An aging-resistant composite sound insulation and noise reduction material and its preparation method
Through a three-layer structure design and nano-modification treatment, the aging resistance and sound insulation effect of aluminum foam composite materials are improved, solving the problem of performance degradation caused by photo-oxidative aging in outdoor use and achieving long-lasting sound insulation and noise reduction effect.
Patent Information
- Application Number
- CN202611260299.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aluminum foam-based composite sound insulation materials are prone to sound insulation and noise reduction performance degradation and shortened service life when used outdoors for a long time due to photo-oxidative aging, powdering, cracking, etc., and lack long-term weather protection.
It adopts a three-layer structure design: the surface layer is a nano-modified weather-resistant coating, the middle layer is a high-damping viscoelastic damping layer, and the core layer is a foamed aluminum layer. The aging resistance and sound insulation and noise reduction effect of the material are improved through nano-modification treatment and composite process.
It maintains stable sound insulation and noise reduction performance during long-term outdoor use, improves the material's weather resistance and damping performance, and extends its service life.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of sound insulation materials technology, and relates to an aging-resistant composite sound insulation and noise reduction material and its preparation method. Background Technology
[0002] Sound insulation and noise reduction materials are widely used in building sound insulation, transportation, ships, aerospace, and industrial equipment, playing a vital role in improving the living environment and ensuring the normal operation of equipment. These materials not only need to possess excellent broadband sound insulation and noise reduction performance, but also require lightweight, high strength, flame retardancy, and weather resistance, maintaining stable acoustic performance during long-term outdoor use.
[0003] As a new type of lightweight and multifunctional material, aluminum foam has the characteristics of low density, high specific strength and specific stiffness, good damping performance and excellent sound absorption and insulation performance, and has received widespread attention in the field of sound insulation and noise reduction in recent years.
[0004] However, existing aluminum foam-based composite sound insulation materials still have the following shortcomings: lack of long-term weather-resistant protection design. When the aluminum foam composite structure is used outdoors for a long time, the surface is directly exposed to natural environments such as sunlight (ultraviolet rays), rain, and temperature changes, which easily leads to photo-oxidative aging, powdering, cracking and other deterioration phenomena, which in turn leads to the decay of the overall sound insulation and noise reduction performance and the shortening of service life, making it difficult to achieve true long-term continuous protection.
[0005] Therefore, there is an urgent need to develop a sound insulation material with excellent aging resistance. Summary of the Invention
[0006] The purpose of this invention is to provide an aging-resistant composite sound insulation and noise reduction material and its preparation method. The prepared material has excellent aging resistance and sound insulation and noise reduction properties.
[0007] The objective of this invention can be achieved through the following technical solutions: An aging-resistant composite sound insulation and noise reduction material, the material comprising a surface layer, a middle layer and a core layer stacked sequentially; The surface layer is a nano-modified weather-resistant coating, which contains the following raw materials in parts by weight: 5-30 parts of nano-SiO2 modified with polyamine compounds, 5-15 parts of modified nano-hollow glass microspheres, and 70-85 parts of resin matrix. The modified hollow glass nanospheres are hollow glass nanospheres with an inner cavity loaded with an ultraviolet absorber and a shell layer hydrolyzed with tetraethyl orthosilicate. Their particle size is 100 nm to 5 μm and their wall thickness is 100 to 500 nm. The intermediate layer is a high-damping viscoelastic damping layer, which contains the following raw materials in parts by weight: 50-80 parts of matrix rubber, 10-30 parts of damping reinforcing resin, and 5-20 parts of sheet filler. The core layer is a foamed aluminum layer.
[0008] The sound insulation and noise reduction material of this invention has a three-layer structure: the surface layer resists photothermal aging and protects the middle and core layers; the middle layer absorbs and dissipates vibration energy, reducing structural noise transmission; and the core layer, as the main structure, provides excellent sound absorption and insulation performance. The three layers work together to ensure that the material maintains stable and efficient sound insulation and noise reduction performance during long-term outdoor use.
[0009] As a preferred embodiment of the present invention, the polyamine compound is at least one of polyethyleneimine, polyallylamine, or polyethyleneamine, and the preparation of nano-SiO2 modified with the polyamine compound includes the following steps: Nano-silica was dispersed in a solvent to obtain a nano-silica dispersion. A polyamine compound was added, and the mixture was stirred at 20-80°C for 12-24 hours. After the mixture was completed, it was separated, washed, and dried to obtain modified nano-silica.
[0010] This method uses polyamine compounds (such as polyethyleneimine) to complete the modification in one step through physical adsorption and hydrogen bonding under ambient temperature and aqueous phase conditions. The process is simple and the conditions are mild (ambient temperature and aqueous phase), requiring no organic solvents or catalysts.
[0011] The surface of the polyethyleneimine coating is rich in amino functional groups. These amino groups can chemically react with the resin matrix (such as epoxy groups of epoxy resin, isocyanate groups of polyurethane, and carboxyl groups of acrylic resin) during the coating curing process to form covalent bonds. The chemical cross-linking network formed by modified nano-SiO2 in the surface coating enhances the cohesive strength of the surface layer, while the interfacial bonding between the surface layer and the intermediate damping layer is stronger, making interlayer delamination less likely. The dispersibility of nano-SiO2 in the coating is significantly improved, effectively preventing nanoparticle aggregation. The surface layer maintains excellent UV shielding capability for a long time, effectively blocking UV penetration and protecting the intermediate damping layer from cross-linking or degradation caused by UV radiation. This ensures that the three-layer composite structure maintains stable sound insulation and noise reduction performance during long-term outdoor use.
[0012] As a preferred embodiment of the present invention, the resin matrix is selected from at least one of fluorocarbon resin, polyurethane resin or acrylic resin.
[0013] As a preferred embodiment of the present invention, the base rubber is one or more of butyl rubber, chlorinated butyl rubber, nitrile rubber, chloroprene rubber, or silicone rubber.
[0014] As a preferred embodiment of the present invention, the damping reinforcing resin is one or more of phenolic resin, epoxy resin, or petroleum resin.
[0015] As a preferred embodiment of the present invention, the sheet-like filler is one or more of mica powder, graphene nanosheets, or montmorillonite.
[0016] In this invention, the sheet-like filler can be oriented in the damping layer to form a layered barrier structure, which can effectively extend the propagation path of sound waves and gases in the material and improve the sound insulation effect. Furthermore, the sheet-like filler generates relative slippage and friction between the layers during vibration, which significantly enhances the damping performance. The matrix rubber provides basic damping performance, the damping-enhancing resin regulates the glass transition temperature range, and the sheet-like filler enhances energy dissipation through interlayer slippage and internal friction. The three work together to enable the damping layer to maintain high damping performance over a wide temperature range, thereby improving the noise reduction effect.
[0017] As a preferred embodiment of the present invention, the preparation process of the modified hollow glass nanospheres is as follows: Disperse nano-hollow glass microspheres in a 0.5-2% hydrofluoric acid solution at a solid-liquid ratio of 1:5-20 g / mL, stir at 20-30℃ for 1-10 min, wash with deionized water until neutral, and vacuum dry at 60-80℃ for 12-24 h to obtain product A. Product A was dispersed in an ethanol solution of 2-hydroxy-4-methoxybenzophenone, with a mass-to-volume ratio of 2-hydroxy-4-methoxybenzophenone to anhydrous ethanol of 1:10~50 g / mL and a mass ratio of 2-hydroxy-4-methoxybenzophenone to nano-hollow glass microspheres of (0.2~1):1. The solution was evacuated to -0.08~-0.1 MPa at 20~30℃ and maintained for 2~6 h. After restoring to normal pressure, the solution was soaked for another 12~24 h. The product was then centrifuged, washed with ethanol, and dried under vacuum at 50~70℃ for 6~12 h to obtain product B. Tetraethyl orthosilicate, anhydrous ethanol, and deionized water were mixed in a molar ratio of 1:(20~40):(2~8), and ammonia was added to adjust the pH to 8~10. The mixture was stirred at 40~60℃ for 2~6 hours, washed 2~3 times with anhydrous ethanol and deionized water, and then vacuum dried at 60~80℃ for 12~24 hours to obtain the modified hollow glass nanospheres.
[0018] In the preparation of modified hollow glass microspheres, the present invention first uses HF etching to form nanoscale microporous channels on the surface of the hollow microsphere shell, providing a pathway for the entry of ultraviolet absorbers while preserving the overall structural integrity of the microspheres; then, after being subjected to vacuum negative pressure loading (-0.08~-0.1MPa, 2~6h), the ultraviolet absorber solution enters the inner cavity under the pressure difference driven by the pressure difference, achieving efficient and uniform loading.
[0019] Tetraethyl orthosilicate hydrolysis sealing is used to deposit a thin layer of SiO2 on the outer surface of hollow glass microspheres, which partially blocks the etched channels and enables the controlled and slow release of the ultraviolet absorber. This solves the problem of rapid failure of traditional ultraviolet absorbers that are directly dispersed in the coating due to migration, volatilization and photodegradation, and gives the surface a long-lasting ultraviolet protection capability.
[0020] As a preferred embodiment of the present invention, the aluminum foam layer is a closed-cell aluminum foam layer or an open-cell aluminum foam layer, the thickness of the aluminum foam layer is 5~50mm, the thickness of the surface layer is 50~500μm, and the thickness of the intermediate layer is 0.5~10mm.
[0021] The high porosity and unique pore structure of aluminum foam endow the material with excellent sound absorption and insulation properties, while also being lightweight and having high specific stiffness. As a core layer, it provides both structural load-bearing and sound insulation functions. The aluminum foam layer thickness is 5~50mm: ensuring sufficient structural strength and sound absorption and insulation performance, while avoiding excessive weight due to excessive thickness; the surface layer thickness is 50~500μm: ensuring sufficient weather resistance without affecting the overall material's flexibility and acoustic properties; too thin a layer provides insufficient protection, while too thick a layer increases cost and may cause coating cracking; the intermediate layer thickness is 0.5~10mm, ensuring sufficient damping energy dissipation capacity while controlling the overall thickness and weight.
[0022] A method for preparing an aging-resistant composite sound insulation and noise reduction material includes the following steps: S1. Surface pretreatment of aluminum foam layer: The surface of the aluminum foam layer near the middle layer is acid-etched or sandblasted to achieve a surface roughness Ra of 5~50μm, and then cleaned and dried. S2. Preparation of high-damping viscoelastic damping layer: The matrix rubber, damping reinforcing resin and sheet filler are mixed in parts by weight and kneaded to obtain a high-damping viscoelastic material. The high-damping viscoelastic material is then composited onto the surface of the pretreated aluminum foam layer in step S1 by hot pressing. The hot pressing temperature is 120~200℃, the hot pressing pressure is 1~10MPa, and the hot pressing time is 5~30min to obtain an aluminum foam-damping layer composite. S3. Preparation of nano-modified weather-resistant coatings: Modified nano-silica, ultraviolet absorber, modified nano-hollow glass microspheres are mixed with resin matrix and dispersed at high speed to obtain nano-modified weather-resistant coating. S4. Surface coating and curing: The nano-modified weather-resistant coating obtained in step S3 is coated onto the surface of the damping layer of the aluminum foam-damping layer composite obtained in step S2, and then cured at 30~150℃ for 24~48h to obtain the aging-resistant composite sound insulation and noise reduction material.
[0023] As a preferred embodiment of the present invention, the acid etching treatment uses a hydrochloric acid solution with a mass fraction of 5-20% and a treatment time of 1-10 minutes; the sandblasting treatment uses corundum sand with a mesh size of 60-200 and a sandblasting pressure of 0.3-0.8 MPa.
[0024] Through the above pretreatment, the interfacial bonding strength between the damping layer and the aluminum foam core layer is significantly improved, ensuring that vibration energy is effectively transferred from the core layer to the damping layer for dissipation, and giving full play to the synergistic sound insulation and noise reduction effect of the three-layer structure.
[0025] This invention first roughens the surface of aluminum foam to form a micro-uneven structure, significantly increasing the contact area and mechanical anchoring force with the damping layer, effectively solving the industry problems of easy oxidation of aluminum foam surface and insufficient adhesion strength with organic materials; then, through hot pressing (120~200℃, 1~10MPa, 5~30min), under heating and pressurization conditions, the high-damping viscoelastic material forms a strong chemical and physical bond with the aluminum foam surface; the hot pressing temperature, pressure and time parameters are optimized to ensure sufficient interface fusion and structural integrity without damaging the pore structure of aluminum foam.
[0026] The beneficial effects of this invention are: (1) The present invention adopts a composite structure of three layers stacked sequentially: "surface layer-middle layer-core layer" to achieve weather protection, damping energy dissipation and sound insulation; the surface layer is a nano-modified weather-resistant coating, in which nano-SiO2 modified by polyamine compounds forms a highly active coating layer rich in amino groups on the particle surface through physical adsorption and hydrogen bonding, which not only significantly improves the dispersion of nano-SiO2 in the resin matrix, but also allows a large number of amino functional groups on its surface to undergo chemical cross-linking reaction with the resin matrix during the coating curing process.
[0027] (2) The modified hollow glass microspheres filled in the surface layer of the present invention are modified in three steps: hydrofluoric acid etching to create pores, vacuum negative pressure loading of ultraviolet absorber, and hydrolysis sealing of tetraethyl orthosilicate. The ultraviolet absorber is physically encapsulated in the inner cavity of the hollow glass microspheres and is released slowly and controllably through the nanopores partially blocked by the shell layer, giving the surface layer long-lasting ultraviolet protection capability and improving aging resistance.
[0028] (3) The intermediate layer uses matrix rubber to provide basic damping performance, damping-enhancing resin to regulate the glass transition temperature range, and sheet filler to enhance energy dissipation through interlayer slip and internal friction; the core layer uses high-porosity foam aluminum as the main structure to provide excellent sound absorption and insulation performance. The three-layer structure works together to ensure that the material maintains stable and efficient sound insulation and noise reduction performance during long-term outdoor use. Detailed Implementation
[0029] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with embodiments, is provided below.
[0030] It should be noted that in the following examples and comparative examples, the fluorocarbon resin is ZHM-2; nano silica is from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., item number: 100361, item number: XFI03; polyethyleneimine is from Shanghai Maclean Biochemical Technology Co., Ltd., product number: E890305; nano hollow glass microspheres are from Hebei Sainade Nanomaterials Technology Co., Ltd., item number: 1; butyl rubber is from Nantong Runfeng Petrochemical Co., Ltd.; and mica powder is from Wuhan Jiyesheng Chemical Co., Ltd., item number: W01264. Unless otherwise specified, the present invention does not specifically limit the source of other raw materials used. Commercially available products or products prepared by conventional preparation methods that are well known to those skilled in the art can be used. Experimental methods that do not specify specific conditions are all conventional methods and conditions well known in the art.
[0031] Example 1
[0032] Nano-silica was dispersed in deionized water to obtain a nano-silica dispersion. Polyethyleneimine was added, with a mass ratio of polyethyleneimine to nano-silica of 0.3:1. The mixture was stirred at 50°C for 19 hours. After the mixture was completed, it was separated, washed three times with deionized water, and vacuum dried at 60°C for 12 hours to obtain modified nano-silica.
[0033] The hollow glass nanospheres were dispersed in a 1% hydrofluoric acid solution at a solid-liquid ratio of 1:10 g / mL, stirred at 25°C for 6 min, washed with deionized water until neutral, and dried under vacuum at 70°C for 18 h to obtain product A. Product A was dispersed in an ethanol solution of 2-hydroxy-4-methoxybenzophenone, with a mass-to-volume ratio of 2-hydroxy-4-methoxybenzophenone to anhydrous ethanol of 1:30 g / mL and a mass ratio of 2-hydroxy-4-methoxybenzophenone to nano-hollow glass microspheres of 0.6:1. The solution was evacuated to -0.1 MPa at 25 °C for 4 h, and then soaked for another 16 h after returning to normal pressure. The product was then centrifuged, washed with ethanol, and dried under vacuum at 60 °C for 9 h to obtain product B. Tetraethyl orthosilicate, anhydrous ethanol, and deionized water were mixed in a molar ratio of 1:30:5. Ammonia was added to adjust the pH to 9. The mixture was stirred at 50°C for 4 hours, washed three times with anhydrous ethanol and deionized water, and then vacuum dried at 70°C for 18 hours to obtain the modified hollow glass nanospheres.
[0034] S1. Surface pretreatment of aluminum foam layer: The surface of the open-cell aluminum foam layer near the middle layer was acid-etched using a 15% hydrochloric acid solution for 10 minutes, then cleaned and dried to achieve a surface roughness Ra of 30 μm. S2. Preparation of high-damping viscoelastic damping layer: 60 parts of butyl rubber, 20 parts of epoxy resin and 12 parts of mica powder were mixed and kneaded to obtain a high-damping viscoelastic material; the high-damping viscoelastic material was then composited onto the surface of the pretreated aluminum foam layer in step S1 by hot pressing at a temperature of 160°C, a pressure of 5 MPa and a time of 20 min to obtain an aluminum foam-damping layer composite. S3. Preparation of nano-modified weather-resistant coatings: 20 parts of nano-SiO2, 10 parts of modified nano-hollow glass microspheres, 75 parts of fluorocarbon resin, and 4 parts of curing agent (Desmodur N3390) were dispersed and mixed at high speed to obtain a nano-modified weather-resistant coating. S4. Surface coating and curing: The nano-modified weather-resistant coating obtained in step S3 is coated on the surface of the damping layer of the aluminum foam-damping layer composite obtained in step S2, and then cured at 80°C for 36 hours to obtain an aging-resistant composite sound insulation and noise reduction material.
[0035] In this embodiment, the thickness of the aluminum foam layer is 20 mm, the thickness of the surface layer is 200 μm, and the thickness of the intermediate layer is 4 mm.
[0036] Example 2
[0037] This embodiment is basically the same as Example 1, except that: The composition includes 80 parts butyl rubber, 30 parts epoxy resin, 20 parts mica powder, 30 parts modified nano-SiO2, 15 parts modified nano-hollow glass microspheres, and 85 parts fluorocarbon resin.
[0038] Example 3
[0039] This embodiment is basically the same as Example 1, except that: 50 parts butyl rubber, 10 parts epoxy resin, 5 parts mica powder, 5 parts modified nano-SiO2, 5 parts modified nano-hollow glass microspheres, and 70 parts fluorocarbon resin.
[0040] Example 4
[0041] This embodiment is basically the same as Example 1, except that: The resin matrix is polyurethane resin, the matrix rubber is nitrile rubber, and the sheet filler is graphene nanosheets (Xianfeng Nano, XF021).
[0042] Example 5
[0043] It is basically the same as Example 1, except that the pretreatment in step S1 is sandblasting, using 120-mesh corundum sand, and the sandblasting pressure is 0.5MPa.
[0044] Comparative Example 1 It is basically the same as Example 1, except that no modified nano-hollow glass microspheres are added to the surface layer of this comparative example.
[0045] Comparative Example 2 It is basically the same as Example 1, except that the surface layer of this comparative example is made of ordinary hollow glass nanospheres that have not been modified in any way.
[0046] Comparative Example 3 This is basically the same as Example 1, except that the surface layer of this comparative example is modified with KH-570 silane coupling agent and contains nano-SiO2.
[0047] Comparative Example 4 This is basically the same as Example 1, except that the surface layer of this comparative example is made of unmodified nano-SiO2.
[0048] Comparative Example 5 This comparative example is basically the same as Example 1, except that it does not have an intermediate high-damping viscoelastic damping layer, and the nano-modified weather-resistant coating is directly coated on the surface of the aluminum foam layer.
[0049] Comparative Example 6 This is basically the same as Example 1, except that the surface layer of this comparative example is a common fluorocarbon varnish coating (without modified nano-SiO2 and modified nano-hollow glass microspheres), and the thickness is the same as that of Example 1.
[0050] Performance testing: 1. UV aging resistance test: Refer to GB / T 23987-2009; Test conditions: UVA-340 lamp, irradiance 0.89 W / (m²) 2 The UV-Vis absorbance at 340 nm was measured using a UV-Vis spectrophotometer. The aging conditions were 4 hours of light exposure at 60°C and 4 hours of condensation at 50°C. The total aging time was 500 hours. The retention rate of UV absorbance at 400 nm was calculated as follows: Retention rate (%) = (Absorbance after aging / Absorbance before aging) * 100%. 2. Salt spray resistance: Referring to GB / T 1771-2007 "Determination of resistance to neutral salt spray of paints and varnishes", the test conditions were: 50 g / L NaCl solution, pH 6.5~7.2, temperature 35℃, continuous spraying for 240 h. The surface condition of the coating was observed after the test, and the results are shown in Table 1 below: Table 1
[0051] As shown in Table 1, the UV absorption capacity retention rate of Example 1 is much higher than that of Comparative Examples 1 and 2, indicating that during the coating application process, the modified hollow glass microspheres used in this invention allow the UV absorber in the inner cavity to be slowly and continuously released into the coating through the sealed pore channels of the shell, providing long-lasting UV protection. Example 5 has the same retention rate as Example 1, indicating that different pretreatment methods have no effect on the surface UV resistance.
[0052] Comparative Example 1 contained no hollow microspheres at all; the small amount of UV absorber it contained was merely a trace additive that might remain in the coating formulation and had no continuous replenishment capability. The unmodified hollow microspheres in Comparative Example 2 exhibited weak UV resistance. The retention rate of Comparative Example 3 was 90.0%, similar to that of Example 1 (90.8%), indicating that PEI modification had no negative impact on the UV absorption function.
[0053] In Comparative Example 4, the unmodified nano-SiO2 surface lacks amino functional groups, making it unable to form chemical cross-links with the resin matrix. As a result, the coating has poor density, and the UV absorber is rapidly lost as the coating deteriorates.
[0054] The retention rate of Comparative Example 6 (ordinary fluorocarbon varnish) was only 70.0%, indicating that ordinary varnish without any functional fillers is prone to deterioration and failure under ultraviolet irradiation.
[0055] Examples 1-5 showed excellent salt spray resistance after 240 hours of salt spray testing, with the coatings remaining intact, free from blistering, rust, and peeling. Comparative Example 6 (ordinary fluorocarbon varnish) showed extensive blistering and localized peeling after the salt spray test, indicating that the synergistic addition of modified nano-SiO2 and modified nano-hollow glass microspheres significantly improved the coating's density and resistance to corrosive media penetration. Comparative Example 3 showed minor blistering at the coating edges, indicating that its coating density was not as good as that of the present invention. Comparative Example 4 showed multiple blistering and localized rust in the coating, indicating that the unmodified nano-SiO2 had poor dispersion in the coating, forming agglomerates. These agglomerates created microscopic defects and pores, thus reducing aging resistance.
[0056] 3. Sound insulation: Referring to GB / T 19889.3-2005 "Acoustics of Buildings and Building Components - Measurement of Sound Insulation - Part 3: Laboratory Measurement of Airborne Sound Insulation of Building Components", the sound transmission loss (sound insulation) of the composite material was tested using the impedance tube method (referring to GB / T 18696.2-2002). The sound transmission loss values (dB) at five frequency points (500Hz, 1000Hz, 2000Hz, and 4000Hz) were recorded. The results are shown in Table 2 below. Table 2
[0057] According to the data in Table 2, the content of each component in Example 2 is the highest and the surface density is the largest. Therefore, the sound insulation is slightly stronger than that in Example 1. The components in Example 4 are different, but the performance is still at a high level. The sandblasting pretreatment in Example 5 is equivalent to the acid etching pretreatment and is basically the same as that in Example 1.
[0058] In Comparative Example 1, the unmodified hollow microspheres lacked the contribution of hollow spheres to scatter sound waves, thus reducing sound insulation. Comparative Example 2 had worse sound insulation than Comparative Example 1 because the negative effect of the unmodified hollow microspheres reducing the surface density outweighed the positive effect of scattering sound waves, leading to a decrease in sound insulation. In Comparative Example 3, KH-570 only provided a single layer of double bonds, resulting in low crosslinking density. In Comparative Example 4, the unmodified SiO2 had poor dispersion and agglomeration, and no chemical bonding with the resin. Comparative Example 5 had no damping layer, thus exhibiting the worst sound insulation. In Comparative Example 6, the varnish had no fillers and the lowest surface density, thus reducing sound insulation.
[0059] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. An aging-resistant composite sound insulation and noise reduction material, characterized in that, The material comprises a surface layer, an intermediate layer, and a core layer that are stacked sequentially. The surface layer is a nano-modified weather-resistant coating, which contains the following raw materials in parts by weight: 5-30 parts of nano-SiO2 modified with polyamine compounds, 5-15 parts of modified nano-hollow glass microspheres, and 70-85 parts of resin matrix. The modified hollow glass nanospheres are hollow glass nanospheres with an inner cavity loaded with an ultraviolet absorber and a shell layer hydrolyzed with tetraethyl orthosilicate. Their particle size is 100 nm to 5 μm and their wall thickness is 100 to 500 nm. The intermediate layer is a high-damping viscoelastic damping layer, which contains the following raw materials in parts by weight: 50-80 parts of matrix rubber, 10-30 parts of damping reinforcing resin, and 5-20 parts of sheet filler. The core layer is a foamed aluminum layer.
2. The aging-resistant composite sound insulation and noise reduction material according to claim 1, characterized in that, The polyamine compound is at least one of polyethyleneimine, polyallylamine, or polyethyleneamine. The preparation of nano-SiO2 modified with the polyamine compound includes the following steps: Nano-silica was dispersed in a solvent to obtain a nano-silica dispersion. A polyamine compound was added, and the mixture was stirred at 20-80°C for 12-24 hours. After the mixture was completed, it was separated, washed, and dried to obtain modified nano-silica.
3. The aging-resistant composite sound insulation and noise reduction material according to claim 1, characterized in that, The resin matrix is selected from at least one of fluorocarbon resin, polyurethane resin, or acrylic resin.
4. The aging-resistant composite sound insulation and noise reduction material according to claim 1, characterized in that, The base rubber is one or more of butyl rubber, chlorinated butyl rubber, nitrile rubber, chloroprene rubber, or silicone rubber.
5. The aging-resistant composite sound insulation and noise reduction material according to claim 1, characterized in that, The damping reinforcing resin is one or more of phenolic resin, epoxy resin, or petroleum resin.
6. The aging-resistant composite sound insulation and noise reduction material according to claim 1, characterized in that, The sheet-like filler is one or more of mica powder, graphene nanosheets, or montmorillonite.
7. The aging-resistant composite sound insulation and noise reduction material according to claim 1, characterized in that, The preparation process of the modified hollow glass nanospheres is as follows: Disperse nano-hollow glass microspheres in a 0.5-2% hydrofluoric acid solution at a solid-liquid ratio of 1:5-20 g / mL, stir at 20-30℃ for 1-10 min, wash with deionized water until neutral, and vacuum dry at 60-80℃ for 12-24 h to obtain product A. Product A was dispersed in an ethanol solution of 2-hydroxy-4-methoxybenzophenone, with a mass-to-volume ratio of 2-hydroxy-4-methoxybenzophenone to anhydrous ethanol of 1:10~50 g / mL and a mass ratio of 2-hydroxy-4-methoxybenzophenone to nano-hollow glass microspheres of (0.2~1):
1. The solution was evacuated to -0.08~-0.1 MPa at 20~30℃ and maintained for 2~6 h. After restoring to normal pressure, the solution was soaked for another 12~24 h. The product was then centrifuged, washed with ethanol, and dried under vacuum at 50~70℃ for 6~12 h to obtain product B. Tetraethyl orthosilicate, anhydrous ethanol, and deionized water were mixed in a molar ratio of 1:(20~40):(2~8), and ammonia was added to adjust the pH to 8~10. After stirring for 2~6 hours, the mixture was washed and dried to obtain the modified hollow glass nanospheres.
8. The aging-resistant composite sound insulation and noise reduction material according to claim 1, characterized in that, The aluminum foam layer is a closed-cell aluminum foam layer or an open-cell aluminum foam layer, the thickness of the aluminum foam layer is 5~50mm, the thickness of the surface layer is 50~500μm, and the thickness of the intermediate layer is 0.5~10mm.
9. A method for preparing an aging-resistant composite sound insulation and noise reduction material as described in any one of claims 1-8, characterized in that, Includes the following steps: S1. Surface pretreatment of aluminum foam layer: The surface of the aluminum foam layer near the middle layer is acid-etched or sandblasted to achieve a surface roughness Ra of 5~50μm, and then cleaned and dried. S2. Preparation of a high-damping viscoelastic damping layer: The matrix rubber, damping reinforcing resin and sheet filler are mixed in parts by weight and kneaded to obtain a high-damping viscoelastic material. The high-damping viscoelastic material is then composited onto the surface of the pretreated aluminum foam layer in step S1 by hot pressing. The hot pressing temperature is 120~200℃, the hot pressing pressure is 1~10MPa, and the hot pressing time is 5~30min to obtain an aluminum foam-damping layer composite. S3. Preparation of nano-modified weather-resistant coatings: Modified nano-silica, ultraviolet absorber, modified nano-hollow glass microspheres and resin matrix are dispersed and mixed at high speed to obtain nano-modified weather-resistant coating; S4. Surface coating and curing: The nano-modified weather-resistant coating obtained in step S3 is coated onto the surface of the damping layer of the aluminum foam-damping layer composite obtained in step S2, and then cured at 30~150℃ for 24~48h to obtain the aging-resistant composite sound insulation and noise reduction material.
10. The method for preparing the aging-resistant composite sound insulation and noise reduction material according to claim 9, characterized in that, The acid etching treatment uses a hydrochloric acid solution with a mass fraction of 5-20% and a treatment time of 1-10 minutes; the sandblasting treatment uses corundum sand with a mesh size of 60-200 and a sandblasting pressure of 0.3-0.8 MPa.