode preparation: Same as in Example 1.

[0080] 3. Battery assembly and testing:

[0081] Assembly: Same as in Example 1.

[0082] Performance testing: The effects of different electrolytes on the battery interfacial impedance were compared using electrochemical impedance spectroscopy (EIS). The results are as follows: Figure 1 As shown in the figure, the battery using pure PAM electrolyte (orange curve) exhibits a larger impedance semicircle, indicating a higher interfacial resistance. In contrast, the battery using PAM / PDAC composite gel electrolyte (blue curve) shows a smaller impedance semicircle, indicating a lower interfacial resistance. This demonstrates that the introduction of PDAC effectively optimizes the electrode / electrolyte interface and promotes ion transport. Figure 2 It can be seen that the composite gel electrolyte with 30 μL of PDAC can achieve an ionic conductivity of 25.51 mS / cm, which is higher than that of pure PAM (18.72 mS / cm). This indicates that PDAC and PAM synergistically construct an ion transport channel.

[0083] Comparative Example 1

[0084] The difference between Comparative Example 1 and Example 1 is that PDAC was not added to the raw materials for electrolyte preparation; only acrylamide monomer was used. All other operations were the same as in Example 1, resulting in the preparation of pure PAM gel electrolyte.

[0085] Comparative Example 1: The pure PAM electrolyte prepared had an ionic conductivity of 18.72 mS / cm.

[0086] To further investigate the effect of PDAC introduction on the ionic conductivity of PAM, EIS was used to test different gel electrolytes, such as... Figure 1 , 2 As shown in the figure. The results indicate that adding PDAC can optimize the electrode / electrolyte interface, suppress side reactions, construct efficient ion transport channels, reduce obstacles in the ion transport process, and improve ion conductivity.

[0087] Comparative Example 2

[0088] Compared with Example 1, the only difference is that the amount of PDAC added is 100 μL, 150 μL, 200 μL, and 300 μL, while the other operations are the same as in Example 1.

[0089] Test results are as follows Figure 11 As shown, when the amount of PDAC added is too large, the electrochemical performance not only does not improve, but actually decreases due to the excessive positive charge repulsion of the polymer and the decrease in compatibility.

[0090] Comparative Example 3:

[0091] Replace the polymeric quaternary ammonium salt PDAC in Example 1 with an equal mass of a small molecule quaternary ammonium salt: hexadecyltrimethylammonium bromide (CTAB), tetraethylammonium chloride (TEAC), or dodecyltrimethylammonium chloride (DTAC), while keeping all other steps exactly the same.

[0092] The results are as follows Figure 10 As shown, the CA curve of the small molecule quaternary ammonium salt is decaying and unstable. This indicates that the small molecule quaternary ammonium salt cannot form a semi-interpenetrating cross-linked network with the PAM backbone like the long-chain polymer PDAC. Under the action of a long-term electric field, it is prone to diffusion, ionization, and loss, and cannot maintain a long-term electrostatic shielding layer on the zinc anode surface. Therefore, it cannot continuously suppress the growth of zinc dendrites.

[0093] Comparative Example 4: Compared with Example 1, the difference is that the gel substrate was replaced with polyvinyl alcohol (PVA), while the other components and amounts remained unchanged, and a PVA / PDAC composite gel was prepared.

[0094] PVA powder was dissolved in deionized water and heated and stirred until completely dissolved. Then, a PDAC solution of the same proportion as in Example 1 and a zinc sulfate electrolyte of the same concentration were added. After mixing evenly, the mixture was poured into a mold, and a physical cross-linking method of repeated freeze-thaw cycles was used to obtain a PVA / PDAC composite gel electrolyte.

[0095] The electrochemical stability windows of the two electrolytes were determined using linear sweep voltammetry (LSV), with a voltage scan range of -0.5V to 3.0V. The test results are as follows: Figure 12 As shown, when using the PVA / PDAC composite gel, the cathode hydrogen evolution potential is more positive, and the anodic oxidation decomposition potential is more negative, resulting in a narrower overall electrochemical stability window. The PAM / PDAC composite gel electrolyte of this invention has a wider electrochemical stability window, and no side reaction currents such as water decomposition occur over a wider voltage range.

[0096] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A shuttle-resistant and dendrite-inhibiting composite gel electrolyte, characterized in that: The composite gel electrolyte uses polyacrylamide as the gel backbone, and polyacrylamide and polydiallyl ammonium chloride (PDAC) are combined to form a semi-interpenetrating and cross-linked network. In the composite gel electrolyte, the mass ratio of acrylamide monomer before polymerization to polydimethyldiallylammonium chloride is 1:0.001-0.005; the composite gel electrolyte also contains an aqueous solution of zinc sulfate.

2. The anti-shuttle dendrite-inhibiting composite gel electrolyte according to claim 1, characterized in that: The molecular weight of the PDAC is Mw < 100,000; the concentration of the zinc sulfate aqueous solution is 1.5~2.5 mol / L.

3. A method for preparing an anti-shuttle dendrite-inhibiting composite gel electrolyte according to claim 1 or 2, characterized in that, Includes the following steps: (1) Weigh acrylamide monomer and polydimethyldiallylammonium chloride (PDAC) at a mass ratio of 1:0.001225 to 0.0049, and prepare an aqueous solution of zinc sulfate as the electrolyte matrix; (2) Acrylamide monomer and PDAC are added to the zinc sulfate aqueous solution and stirred to form a homogeneous mixture; then the initiator and crosslinking agent are added in sequence; under constant temperature stirring conditions, the mixture undergoes in-situ free radical polymerization to form a crosslinked network composite gel; (3) The polymerized mixture is injected into a mold and heated in a forced-air drying oven at 55~75℃ for 3~4 hours to complete the cross-linking and curing, thus obtaining the anti-shuttle dendrite composite gel electrolyte.

4. The preparation method of the anti-shuttle dendrite-inhibiting composite gel electrolyte according to claim 3, characterized in that, In step (2), the initiator is ammonium persulfate, and the crosslinking agent is N,N'-methylenebisacrylamide; the mass ratio of the crosslinking agent to the acrylamide monomer is 1:1000 to 1:3000; the mass ratio of the initiator to the acrylamide monomer is 0.005:1 to 0.015:1; and the ratio of the mass of the acrylamide monomer to the volume of the zinc sulfate aqueous solution is 1g:2.5 to 4.5mL.

5. A shuttle-resistant, dendrite-suppressing zinc-ion battery, characterized in that, The battery adopts a sandwich structure, comprising, in sequence: a positive electrode, an electrolyte which is the anti-shuttle dendrite-suppressing composite gel electrolyte as described in claim 1 or 2, and a zinc metal negative electrode.

6. The zinc-ion battery according to claim 5, characterized in that, The active component of the positive electrode is an iodine-carbon composite, wherein the mass ratio of iodine to carbon is 1:1, and the carbon is porous activated carbon; the positive electrode is prepared by mixing the iodine-carbon composite, the conductive agent acetylene black, and the binder polyvinylidene fluoride, and coating it onto a carbon cloth current collector.

7. The zinc-ion battery according to claim 5, characterized in that, The battery is externally packaged as a button cell casing or a flexible aluminum-plastic film casing.