A method for manufacturing a heat-resistant aluminum alloy fork hinge for commercial satellites
By combining radial rotation hot forging for diameter reduction and elongation with die forging processes and heat treatment, the problem of poor plastic deformation capacity of commercial satellite components in die forging has been solved, realizing the efficient and low-cost preparation of aluminum alloy fork hinges, which are suitable for load-bearing components of commercial satellites.
Patent Information
- Application Number
- CN202611619923.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Commercial satellite components face the problem of poor material plastic deformation capacity during die forging. Traditional casting or machining methods are difficult to meet the requirements of low-cost and high-efficiency manufacturing. Existing high-strength heat-resistant aluminum alloy ZL205A has technical bottlenecks in the die forging process.
A heat-resistant Al-Cu-Mn alloy rod, produced by semi-continuous casting, is used to manufacture aluminum alloy fork-shaped hinges suitable for commercial satellites through radial rotation hot forging for diameter reduction and elongation, rough forging, and precision forging processes, combined with heat treatment and machining. This process eliminates surface stress and improves mechanical properties.
The forging of ZL205A aluminum alloy was achieved, which improved production efficiency and product qualification rate, reduced machining workload, and met the demand of commercial satellites for high-efficiency, low-cost mass production.
Smart Images

Figure CN123102916A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal material plastic processing technology, and particularly relates to a method for preparing a heat-resistant aluminum alloy fork hinge for commercial satellites. Background Technology
[0002] Aluminum alloys are widely used in the aerospace field due to their low density and excellent comprehensive mechanical properties. Especially in the satellite field, aluminum alloys account for 40%-50% of the total mass of satellites, including the main load-bearing frame, mounting plates, brackets, solar cell array substrates, and deployment mechanisms.
[0003] Before the rise of the commercial space industry, the manufacturing of traditional satellite components was limited by small batch sizes and diverse structural designs, typically employing casting or extensive machining. Only a small number of simple components or those with extremely high performance requirements were manufactured using forging. Furthermore, due to the high cost of forging molds, these small-batch components were rarely manufactured using forging. However, in recent years, with the rapid development of commercial spaceflight, low-cost mass production has become a core requirement for commercial satellite manufacturing. Traditional casting or machining methods are insufficient to meet the demands for high efficiency and low cost. In the context of mass production needs, forging demonstrates significant advantages. On the one hand, batch production distributes the mold costs per unit; on the other hand, the high production efficiency of forging, coupled with minimal or even no machining allowance, greatly improves production efficiency. Therefore, adopting forging technology to produce commercial satellite components has become an urgent need in the current commercial space industry.
[0004] However, the reason why forged parts are not widely used in commercial satellite components is not only due to limitations in traditional design concepts, but also due to material limitations. Due to the harsh space environment, the high-strength, heat-resistant aluminum alloys used in existing satellites are mainly ZL205A alloys. The high strength and heat resistance of this alloy, along with its good casting properties, perfectly match the requirements of traditional satellite component manufacturing. However, as a cast aluminum alloy, ZL205A alloy has poor plastic deformation capacity, posing a significant technical bottleneck when it is die-forged. Other high-strength, heat-resistant aluminum alloy systems that can be die-forged have not been tested in application environments.
[0005] Therefore, developing plastic forming technology based on ZL205A aluminum alloys, especially die forging technology, to achieve low-cost and high-efficiency manufacturing of satellite components is an urgent problem that needs to be solved in the commercial satellite manufacturing field. Summary of the Invention
[0006] To address the aforementioned technical problems and shortcomings in this field, the present invention aims to provide a method for preparing a heat-resistant aluminum alloy fork hinge for commercial satellites. This method addresses the plastic forming issues of ZL205A aluminum alloys, using semi-continuously cast heat-resistant Al-Cu-Mn alloy ingots as raw materials. Through a series of interconnected processes, a die forging process is achieved to obtain a blank for the aluminum alloy fork hinge for commercial satellites. Following heat treatment and machining, an aluminum alloy fork hinge with excellent room temperature and high-temperature mechanical properties is obtained. This aluminum alloy fork hinge can be used as a load-bearing component in commercial satellites.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] This invention discloses a method for preparing a heat-resistant aluminum alloy fork-shaped hinge for commercial satellites. The method involves radially rotating and hot-forging a semi-continuous cast heat-resistant aluminum alloy rod to reduce its diameter and length, obtaining a forged rod. The forged rod is then slit to obtain a blank, which is heated to 430℃~450℃ and held for 1~1.5 hours before rough forging to obtain a hot rough forging. The flash of the hot rough forging is removed directly without cooling. Then, it is held at 400℃~420℃ for 5~10 minutes before hot finish forging to obtain a hot finish forging. The flash of the hot finish forging is removed directly without cooling, and then it is air-cooled to room temperature to obtain a fork-shaped hinge finish forging blank. The fork-shaped hinge finish forging blank is then rough-machined and subjected to T6 heat treatment. After T6 heat treatment, it is precision-machined to the final dimensions to obtain the heat-resistant aluminum alloy fork-shaped hinge.
[0009] The preparation method of this invention uses a heat-resistant aluminum alloy semi-continuous cast ingot as raw material. First, a forged ingot is obtained by radial rotational hot forging to reduce its diameter. The heat-resistant aluminum alloy semi-continuous cast ingot is then reduced in diameter and lengthened by radial rotational hot forging. Next, the billet to be forged is heated to 430℃~450℃. At this temperature, rough forging deformation is achieved. The hot rough forging does not require cooling; the flash is directly removed, resulting in low flash cutting force. Furthermore, after flash cutting, the material can be quickly and directly heated to the temperature required for precision forging by placing it back in the furnace. Because the rough forging process transforms the material's microstructure from a cast state to a deformed state, its plastic deformation capacity is significantly increased. Therefore, a lower hot precision forging heating temperature of 400℃~420℃ is used for precision forging compared to rough forging. By reducing the grain size of the forging and improving the mechanical properties of the parts, after hot precision forging, the flash is removed directly without cooling, and then air-cooled to room temperature to obtain a forked hinge precision forging blank. Finally, rough machining and precision machining are set before and after T6 heat treatment, respectively. The heat treatment process eliminates the surface stress introduced by rough machining, and the subsequent precision machining can avoid the deformation and scrapping of parts caused by quenching. Moreover, the surface machining stress introduced by the extremely small machining amount (0.5mm~0.8mm) is also extremely small and has almost no impact on the dimensional accuracy of the parts. Through the above-mentioned interlocking processes, this invention has pioneered the die forging of ZL205A system aluminum alloys to obtain heat-resistant aluminum alloy forked hinges suitable for commercial satellites.
[0010] In a preferred embodiment, the heat-resistant aluminum alloy fork hinge has the following composition by weight percentage: Cu: 4.8~5.6wt%; Mn: 0.3~0.5wt%; Cd: 0.15~0.25wt%; Ti: 0.18~0.25wt%; Zr: 0.1~0.2wt%; V: 0.15~0.3wt%; B: 0.005~0.06wt%; Mg≤0.01wt%; Zn≤0.01wt%; Fe≤0.03wt%; Si≤0.05wt%; the balance being Al and unavoidable impurities, with the content of any single impurity <0.001wt%.
[0011] The heat-resistant aluminum alloy fork hinge in this invention has a main component that is comparable to the ZL205A cast aluminum alloy currently used in satellites. This allows the final fork hinge to be directly replaced as long as it meets the performance indicators, without the need for long-term and complex application environment verification.
[0012] Based on the process of this invention, the contents of Mg, Zn, Fe, and Si are controlled at extremely low levels. This is because the original material of this invention is a semi-continuous ingot. For Al-Cu alloys with high copper content, the preparation of semi-continuous ingots is inherently difficult due to their high tendency for hot cracking. Furthermore, Zn and Mg elements further exacerbate this tendency. On the other hand, the strengthening phases containing Zn and Mg have poor thermal stability, and the mechanical properties of the alloy decrease significantly under high-temperature conditions or after heat exposure. Therefore, it is necessary to control the contents of Zn and Mg at low levels. Fe and Si elements form brittle, coarse intermetallic compounds in aluminum alloys, thereby reducing the mechanical properties of the alloy. However, Si elements improve melt fluidity and enhance casting performance in the casting process; Fe elements facilitate demolding of castings. Therefore, the upper limit of Fe and Si element contents is appropriately increased in conventional casting alloys. The forging process used in this invention does not involve issues of melt fluidity and casting release properties. Therefore, it is necessary to minimize the adverse effects of Fe and Si. The brittle intermetallic compounds formed by Fe and Si not only reduce the mechanical properties of the final material, but also cause them to fracture during forging due to localized stress concentration, leading to forging cracks. Therefore, considering the role of the elements and the characteristics of the preparation process, the content of these elements in this invention must be limited to extremely low levels.
[0013] In a further preferred embodiment, the heat-resistant aluminum alloy fork hinge has the following composition by weight percentage: Cu: 5.2~5.6wt%; Mn: 0.3~0.4wt%; Cd: 0.2~0.25wt%; Ti: 0.18~0.22wt%; Zr: 0.15~0.2wt%; V: 0.15~0.2wt%; B: 0.005~0.02wt%; Mg≤0.01wt%; Zn≤0.01wt%; Fe≤0.03wt%; Si≤0.05wt%; the balance being Al and unavoidable impurities, with the content of any single impurity <0.001wt%.
[0014] In a preferred embodiment, the diameter of the heat-resistant aluminum alloy semi-continuous casting rod is 100mm~120mm. In actual operation, the surface oxide scale and impurities of the heat-resistant aluminum alloy semi-continuous casting rod need to be machined off.
[0015] Controlling the diameter of the heat-resistant aluminum alloy semi-continuous casting rod within the range of this invention is based on its relation to the total deformation amount of subsequent drawing and die forging. If the diameter is too small, the total deformation amount is small, making it difficult to guarantee the mechanical properties of the final part. If the diameter is too large, it increases the total deformation amount of subsequent forging, increasing the forging difficulty and even causing difficulties in forming. In addition, considering the semi-continuous casting rods of the composition materials described in this invention that are currently available on the market, it is preferable to select a semi-continuous casting rod with a diameter of 100mm to 120mm.
[0016] In a preferred embodiment, the radial rotation hot forging for diameter reduction and elongation is preheated before the process. The preheating process is as follows: the heat-resistant aluminum alloy semi-continuous casting rod is first heated to 530℃~540℃ and held for 12~15h, and then cooled to 430℃~450℃ and held for 3~5h.
[0017] Before radial rotary hot forging for diameter reduction and elongation, the ingot is first heated to 530℃~540℃ and held at that temperature for 12~15 hours. This process allows the second-phase dendrites formed during the semi-continuous casting solidification process to re-dissolve into the aluminum matrix, achieving homogenization of alloying elements. The subsequent furnace cooling process allows Zr, V, Mn, and Ti elements in the alloy to precipitate as nanoscale second phases, particularly at grain boundaries. These precipitated phases inhibit dynamic recrystallization and hinder recrystallized grain growth during the subsequent hot forging process, ensuring a fine-grained microstructure after forging. Cooling to 430℃~450℃ and holding for 3~5 hours before rotary hot forging for diameter reduction and elongation avoids severe grain growth caused by the first-stage high-temperature elongation. Furthermore, this temperature ensures the alloy retains good plastic deformation capacity, preventing elongation cracking.
[0018] In the preferred embodiment, during the radial rotation hot forging for diameter reduction and elongation, the forging speed is controlled at 3~5 mm / s, the single forging reduction is 5 mm~10 mm, and the final forging temperature is 380℃~420℃.
[0019] Experiments have shown that, since the deformation per pass in rotary drawing is usually small, controlling the temperature between 380℃ and 420℃ can effectively prevent the material's plastic deformation capacity from deteriorating in the later stages of drawing. The purpose of the radial rotary hot forging reduction drawing process in this invention is to unidirectionally draw a large-diameter round cast bar into a smaller-diameter round forged bar. Therefore, it is necessary to control the deformation per pass. A small deformation per pass results in longer processing time and significant heat dissipation, making it difficult to meet the final forging temperature requirements. An excessive deformation per pass requires repeated rounding to ensure dimensional accuracy, which also delays processing time. Experiments have shown that a deformation per pass of 5mm to 10mm minimizes processing time while ensuring the final forging temperature remains within the required range. When the final forging temperature and the amount of deformation per pass are required to be controlled within a specific range, the forging speed needs to be controlled to match them. If the forging speed is too slow, the temperature loss will be greater than the temperature rise during deformation, resulting in a severe temperature drop in the billet. If the forging speed is too fast, the temperature rise during deformation will be greater than the temperature loss, resulting in a significant temperature rise in the billet. In both cases, it is difficult to ensure that the final forging temperature is within the required range. However, by controlling the forging speed within the range of 3~5 mm / s of this invention, the requirements for the amount of reduction per pass and the final forging temperature can be matched.
[0020] In a preferred embodiment, the diameter of the forged bar is 45mm to 48mm. The forged bar is obtained by radial rotational hot forging and diameter reduction on a forging press, resulting in a diameter of 45mm to 48mm.
[0021] The length of the forging billet obtained after slitting the forging bar needs to be calculated based on the weight of the final forged part, the lengths of the long and short sides, and the diameter of the drawn bar. If the length is too short, the long side of the final part will be difficult to completely fill; if the length is too long, it will lead to severe flash during die forging, causing the height dimension of the forging to exceed the standard. Through calculation and actual experimental verification, it is advisable to select a billet with a length 10mm~15mm longer than the target fork hinge length. For example, if the target fork hinge length is 150mm, a billet with a length of 160mm~165mm is preferable.
[0022] In a preferred embodiment, the hot rough forging is completed in one pass, the forging direction is perpendicular to the axial direction of the billet to be forged, the forging speed is 8~10mm / s, and the final forging temperature of the hot rough forging is 400℃~420℃.
[0023] Although the rotary hot forging process for reducing diameter and elongating meets the dimensional requirements of the billet, its total plastic deformation is not large. In order to ensure that the hot rough forging process can be formed smoothly, the heating temperature of the billet still needs to be controlled at 430℃~450℃ before forging. The reason is the same as the temperature control principle of rotary hot forging elongation. However, the contact area between the billet and the die in the rough forging process is larger than that in rotary elongation, and its temperature drop rate is also significantly greater than that in rotary elongation. Therefore, the rough forging needs to be completed in a shorter time, that is, a forging speed faster than rotary forging elongation should be selected.
[0024] Because the friction between the billet metal and the die varies at different locations during die forging, the frictional heat differences between these locations can be significant. Temperature directly affects the grain size of the forging, thus influencing its mechanical properties. To ensure the uniformity of properties across all locations in the final forging, the final forging temperature needs to be controlled within a narrower range. Experiments have shown that, based on the limitations of hot rough forging heating temperature and forging speed, controlling the final die forging temperature within the range of 400℃~420℃ not only facilitates deformation but also prevents grain growth in the forging, while ensuring the uniformity of the microstructure across all locations in the rough forging. If the final forging temperature is too low, a slower forging speed is required, which not only reduces processing efficiency but also easily leads to microcracks and a significant increase in forging force. If the temperature is too high, dynamic recrystallization and grain growth occur, resulting in a decrease in the mechanical properties of the final part.
[0025] In a preferred embodiment, during the hot rough forging, the final forging thickness is controlled to be 3-4 mm thicker than the final forging circle dimension. In this invention, the final forging circle dimension refers to the dimension in the forging drawing, i.e., the dimension before rough machining.
[0026] Experiments have shown that controlling the thickness of the rough forging to be 3-4 mm thicker than the final forged fork hinge circle results in the best forging effect and facilitates the control of subsequent hot forging precision. If the final forging thickness is too small, the deformation in this pass will be too large, which will not only significantly increase the forging force but also easily lead to forging cracks; if the final forging thickness is too large, the deformation in subsequent precision forging will increase, which is detrimental to precision control.
[0027] In a preferred embodiment, the hot precision forging is completed in one pass, the forging speed is 5~8 mm / s, and the final forging temperature is 380℃~400℃.
[0028] Since the rough forging process transforms the material's microstructure into a deformable microstructure, its plastic deformation capacity is significantly increased. Therefore, this invention uses a lower hot finishing forging temperature of 400℃~420℃ compared to rough forging, and the corresponding final forging temperature is also reduced to 380℃~400℃. Combined with a forging speed of 5~8mm / s lower than rough forging, the grain size of the forging can be reduced, and the mechanical properties of the parts can be improved.
[0029] In a preferred embodiment, during the hot precision forging process, the final forging thickness is controlled to be the same as the final forging circle size.
[0030] In a preferred embodiment, during the rough machining process, a single-sided allowance of 0.5mm to 0.8mm is retained to obtain a rough-machined fork-shaped hinge part.
[0031] In practice, hot-forged parts have their flash removed directly on a trimming machine and then air-cooled to room temperature to obtain the forging blank for the aluminum alloy fork hinge used in commercial satellites. However, since satellite fork hinges are precision parts with mounting holes and surfaces, precision forging still requires subsequent machining to achieve the required dimensional accuracy. Furthermore, the heat-resistant aluminum alloy described in this invention is a heat-treatable alloy, and the forged parts need heat treatment to achieve the required performance indicators. The traditional process of heat treatment followed by machining inevitably introduces machining stress into the part surface. During subsequent use, this stress gradually releases, causing dimensional deviations and ultimately leading to the failure of high-precision satellite components. While machining followed by heat treatment avoids introducing machining stress into the part surface, the quenching process introduces quenching stress into the part's interior. This quenching stress can directly cause deformation and render the machined part unusable. This invention differs from the traditional manufacturing routes of machining followed by heat treatment or heat treatment followed by machining by placing the heat treatment process between rough machining and precision machining. The heat treatment process eliminates the surface stress introduced by rough machining, and the subsequent precision machining can avoid the deformation and scrapping of parts caused by quenching. Moreover, the surface machining stress introduced by the extremely small machining amount (0.5mm~0.8mm) is also very small and has almost no impact on the dimensional accuracy of the parts.
[0032] In a preferred embodiment, the T6 heat treatment process involves first performing a solution treatment, followed by room temperature quenching, and then artificial aging.
[0033] In a further preferred embodiment, the solution treatment temperature is 520℃~540℃, and the solution treatment time is 2~3h.
[0034] In a further preferred embodiment, the temperature for artificial aging is 165℃~180℃, and the artificial aging time is 8~12h.
[0035] The aluminum alloy described in this invention is a high-copper-content Al-Cu alloy. In existing technologies, solution treatment of this series of alloys requires two or even multiple stages. However, because the aluminum alloy fork hinge in this invention has extremely low contents of Mg, Zn, Fe, and Si, and the microstructure does not contain low- or high-melting-point compounds containing these elements, a single-stage solution heat treatment is sufficient to ensure the dissolution of the Al2Cu phase. Experiments have shown that holding at 520℃~540℃ achieves the solution of the Al2Cu phase, and the aging process only needs to consider the nanoscale. The strengthening phase is sufficient, and the optimal mechanical properties can be achieved by aging at 165℃~180℃ for 8~12h as described in this invention.
[0036] In a preferred embodiment, the heat-resistant aluminum alloy fork hinge has a room temperature tensile strength ≥460MPa, a yield strength ≥370MPa, and an elongation ≥10% in the length direction; a high temperature tensile strength ≥370MPa, a yield strength ≥350MPa, and an elongation ≥9% at 200℃; and a room temperature tensile strength ≥380MPa, a yield strength ≥270MPa, and an elongation ≥8% after 100 hours of heat exposure at 200℃.
[0037] Principles and advantages:
[0038] The preparation method of this invention uses a heat-resistant aluminum alloy semi-continuous casting rod as raw material. First, a forged rod is obtained by radial rotational hot forging to reduce its diameter and lengthen it. Then, the forged billet is heated to 430℃~450℃. At this temperature, rough forging deformation is achieved. The flash of the hot rough forging is directly removed without cooling, resulting in low cutting force. Furthermore, after cutting, the material can be quickly and directly heated to the temperature required for precision forging by placing it back in the furnace. Because the rough forging process transforms the material's microstructure from a casting microstructure to a deformed microstructure, its plastic deformation capacity is significantly increased. Therefore, a lower hot precision forging heating temperature of 400℃~420℃ is used for precision forging compared to rough forging. By reducing the grain size of the forging and improving the mechanical properties of the parts, after hot precision forging, the flash is removed directly without cooling, and then air-cooled to room temperature to obtain a forked hinge precision forging blank. Finally, rough machining and precision machining are set before and after T6 heat treatment, respectively. The heat treatment process eliminates the surface stress introduced by rough machining, and the subsequent precision machining can avoid the deformation and scrapping of parts caused by quenching. Moreover, the surface machining stress introduced by the extremely small machining amount (0.5mm~0.8mm) is also extremely small and has almost no impact on the dimensional accuracy of the parts. Through the above-mentioned interlocking processes, this invention has pioneered the die forging of ZL205A system aluminum alloys to obtain heat-resistant aluminum alloy forked hinges suitable for commercial satellites.
[0039] This invention targets the poor plastic deformation capacity of ZL205A aluminum alloy used in satellites. By effectively utilizing the process window for plastic deformation in each step of radial rotary hot forging (diameter reduction and elongation), rough forging, and finish forging, it successfully achieves the die forging of ZL205A aluminum alloy. This invention breaks through the existing technical path that fork-shaped hinges made of ZL205A aluminum alloy for satellites can only be produced by casting. The fork-shaped hinge forging blank is prepared through a two-step die forging process (rough forging + finish forging). Compared with casting, die forging significantly improves production efficiency and product yield. Furthermore, the technology of this invention significantly reduces machining workload, resulting in significant advantages in production efficiency and cost. Therefore, the manufacturing method provided by this invention is more suitable for the high-efficiency, low-cost, and mass production requirements of components in the commercial satellite field. Attached Figure Description
[0040] Figure 1 This is a die-forged blank for the heat-resistant aluminum alloy fork-shaped hinge prepared according to the present invention.
[0041] Figure 2 This is a full-size heat-resistant aluminum alloy fork hinge that has undergone precision machining according to the present invention.
[0042] Figure 3 The metallographic structure of the forged blank of the forked hinge prepared in Example 1 of the present invention shows that the grains are fine and uniform.
[0043] Figure 4 The room temperature tensile mechanical property curves of the fork-shaped hinge prepared in Example 1 of the present invention.
[0044] Figure 5 The tensile mechanical property curve of the fork-shaped hinge prepared in Example 1 of the present invention under 200°C conditions.
[0045] Figure 6 The figure shows the room temperature tensile mechanical properties of the fork-shaped hinge prepared in Example 1 of this invention after being exposed to heat at 200°C for 100 hours.
[0046] Figure 7 The metallographic structure of the forged blank of the forked hinge prepared in Comparative Example 2 shows that the grains have grown significantly and are not uniform.
[0047] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Detailed Implementation
[0048] Example 1
[0049] The raw material is a ZL205A aluminum alloy semi-continuous casting rod with a diameter of 120mm and a length of 0.5m. Its chemical composition is as follows: Cu: 5.53wt%; Mn: 0.38wt%; Cd: 0.21wt%; Ti: 0.20wt%; Zr: 0.17wt%; V: 0.18wt%; B: 0.008wt%; Mg: 0.003wt%; Zn: 0.001wt%; Fe: 0.02wt%; Si: 0.03wt%; with the balance being Al and unavoidable impurities, and the content of any single impurity is <0.001wt%.
[0050] After removing the surface oxide scale and impurities from the semi-continuous casting bar, it is placed in a furnace and heated to 540℃, then held for 15 hours. It is then cooled to 450℃ and held for 3 hours. Subsequently, it undergoes radial rotary hot forging to reduce its diameter and length on a forging press, controlling the forging speed at 3 mm / s, with a single forging reduction of 10 mm, and a final forging temperature of 380℃~420℃, until the bar billet diameter is reduced to 48 mm, at which point the billet length is approximately 3 m. The reduced-diameter and lengthened forged bar is then trimmed and cut into 160 mm long billets, which are placed in a holding furnace at 430℃ for 1.5 hours. Afterward, hot rough forging is performed in a die forging mold. The rough forging is completed in one pass, with the forging direction perpendicular to the billet axis, a forging speed of 8 mm / s, and a final forging thickness 4 mm thicker than the final forged part's round dimension, at a final forging temperature of 400℃~420℃. After hot rough forging, the flash is removed directly on a trimming machine and then placed in a 420℃ furnace for 5 minutes. Hot finish forging is then performed in a die forging mold. The hot finish forging is completed in one pass at a forging speed of 8 mm / s. The final forging thickness is the same as the final forging circle size, and the final forging temperature is 380℃~400℃. The hot finish forged parts have their flash removed directly on the trimming machine and then air-cooled to room temperature to obtain a fork-shaped hinge forging blank.
[0051] The forged billet was rough-machined on a four-axis machining center, with a single-sided allowance of 0.8mm retained according to the final drawing dimensions. The rough-machined part was then solution-treated in a 540℃ holding furnace for 2 hours, followed by room temperature quenching. After quenching, it was placed directly into an aging furnace at 180℃ for 8 hours without resting, and then air-cooled. The aging-treated part was then finish-machined on a four-axis machining center according to the final dimensions, resulting in a 150mm long aluminum alloy fork hinge for commercial satellites.
[0052] The aluminum alloy fork hinge has a room temperature tensile strength of 474 MPa, a yield strength of 407 MPa, and an elongation of 10.4% in the longitudinal direction; a high temperature tensile strength of 378 MPa, a yield strength of 374 MPa, and an elongation of 10% at 200℃; and a room temperature tensile strength of 382 MPa, a yield strength of 278 MPa, and an elongation of 10% after 100 hours of heat exposure at 200℃.
[0053] Example 2
[0054] The raw material is a ZL205A aluminum alloy semi-continuous casting rod with a diameter of 100mm and a length of 0.5m. Its chemical composition is as follows: Cu: 5.53wt%; Mn: 0.38wt%; Cd: 0.21wt%; Ti: 0.20wt%; Zr: 0.17wt%; V: 0.18wt%; B: 0.008wt%; Mg: 0.003wt%; Zn: 0.001wt%; Fe: 0.02wt%; Si: 0.03wt%; the balance is Al and unavoidable impurities, and the content of a single impurity is <0.001wt%.
[0055] After removing the surface oxide scale and impurities from the semi-continuous casting bar, it is placed in a furnace and heated to 530℃ and held for 12 hours. Then, it is cooled to 430℃ and held for 5 hours. Subsequently, it undergoes radial rotary hot forging to reduce its diameter and length on a forging press, controlling the forging speed at 5 mm / s, with a single forging reduction of 5 mm, and a final forging temperature of 380℃~420℃, until the bar billet diameter is reduced to 45 mm, at which point the billet length is approximately 2.5 m. The reduced-diameter and lengthened forged bar is then trimmed and cut into 165 mm long billets, which are placed in a holding furnace at 450℃ and held for 1 hour. Afterward, hot rough forging is performed in a die forging mold. The rough forging is completed in one pass, with the forging direction perpendicular to the billet axis, a forging speed of 10 mm / s, and a final forging thickness 3 mm thicker than the final forged part's round dimension. The final forging temperature is 400℃~420℃. After hot rough forging, the flash is removed directly on a trimming machine and then placed in a 400℃ heating furnace. After holding at this temperature for 10 minutes, hot finish forging continues in a die forging mold. Hot finish forging is completed in one pass at a forging speed of 5 mm / s. The final forging thickness is the same as the final forging circle size, and the final forging temperature is 380℃~400℃. The hot finish forged parts have their flash removed directly on the trimming machine and then air-cooled to room temperature to obtain a fork-shaped hinge forging blank.
[0056] The precision-forged billet is rough-machined on a four-axis machining center. According to the final drawing dimensions, the rough-machined part retains a single-sided allowance of 0.5mm. Then, the rough-machined part is placed in a 520℃ holding furnace for solution treatment for 3 hours, followed by room temperature quenching. After quenching, without resting, it is directly placed in a 165℃ aging furnace for 12 hours and then air-cooled. The aging-treated part is then precision-machined on a four-axis machining center according to the final dimensions, ultimately obtaining a 150mm long aluminum alloy fork-shaped hinge for commercial satellites.
[0057] The aluminum alloy fork hinge has a room temperature tensile strength of 468 MPa, a yield strength of 402 MPa, and an elongation of 11% in the longitudinal direction; a high temperature tensile strength of 376 MPa, a yield strength of 368 MPa, and an elongation of 10.4% at 200℃; and a room temperature tensile strength of 389 MPa, a yield strength of 282 MPa, and an elongation of 9.5% after 100 hours of heat exposure at 200℃.
[0058] Example 3
[0059] The raw material is a ZL205A aluminum alloy semi-continuous casting rod with a diameter of 120mm and a length of 0.5m. Its chemical composition is as follows: Cu: 5.53wt%; Mn: 0.38wt%; Cd: 0.21wt%; Ti: 0.20wt%; Zr: 0.17wt%; V: 0.18wt%; B: 0.008wt%; Mg: 0.003wt%; Zn: 0.001wt%; Fe: 0.02wt%; Si: 0.03wt%; with the balance being Al and unavoidable impurities, and the content of any single impurity is <0.001wt%.
[0060] After removing surface oxide scale and impurities, the semi-continuous casting bar is placed in a furnace and heated to 535℃, then held for 15 hours. It is then cooled to 440℃ and held for 4 hours. Subsequently, it undergoes radial rotary hot forging to reduce its diameter and length on a forging press, controlling the forging speed at 4 mm / s, with a single forging reduction of 8 mm. The final forging temperature is 380℃~420℃, until the bar billet diameter is reduced to 45 mm, at which point the billet length is approximately 3.5 m. The reduced-diameter and lengthened forged bar is then trimmed and cut into 160 mm long billets, which are placed in a holding furnace at 440℃ for 1 hour. After this holding period, hot rough forging is performed in a die forging mold. The rough forging is completed in one pass, with the forging direction perpendicular to the billet axis, a forging speed of 9 mm / s, and a final forging thickness 3.5 mm thicker than the final forged part's circular dimension. The final forging temperature is 400℃~420℃. After hot rough forging, the flash is removed directly on a trimming machine and then placed in a 410℃ furnace for 10 minutes. Hot finish forging is then performed in a die forging mold. The hot finish forging is completed in one pass at a forging speed of 6 mm / s. The final forging thickness is the same as the final forging circle size, and the final forging temperature is 380℃~400℃. The hot finish forged parts have their flash removed directly on the trimming machine and are then air-cooled to room temperature to obtain a fork-shaped hinge forging blank.
[0061] The precision-forged billet is rough-machined on a four-axis machining center. According to the final drawing dimensions, the rough-machined part retains a single-sided allowance of 0.6mm. The rough-machined part is then solution-treated in a 530℃ holding furnace for 3 hours, followed by room temperature quenching. After quenching, it is placed directly in an aging furnace at 175℃ for 10 hours without resting, and then air-cooled. The aging-treated part is then precision-machined on a four-axis machining center according to the final dimensions, ultimately yielding a 150mm long aluminum alloy fork-shaped hinge for commercial satellites.
[0062] The aluminum alloy fork hinge has a room temperature tensile strength of 476 MPa, a yield strength of 410 MPa, and an elongation of 11.4% in the longitudinal direction; a high temperature tensile strength of 382 MPa, a yield strength of 371 MPa, and an elongation of 10.3% at 200℃; and a room temperature tensile strength of 392 MPa, a yield strength of 281 MPa, and an elongation of 9.4% after 100 hours of heat exposure at 200℃.
[0063] Example 4
[0064] The raw material is a ZL205A aluminum alloy semi-continuous casting rod with a diameter of 100mm and a length of 0.5m. Its chemical composition is as follows: Cu: 5.53wt%; Mn: 0.38wt%; Cd: 0.21wt%; Ti: 0.20wt%; Zr: 0.17wt%; V: 0.18wt%; B: 0.008wt%; Mg: 0.003wt%; Zn: 0.001wt%; Fe: 0.02wt%; Si: 0.03wt%; the balance is Al and unavoidable impurities, and the content of a single impurity is <0.001wt%.
[0065] After removing the surface oxide scale and impurities from the semi-continuous casting bar, it is placed in a furnace and heated to 535℃ and held for 12 hours. Then, it is cooled to 450℃ and held for 4 hours. Subsequently, it undergoes radial rotary hot forging to reduce its diameter and length on a forging press, controlling the forging speed at 5 mm / s, with a single forging reduction of 5 mm, and a final forging temperature of 380℃~420℃, until the bar billet diameter is reduced to 46 mm, at which point the billet length is approximately 2.4 m. The reduced-diameter and lengthened forged bar is then trimmed and cut into 165 mm long billets, which are placed in a holding furnace at 450℃ and held for 1.5 hours. Afterward, it undergoes hot rough forging in a die forging mold. The rough forging is completed in one pass, with the forging direction perpendicular to the billet axis, a forging speed of 10 mm / s, and a final forging thickness 4 mm thicker than the final forged part's round dimension. The final forging temperature is 400℃~420℃. After hot rough forging, the flash is removed directly on a trimming machine and then placed in a 415℃ furnace for 8 minutes. Hot finish forging is then performed in a die forging mold. The hot finish forging is completed in one pass at a forging speed of 7 mm / s. The final forging thickness is the same as the final forging circle size, and the final forging temperature is 380℃~400℃. The hot finish forged parts have their flash removed directly on the trimming machine and then air-cooled to room temperature to obtain a fork-shaped hinge forging blank.
[0066] The forged billet was rough-machined on a four-axis machining center, with a single-sided allowance of 0.5mm retained according to the final drawing dimensions. The rough-machined part was then solution-treated in a 535℃ furnace for 2 hours, followed by room temperature quenching. After quenching, it was immediately placed in an aging furnace at 170℃ for 11 hours and then air-cooled. The aging-treated part was then finish-machined on a four-axis machining center according to the final dimensions, resulting in a 150mm long aluminum alloy fork-shaped hinge for commercial satellites.
[0067] The aluminum alloy fork hinge has a room temperature tensile strength of 475 MPa, a yield strength of 401 MPa, and an elongation of 12.4% in the longitudinal direction; a high temperature tensile strength of 376 MPa, a yield strength of 368 MPa, and an elongation of 10.4% at 200℃; and a room temperature tensile strength of 388 MPa, a yield strength of 282 MPa, and an elongation of 8.6% after 100 hours of heat exposure at 200℃.
[0068] Comparative Example 1
[0069] This comparative example is the same as Example 1, except that the heating temperature in the first stage of radial rotation hot forging and diameter reduction drawing is reduced to the same 450°C as the second stage. That is, hot forging and drawing are performed after holding at 450°C for 18 hours. During the drawing process, cracks occur at the head, and a large number of fine cracks are also generated radially. The main reason is that the purpose of holding in the first stage is to eliminate casting dendrites and achieve material composition homogenization. However, when the homogenization temperature is set to 450°C, the diffusion rate of alloying elements is slow. Even after 18 hours of holding, it is still difficult to eliminate dendrite segregation. The presence of these dendrites leads to a decrease in the plastic deformation ability of the alloy, resulting in cracking during the diameter reduction drawing process.
[0070] Comparative Example 2
[0071] This comparative example is the same as Example 1, except that the heating temperature before hot rough forging is increased to 500°C and the forging speed is increased to 20 mm / s. The increased deformation temperature enhances the material's plastic deformation capacity. Normally, to improve production efficiency, a higher forging speed can be used while still ensuring the integrity of the forging. In this comparative example, increasing the heating temperature and forging speed allows the rough forging process to be completed smoothly, and no cracks appear in the forging. However, the increase in these two parameters leads to a final forging temperature of 460°C. Such a high deformation and final forging temperature results in significant recrystallization grain growth, as shown in the attached figure. Figure 7 As shown, the final fork-shaped hinge has a room temperature tensile strength of only 416 MPa, a yield strength of only 325 MPa, and an elongation of 10.7%, which cannot meet the design requirements under operating conditions.
[0072] Comparative Example 3
[0073] This comparative example is the same as Example 1, except that the heating temperature for hot forging is increased to 480°C and the forging speed is increased to 15 mm / s. In this comparative example, the increased heating temperature and forging speed allow for successful forging without cracking of the forging. However, the increase in these two parameters leads to a final forging temperature of 450°C. Such high deformation and final forging temperatures result in significant grain growth during material recrystallization. The final forked hinge exhibits a room temperature tensile strength of only 425 MPa, a yield strength of only 340 MPa, and an elongation of 9.6%, which fails to meet the design requirements under operating conditions.
[0074] Comparative Example 4
[0075] This comparative example is the same as Example 1, except that the forged fork hinge blank is first rough-machined and then finished before heat treatment. In actual testing, it was found that after finishing and before heat treatment, the dimensions of the fork hinge fully met the design requirements of the drawings. However, after heat treatment, re-measuring revealed that the flatness of some thin-walled areas deteriorated, and the parts exhibited slight deformation, rendering them unusable. The main reason for this was that the rapid cooling during the quenching process caused residual stress inside the parts. This residual stress was insufficient to cause deformation in the thick-walled areas, but deformation occurred in the thin-walled areas due to their lower load-bearing capacity.
[0076] Comparative Example 5
[0077] This comparative example is the same as Example 1, except that the solution temperature is set to 450°C. Because the alloying elements failed to fully dissolve into the matrix, precipitation occurred during the subsequent aging process. The number of reinforcing phases is significantly reduced, while coarse undissolved second phases remain. Under the combined influence of these two factors, the strength and plasticity of the fork hinge are reduced. The room temperature tensile strength in the length direction is only 420 MPa, the yield strength is only 332 MPa, and the elongation is only 7.3%, which cannot meet the design requirements under the service conditions.
[0078] Comparative Example 6
[0079] This comparative example is the same as Example 1, except that the solution temperature is set to 550°C. After quenching, small bubbles appear on the surface of the part, indicating that overheating has occurred, and the part is scrapped.
Claims
1. A method for manufacturing a heat-resistant aluminum alloy fork-shaped hinge for commercial satellites, characterized in that: A heat-resistant aluminum alloy semi-continuous casting rod is radially rotated and hot-forged to reduce its diameter and length to obtain a forged rod. The forged rod is then cut into sections, and the resulting billet is heated to 430℃~450℃ and held for 1~1.5h before rough forging to obtain a hot rough forging. The flash of the hot rough forging is removed directly without cooling. Then, it is held at 400℃~420℃ for 5~10min before hot precision forging to obtain a hot precision forging. The flash of the hot precision forging is removed directly without cooling, and then it is air-cooled to room temperature to obtain a forked hinge precision forging billet. The forked hinge precision forging billet is then rough-machined and then subjected to T6 heat treatment. After T6 heat treatment, it is precision-machined to the final dimensions to obtain a heat-resistant aluminum alloy forked hinge.
2. The method for preparing a heat-resistant aluminum alloy fork hinge for commercial satellites according to claim 1, characterized in that: The heat-resistant aluminum alloy fork hinge has the following composition by weight percentage: Cu: 4.8~5.6wt%; Mn: 0.3~0.5wt%; Cd: 0.15~0.25wt% Ti: 0.18~0.25wt%; Zr: 0.1~0.2wt% V: 0.15~0.3wt%; B: 0.005~0.06wt%; Mg≤0.01wt%; Zn≤0.01wt%; Fe≤0.03wt%; Si≤0.05wt%; balance is Al and unavoidable impurities.
3. The method for preparing a heat-resistant aluminum alloy fork-shaped hinge for commercial satellites according to claim 1, characterized in that: The diameter of the heat-resistant aluminum alloy semi-continuous casting rod is 100mm~120mm.
4. The method for preparing a heat-resistant aluminum alloy fork hinge for commercial satellites according to claim 1, characterized in that: Before radial rotation hot forging, the diameter reduction and drawing process is preheated. The preheating process is as follows: first, heat the heat-resistant aluminum alloy semi-continuous casting rod to 530℃~540℃ and hold it for 12~15h, then cool it down to 430℃~450℃ and hold it for 3~5h.
5. The method for preparing a heat-resistant aluminum alloy fork hinge for commercial satellites according to claim 1, characterized in that: During the radial rotation hot forging reduction and elongation process, the forging speed is controlled at 3~5 mm / s, the single forging reduction is 5 mm~10 mm, and the final forging temperature is 380℃~420℃; the diameter of the forging bar is 45 mm~48 mm.
6. The method for preparing a heat-resistant aluminum alloy fork-shaped hinge for commercial satellites according to claim 1, characterized in that: The hot rough forging is completed in one pass, with the forging direction perpendicular to the axial direction of the billet to be forged, the forging speed being 8~10 mm / s, and the final forging temperature being 400℃~420℃. During the hot rough forging process, the final forging thickness is controlled to be 3-4 mm thicker than the final forging circle size.
7. The method for preparing a heat-resistant aluminum alloy fork-shaped hinge for commercial satellites according to claim 1, characterized in that: The hot precision forging is completed in one pass, with a forging speed of 5~8 mm / s and a final forging temperature of 380℃~400℃. During the hot precision forging process, the final forging thickness is controlled to be the same as the final forging circle size.
8. The method for preparing a heat-resistant aluminum alloy fork hinge for commercial satellites according to claim 1, characterized in that: During the rough machining process, a single-sided allowance of 0.5mm to 0.8mm is retained to obtain a rough-machined fork-shaped hinge part.
9. The method for preparing a heat-resistant aluminum alloy fork hinge for commercial satellites according to claim 1, characterized in that: The T6 heat treatment process is as follows: first, solution treatment is performed; after the solution treatment is completed, quenching is performed at room temperature; and then artificial aging is performed. The solution treatment temperature is 520℃~540℃, and the solution treatment time is 2~3h; The temperature for artificial aging is 165℃~180℃, and the aging time is 8~12h.
10. A method for preparing a heat-resistant aluminum alloy fork-shaped hinge for commercial satellites according to any one of claims 1-9, characterized in that: The heat-resistant aluminum alloy fork hinge has a room temperature tensile strength ≥460MPa, a yield strength ≥370MPa, and an elongation ≥10% in the length direction; a high temperature tensile strength ≥370MPa, a yield strength ≥350MPa, and an elongation ≥9% at 200℃; and a room temperature tensile strength ≥380MPa, a yield strength ≥270MPa, and an elongation ≥8% after 100h of heat exposure at 200℃.