A biodegradable personalized silk fibroin web, its preparation method and application

By preparing personalized silk fibroin mesh, the problem of insufficient pressure and bending resistance of the barrier membrane in GBR surgery was solved, and the biocompatibility and mechanical properties were improved, meeting the clinical needs of bone defect repair.

CN123101751APending Publication Date: 2026-11-17FOSHAN ANGELS BIOTECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611253725.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the barrier membrane has limited resistance to pressure and bending during GBR surgery, making it difficult to maintain a stable bone regeneration space. Furthermore, it is non-degradable and requires a second surgery for removal, increasing the complexity of the procedure. Porous zinc-based alloy meshes lack sufficient mechanical strength to meet the needs of bone defect repair.

Method used

Personalized silk fibroin meshes are fabricated by hot pressing silk fibroin powder, combined with CBCT image processing and 3D printing technology. Fixation holes and mesh pores are formed by laser processing, and the mesh is softened and shaped in hot water to ensure that the mesh fits the bone defect area. It has excellent biocompatibility and bending strength comparable to titanium meshes.

Benefits of technology

Personalized silk fibroin mesh exhibits excellent biocompatibility and mechanical properties, providing support and adhesion to bone defect areas. It has no adverse effects after degradation, reducing patient pain, meeting the needs of GBR surgery, and possesses good elasticity and bending resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123101751A_ABST
    Figure CN123101751A_ABST
Patent Text Reader

Abstract

This application belongs to the field of biomedical materials technology, and discloses a biodegradable personalized silk fibroin mesh, its preparation method, and its application. The preparation method of the personalized silk fibroin mesh includes the following steps: obtaining a silk fibroin mesh preform by hot pressing silk fibroin powder; acquiring CBCT images of the patient's maxillofacial region to obtain a three-dimensional model of the jawbone defect, and performing 3D printing to obtain a 3D printed model of the jawbone defect; virtually implanting the silk fibroin mesh to obtain the fixation pore sites; drawing the inner surface of the silk fibroin mesh to obtain a three-dimensional model; converting the three-dimensional model of the silk fibroin mesh into a two-dimensional model, laser processing to obtain the silk fibroin mesh; softening the silk fibroin mesh, then fixing it onto the 3D printed model of the jawbone defect, heat-treating for shaping, and removing the silk fibroin mesh to obtain the personalized silk fibroin mesh. The biodegradable personalized silk fibroin mesh has excellent biocompatibility and bending strength comparable to titanium mesh.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of biomedical materials technology, and specifically relates to a biodegradable personalized silk fibroin mesh, its preparation method and application. Background Technology

[0002] In dental implant bone augmentation, the GBR (Guided Bone Regeneration) technique, based on barrier membranes and bone powder materials, is widely used. However, when faced with severe and complex bone defects, especially in vertical bone augmentation, the barrier membrane, due to its limited resistance to compression and bending, exhibits significant deformation and struggles to maintain a stable space for bone regeneration. During the healing process, soft tissue pressure often leads to micromovement, affecting the effectiveness of bone regeneration and augmentation.

[0003] Patent CN113230002A discloses a method for preparing personalized titanium mesh for bone defect reconstruction in dental implant areas. However, personalized titanium meshes prepared by 3D printing have problems such as easy formation of pseudo-periosteum and high exposure risk. Furthermore, titanium meshes are non-absorbable, requiring a second surgery for removal, increasing the complexity of the surgery and the burden on patients. Patent CN121197509A discloses a biodegradable GBR membrane with a double-sided heterogeneous nanofiber coating constructed on the surface of a porous zinc-based alloy mesh using electrospinning technology. One side of the membrane is loaded with antibacterial drugs to block soft tissue, and the other side is loaded with osteogenic factors to promote bone regeneration. However, the mechanical strength of porous zinc-based alloy meshes is far lower than that of titanium meshes. Summary of the Invention

[0004] This application aims to address at least one of the technical problems existing in the prior art. To this end, this application proposes a biodegradable personalized silk fibroin mesh, its preparation method, and its application. This biodegradable personalized silk fibroin mesh possesses excellent biocompatibility and bending strength comparable to titanium mesh.

[0005] The first aspect of this application provides a method for preparing a personalized silk fibroin web, comprising the following steps: Silk fibroin powder is hot-pressed to obtain silk fibroin web preform; Acquire CBCT images of the patient's maxillofacial region, perform thresholding and three-dimensional reconstruction on the CBCT images to obtain a three-dimensional model of the jawbone bone defect, and perform 3D printing to obtain a 3D printed model of the jawbone bone defect. Virtual implantation was performed based on the three-dimensional model of the jawbone defect to obtain the fixation pore sites of the silk fibroin mesh. The inner surface of the silk fibroin mesh is drawn based on the three-dimensional model of the jawbone bone defect and the fixation pore sites of the silk fibroin mesh, and the thickness is increased along the outer normal direction of the inner surface of the silk fibroin mesh to obtain the three-dimensional model of the silk fibroin mesh. The three-dimensional model of the silk fibroin mesh is converted into a two-dimensional model, and the silk fibroin mesh blank is laser-processed according to the two-dimensional model to obtain a silk fibroin mesh with fixation holes and mesh holes. The silk fibroin mesh is softened by immersing it in hot water. The softened silk fibroin mesh is then fixed onto the 3D printed model of the jawbone defect. After heat treatment to set the shape, the silk fibroin mesh is removed to obtain the personalized silk fibroin mesh.

[0006] The three-dimensional model of jawbone defects obtained in this application includes the alveolar bone defect area, the three-dimensional model of the alveolar bone, and the three-dimensional model of the teeth adjacent to the alveolar bone defect area.

[0007] In some embodiments, the method for preparing the silk fibroin powder includes the following steps: Prepare silk fibroin solution; The silk fibroin solution was dialyzed, centrifuged, freeze-dried, and pulverized to obtain the silk fibroin powder.

[0008] In some embodiments, the method for preparing the silk fibroin solution includes the following steps: The raw silk is degummed, then washed with water to remove the sericin, and dried to obtain degummed silk. The degummed silk is mixed with a good solvent and dissolved to obtain the silk fibroin solution.

[0009] In some embodiments, the degumming process uses an alkaline solution for degumming.

[0010] In some embodiments, the alkaline solution includes at least one of Na2CO3 solution, NaOH solution, NaHCO3, and urea.

[0011] In some embodiments, the concentration of the alkaline solution is 0.05-0.5 wt%.

[0012] In some embodiments, the good solvent includes at least one of LiBr solution, calcium chloride ternary solution, hexafluoroisopropanol (HFIP), hydrated hexafluoroacetone, and formic acid.

[0013] In some embodiments, the ternary calcium chloride solution is composed of calcium chloride, ethanol, and water.

[0014] In some embodiments, the molar ratio of calcium chloride, ethanol, and water in the ternary calcium chloride solution is 1:2:8.

[0015] In some embodiments, the mass ratio of the degummed silk to the good solvent is 1:(10-20).

[0016] In some embodiments, the concentration of the good solvent is 5-10 mol / L.

[0017] In some embodiments, the dissolution temperature is 55-65°C and the dissolution time is 3-6 hours.

[0018] In some embodiments, the dialysis is performed using a dialysis bag with a molecular weight cutoff of 3,500-14,000; the preferred molecular weight cutoff is 6,000-13,000; more preferably 8,000-12,000.

[0019] In some embodiments, the conductivity of the dialyzed water after dialysis of the silk fibroin solution is <5 μS / cm.

[0020] In some embodiments, the freeze-drying temperature is -75°C to -85°C and the pressure is 1-3 Pa.

[0021] In some embodiments, the hot pressing conditions satisfy at least one of the following A1-A3: A1, the hot pressing pressure is 180-220 MPa; A2, the hot pressing temperature is 80-100°C; A3, the hot pressing time is 10-20 min.

[0022] In some embodiments, the silk fibroin mesh retains ≥1.5 mm of alveolar bone on both the labial / buccal and lingual / palatal sides.

[0023] In some embodiments, the thickness of the silk fibroin web is 0.6-1 mm.

[0024] In some embodiments, the retention holes are located on the labial / buccal side and the lingual / palatal side of the silk fibroin mesh.

[0025] In some embodiments, the retention holes satisfy at least one of the following B1-B3: B1, the number of retention holes on the lingual-palatal side is 1-3; B2, the number of retention holes on the labial-buccal side is 1-3 mm; B3, the distance of the retention hole from the edge line is 1-3 mm. The retention holes are matched with the shape and size of conventional retention pins in the art, and the silk fibroin mesh is connected and fixed to the alveolar bone through its retention holes and retention pins.

[0026] In some embodiments, the mesh openings are evenly distributed on the silk fibroin web; the spacing between two adjacent mesh openings is 2-4 mm.

[0027] In some embodiments, the diameter of the mesh openings is 0.5-1 mm.

[0028] In some embodiments, the laser processing conditions include a wavelength of 1030 nm and a focal length of F = 100 mm.

[0029] In some embodiments, the laser processing conditions satisfy at least one of the following C1-C4: C1, frequency of 30-400kHz, preferably 100-300kHz; C2, rotational speed of 1000-5000rpm, preferably 2000-4000rpm; C3, power of 10-50W, preferably 20-40W; C4, pulse width of 0.5-10ps, preferably 0.5-2ps. The rotational speed refers to the beam spin-cutting speed, that is, the rotational speed of the laser focus when performing a circular scan on the material surface.

[0030] In some embodiments, the laser used for laser processing is an infrared femtosecond laser.

[0031] In some embodiments, the heat treatment setting involves steaming the silk fibroin web with high-temperature water vapor; the temperature of the high-temperature water vapor is 100-121°C.

[0032] In some embodiments, the fumigation time is 5-10 minutes.

[0033] A second aspect of this application provides a personalized silk fibroin mesh, prepared by the preparation method described in the first aspect of this application.

[0034] A third aspect of this application provides the use of the personalized silk fibroin mesh described in the second aspect of this application in the preparation of therapeutic dental implant products.

[0035] Compared to existing technologies, the beneficial effects of this application are as follows: (1) The personalized silk fibroin mesh prepared in this application has excellent biocompatibility, does not cause immunogenic reactions, and can be degraded in vivo and in vitro. Its products are mainly various amino acids and peptides, which can be absorbed by the human body and will not have adverse effects on organisms after degradation.

[0036] (2) The personalized silk fibroin mesh prepared in this application serves as a barrier membrane to meet the clinical needs of GBR surgery. It provides support in the bone defect area and also forms a good adhesion effect with the tissue.

[0037] (3) The personalized silk fibroin mesh prepared in this application has multiple uniformly distributed mesh holes through laser processing and perforation, which can block epithelial tissue from entering the defect area while allowing oxygen, blood and bioactive substances to enter.

[0038] (4) The personalized silk fibroin mesh prepared in this application can be bent in a personalized way, providing precise height and width for the defect site and protecting the shape of the bone filler; similarly, the personalized silk fibroin mesh has an active induction effect on osteoblasts, and its low stiffness reduces the risk of exposure, has better fit, and reduces patient pain.

[0039] (5) The solvent used in the personalized bending and shaping process of this application is water, which does not involve additional solvents, conforms to the principle of green production, and is mild and easy to operate. Attached Figure Description

[0040] Figure 1 This is a physical image of the 3D-printed model of the jawbone defect obtained in Embodiment 1 of this application; Figure 2 This is a partially enlarged view of the silk fibroin web obtained after laser processing of the silk fibroin web preform of Example 1 of this application; Figure 3 This is a photograph of the personalized silk fibroin web prepared in Example 1 of this application. Figure 4 The test results of the three-point bending test are for the samples prepared in Example 1 and Comparative Examples 1-2 of this application. Figure 5 The stress-strain curves are for the samples prepared in Example 1 and Comparative Examples 1-2 of this application. Detailed Implementation

[0041] The following specific embodiments further illustrate the content of this application in detail. Unless otherwise specified, the raw materials, reagents, or apparatus used in the embodiments can be obtained from conventional commercial sources or by existing technical methods. Unless otherwise specified, the experimental or testing methods are conventional methods in the art.

[0042] Example 1 This embodiment provides a method for preparing a personalized silk fibroin web, including the following steps: S1. Degumming of raw silk is performed using a 0.5wt% Na2CO3 solution, followed by washing with deionized water to remove sericin, and drying to obtain degummed silk.

[0043] S2. Degummed silk is added to a ternary calcium chloride solution, wherein the molar ratio of calcium chloride:ethanol:water is 1:2:8, and the solution is heated in a water bath at 60°C for 4 hours until completely dissolved to obtain a silk fibroin solution; wherein the mass ratio of degummed silk to the ternary calcium chloride solution is 1:10. S3. Place the silk fibroin solution in a dialysis bag with a molecular weight cutoff of 10,000, then place the dialysis bag in deionized water for dialysis until the conductivity of the dialysis water is <5μS / cm. Then centrifuge to remove insoluble impurities, and then place it in a freeze dryer at a temperature of 80℃ and a pressure of 2Pa for freeze drying and pulverize to obtain silk fibroin powder. S4. Place the silk fibroin powder into a hot press mold, then place the hot press mold into a hot press machine for hot pressing to shape the material. After natural cooling, remove the material to obtain the silk fibroin mesh blank. The hot pressing parameters are: pressure 200MPa, temperature 100℃, and time 20min.

[0044] S5. Acquire CBCT images of the patient's maxillofacial region, perform thresholding and 3D reconstruction on the CBCT images to obtain a 3D model of the jawbone bone defect, and perform 3D printing to obtain a 3D printed model of the jawbone bone defect (e.g., Figure 1 (as shown) S6. Virtual implantation is performed based on the three-dimensional model of the jawbone defect to obtain the fixation pore sites of the silk fibroin mesh. S7. Draw the inner surface of the silk fibroin network based on the three-dimensional model of the jawbone bone defect and the fixation pore sites of the silk fibroin network, and increase the thickness along the outer normal direction of the inner surface of the silk fibroin network to obtain the three-dimensional model of the silk fibroin network; the three-dimensional model of the silk fibroin network extends to the position of the normal alveolar bone morphology on the surface of the alveolar bone defect, ensuring that 1.5 mm of alveolar bone volume is retained on the labial and buccal sides and the lingual and palatal sides; S8. Convert the 3D model of the silk fibroin mesh into a 2D model, and perform laser processing (infrared femtosecond laser) on the silk fibroin mesh blank according to the 2D model to obtain a silk fibroin mesh with fixation pores and mesh openings; the main body thickness of the silk fibroin mesh is 0.8mm; there are two fixation pores on both the palatal and labial / buccal sides, and the fixation pores are 2mm away from the edge line; the mesh openings are evenly distributed on the silk fibroin mesh (e.g., ...). Figure 2 As shown in the figure, the spacing between two adjacent meshes is 3mm, and the diameter of the mesh is 0.8mm; the laser processing parameters are: 200kHz, 3000rpm, laser power 30W, pulse width 1ps, focal length F=100mm, wavelength 1030nm.

[0045] S9. Immerse the silk fibroin mesh in 90℃ hot water for 30 minutes to fully soften it. Fix the softened silk fibroin mesh onto the 3D printed model of the jawbone defect, ensuring that the silk fibroin mesh completely conforms to the alveolar bone defect area. Use 100℃ steam to fumigate and shape the silk fibroin mesh for 5 minutes. After natural cooling, remove the silk fibroin mesh to obtain the personalized silk fibroin mesh (e.g., ...). Figure 3 (As shown).

[0046] Comparative Example 1 This example uses a titanium mesh with a thickness of 0.8 mm, a length of 24.52 mm, a width of 14.77 mm, a aperture of 0.8 mm, and a hole spacing of 3 mm.

[0047] Comparative Example 2 This example refers to the preparation method of the invention patent with publication number CN121197509A. A Zn-3Ag alloy mesh with a thickness of 0.8 mm, a pore size of 1.0 mm, and a pore spacing of 3 mm is used. Through electrospinning, a gelatin nanofiber coating loaded with BMP-2 is formed on the lower surface of the alloy mesh, and a hydrophobic drug-loaded PCL nanofiber membrane is formed on the upper surface of the alloy mesh.

[0048] Three-point bending test The products prepared in Example 1 and Comparative Examples 1-2 were used as test samples. Each group contained 5 samples. Three-point bending tests were performed using a computer-controlled electronic universal testing machine, following the requirements of YB / T 5349-2014. At an ambient temperature of 25°C, a force of 1 mm / min was applied vertically along the centerline of the sample. A constant vertical pressure was applied until the sample fractured, and the average compressive modulus of each group was calculated. Figure 4 As shown.

[0049] Depend on Figure 4 As can be seen, the personalized silk fibroin mesh prepared in this embodiment exhibits a compressive modulus comparable to that of titanium mesh in the three-point bending mechanical property test, highlighting its superior mechanical properties and bending resistance. This excellent bending strength means that the personalized silk fibroin mesh of this application can maintain structural integrity when subjected to large bending loads, which is crucial for many engineering and biomedical applications.

[0050] In addition, such as Figure 5 As shown, the stress-strain curve slope of the personalized silk fibroin mesh of this application is similar to that of the titanium mesh, demonstrating its good elastic properties. This allows the material to recover its original shape after being subjected to stress, reducing the risk of permanent deformation.

[0051] Furthermore, within the parameter range defined in this application, by adjusting the process parameters in Example 1, the mechanical properties of the resulting personalized silk fibroin web are not significantly different from those of the sample in Example 1.

[0052] The preferred embodiments of this application have been described in detail above, but the invention of this application is not limited to the embodiments described. Those skilled in the art can make various equivalent modifications or substitutions without departing from the spirit of this application, and these equivalent modifications or substitutions are all included within the scope defined by the claims of this application.

Claims

1. A method for preparing a personalized silk fibroin web, characterized in that, Includes the following steps: Silk fibroin powder is hot-pressed to obtain silk fibroin web preform; Acquire CBCT images of the patient's maxillofacial region, perform thresholding and three-dimensional reconstruction on the CBCT images to obtain a three-dimensional model of the jawbone bone defect, and perform 3D printing to obtain a 3D printed model of the jawbone bone defect. Virtual implantation was performed based on the three-dimensional model of the jawbone defect to obtain the fixation pore sites of the silk fibroin mesh. The inner surface of the silk fibroin mesh is drawn based on the three-dimensional model of the jawbone bone defect and the fixation pore sites of the silk fibroin mesh, and the thickness is increased along the outer normal direction of the inner surface of the silk fibroin mesh to obtain the three-dimensional model of the silk fibroin mesh. The three-dimensional model of the silk fibroin mesh is converted into a two-dimensional model, and the silk fibroin mesh blank is laser-processed according to the two-dimensional model to obtain a silk fibroin mesh with fixation holes and mesh holes. The silk fibroin mesh is softened by immersing it in hot water. The softened silk fibroin mesh is then fixed onto the 3D printed model of the jawbone defect. After heat treatment to set the shape, the silk fibroin mesh is removed to obtain the personalized silk fibroin mesh.

2. The preparation method according to claim 1, characterized in that, The hot pressing conditions satisfy at least one of the following A1-A3: A1, the hot pressing pressure is 180-220MPa; A2, the hot pressing temperature is 80-100℃; A3, the hot pressing time is 10-20min.

3. The preparation method according to claim 1, characterized in that, The silk fibroin mesh retains ≥1.5 mm of alveolar bone on both the labial / buccal and lingual / palatal sides; and / or, the thickness of the silk fibroin mesh is 0.6-1 mm.

4. The preparation method according to claim 1, characterized in that, The retention pores are located on the labial and buccal sides and the lingual and palatal sides of the silk fibroin mesh.

5. The preparation method according to claim 4, characterized in that, The retention holes satisfy at least one of the following B1-B3: B1, the number of retention holes on the lingual palatal side is 1-3; B2, the number of retention holes on the labial buccal side is 1-3; B3, the distance of the retention holes from the edge line is 1-3 mm.

6. The preparation method according to claim 1, characterized in that, The mesh openings are evenly distributed on the silk fibroin web; the spacing between two adjacent mesh openings is 2-4 mm; and / or, the diameter of the mesh openings is 0.5-1 mm.

7. The preparation method according to claim 1, characterized in that, The laser processing conditions include: a wavelength of 1030nm and a focal length of F=100mm; and satisfying at least one of the following C1-C4: C1, frequency of 30-400kHz; C2, rotation speed of 1000-5000rpm; C3, power of 10-50W; C4, pulse width of 0.5-10ps.

8. The preparation method according to claim 1, characterized in that, The heat treatment and shaping process involves fumigating the silk fibroin web with high-temperature steam; the temperature of the high-temperature steam is 100-121℃; and / or the fumigation time is 5-10 minutes.

9. A personalized silk fibroin web, characterized in that, It is prepared by the preparation method according to any one of claims 1-8.

10. The application of the personalized silk fibroin mesh according to claim 9 in the preparation of therapeutic dental implant products.

Citation Information

Patent Citations

  • Preparation method of personalized titanium mesh for bone defect reconstruction in tooth implantation area

    CN113230002A

  • Degradable zinc-based composite GBR film with nano electrostatic spinning fiber coating loaded on surface and preparation and application of degradable zinc-based composite GBR film

    CN121197509A