A method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid
By using citric acid compounds to assist precipitation in the acid leaching solution of sludge ash and iron-containing wastewater, and by treating with copper powder and iodide reducing agents, the problems of insufficient phosphorus and iron purity and arsenic impurity removal in sludge incineration ash were solved, achieving efficient preparation of battery-grade iron phosphate and reducing costs and waste emissions.
Patent Information
- Application Number
- CN202611414020.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to effectively utilize sludge incineration ash to prepare battery-grade iron phosphate. The purity of phosphorus and iron sources is insufficient, and the removal of arsenic impurities is difficult, making it hard to meet battery-grade purity requirements.
By mixing and stirring sludge ash acid leaching solution and iron-containing waste liquid, and then using citric acid compounds to assist precipitation and acid-base treatment, combined with the synergistic effect of copper powder, iodide and reducing agent, phosphorus and iron can be recovered and purified simultaneously, and arsenic impurities can be deeply removed.
It achieves battery-grade purity of iron phosphate, shortens the process flow, improves purification efficiency, reduces reagent consumption and secondary waste, and lowers production costs.
Smart Images

Figure CN123105577A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of waste resource utilization technology, specifically relating to a method for preparing iron phosphate using sludge ash acid leaching solution and iron-containing waste liquid. Background Technology
[0002] Battery-grade iron phosphate, as a key precursor for lithium iron phosphate cathode materials, directly determines the economics of power batteries and energy storage systems through its production cost control and supply stability. It is a crucial foundation for the large-scale development of the new energy vehicle and energy storage industries. Currently, the industry primarily uses high-purity iron sources (such as ferrous sulfate) and phosphorus sources (such as monoammonium phosphate) as raw materials to produce battery-grade iron phosphate. The raw material costs of iron and phosphorus sources account for more than 50% of the total production cost. Reducing the costs of iron and phosphorus sources can effectively alleviate cost pressures across the entire battery industry chain, contributing to the sustainable and healthy development of the new energy industry.
[0003] Recycling phosphorus and iron components from industrial solid / liquid waste is one of the potential pathways to obtain low-cost phosphorus and iron sources. Among these, phosphorus extraction from sludge incineration ash (hereinafter referred to as sludge ash) is an important way to achieve the recycling of phosphorus resources. Global phosphate rock resources are becoming increasingly depleted, while sludge incineration ash is enriched with more than 90% of the phosphorus from wastewater, with phosphorus content reaching the level of low- to medium-grade phosphate rock, making it a highly promising "urban phosphate mine." However, existing technologies for preparing iron phosphate from sludge incineration ash have insufficient purity, making it difficult to meet the purity requirements for battery-grade applications. Summary of the Invention
[0004] This application aims to at least partially address one of the technical problems in the related art. Therefore, the purpose of this application is to propose a method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid.
[0005] This application proposes a method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid. According to embodiments of this application, the method includes the following steps: The sludge ash acid leaching solution and iron-containing waste liquid are mixed, stirred, and separated into solid and liquid components to obtain the first solution; A citric acid compound was added to the first solution to induce a first precipitation and solid-liquid separation, yielding a first precipitate. The first precipitate was subjected to a first acid dissolution and solid-liquid separation to obtain a second solution; A citric acid compound was added to the second solution to induce a second precipitation and solid-liquid separation, yielding a second precipitate. The second precipitate was subjected to alkaline dissolution and solid-liquid separation to obtain a third precipitate and a third solution; The third precipitate is subjected to a second acid dissolution to obtain an iron source solution; Calcium salt is added to the third solution to perform a third precipitation and solid-liquid separation, yielding a fourth precipitate; The fourth precipitate is subjected to a third acid dissolution and solid-liquid separation to obtain a fifth solution; The fifth solution is subjected to arsenic removal and solid-liquid separation to obtain a phosphorus source solution; Ferric phosphate is prepared using the iron source solution and the phosphorus source solution as raw materials; The working conditions for the first and second precipitates are each independently defined as follows: the molar ratio of citrate to phosphate is 0.1-1.0, the pH is 1.0-3.0, the temperature is 15-40℃, and the stirring time is 0.5-5h. The arsenic removal composition includes copper powder, iodide, and reducing agent.
[0006] The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid described in the above embodiments of this application mainly involves simultaneously recovering and purifying phosphorus and iron through steps such as precipitation of ferric phosphate in sludge ash acid leaching solution and iron-containing waste liquid with the assistance of citric acid compounds, and removing arsenic impurities through steps such as reduction with copper powder and iodide combined reduction using reducing agents such as ascorbic acid, so that the ferric phosphate product reaches the purity level of battery grade. This method achieves simultaneous recovery and purification of phosphorus and iron components from phosphorus-containing and iron-containing waste, with a shorter overall process flow and higher purification efficiency.
[0007] In addition, the method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, the pH of the first solution is 0.5-1.0; The concentration of phosphate in the sludge ash acid leaching solution is 0.1-2 mol / L; The molar ratio of ferric iron to phosphorus in the first solution is 1.0-2.0; The concentration of ferric ions in the iron-containing waste liquid is 0.1-2 mol / L; The citric acid compounds include at least one of citric acid, sodium citrate, calcium citrate, and ammonium citrate; The reducing agent includes at least one of ascorbic acid and sodium sulfite.
[0008] In some embodiments of this application, the first acid solution of the first acid dissolution, the second acid solution of the second acid dissolution, and the third acid solution of the third acid dissolution each independently comprise a sulfuric acid solution with a concentration of 4-8 mol / L.
[0009] In some embodiments of this application, the working conditions parameters of the first acid dissolution include: pH 0.5-1.0, temperature 15-40℃, time 0.5-5h, and the liquid-solid ratio of the first precipitate to the first acid solution is (1-10):1; The working conditions for the second acid dissolution include: pH 0.5-1.5, temperature 15-40℃, time 0.5-5h, and the liquid-solid ratio of the third precipitate to the second acid solution is (1-10):1. The working conditions for the third acid solution include: pH ≤ 1.0, temperature 15-40℃, time 0.5-5h, and the liquid-to-solid ratio of the fourth precipitate to the third acid solution is (1-10):1.
[0010] In some embodiments of this application, the working conditions for alkali dissolution include: pH ≥ 12.0, temperature 15-40℃, and time 0.5-5h; The operating conditions for the third precipitate include: the amount of calcium salt added is 1.5-2.0 times the amount of phosphate in the third solution, the temperature is 15-40℃, and the time is 0.5-5h. The calcium salt includes calcium hydroxide.
[0011] In some embodiments of this application, the arsenic removal step includes the following process: adding copper powder, iodide and reducing agent to the fifth solution and stirring, controlling the pH to 0.5-1.0, the temperature to 15-40℃, and the stirring time to 0.5-5h to obtain the sixth solution; Add copper salt to the sixth solution, at a temperature of 15-40℃, and stir for 0.5-5 hours to separate the solid and liquid phases, yielding the seventh solution and the fifth precipitate. Ammonia water was added to the seventh solution to adjust the pH of the solution to 5.0-7.0, the temperature to 15-40℃, and the stirring time to 0.5-5h. Solid-liquid separation was performed to obtain the sixth precipitate and the phosphorus source solution. The amount of copper powder added is 10-500 times the total amount of arsenic in the fifth solution, the amount of iodide added is 5-100 times the total amount of arsenic in the fifth solution, and the amount of reducing agent added is 2-20 times the amount of iodide. The copper salt includes at least one of copper sulfate and copper phosphate, and the amount of copper added to the copper salt is 2-20 times the total amount of iodine in the sixth solution.
[0012] In some embodiments of this application, the steps for preparing ferric phosphate using the iron source solution and the phosphorus source solution as raw materials include the following processes: The iron source solution and the phosphorus source solution are mixed to obtain a mixed solution with a molar ratio of iron to phosphorus of 1.0-1.1; Ammonium citrate was added to the mixture to make the molar ratio of citrate to phosphate in the mixture 0.1-0.5. The pH of the system was adjusted to 1.0-3.0 with ammonia water. Solid-liquid separation was performed to obtain the iron phosphate and the eighth solution.
[0013] In some embodiments of this application, it also includes: The fifth precipitate was mixed with sodium hydroxide solution, and the system pH was 8.0-14.0. The precipitate was collected by filtration and mixed with sulfuric acid solution containing hydrogen peroxide, and the system pH was ≤2.0. Copper powder and a first supernatant were obtained by solid-liquid separation. Ammonia was added to the first supernatant to adjust the pH to 3.0-6.0. Copper arsenate precipitate and copper sulfate solution were obtained by solid-liquid separation.
[0014] In some embodiments of this application, it also includes: The eighth solution and calcium citrate are mixed, and the molar ratio of calcium to sulfate is controlled at 0.9-1.0 and the pH of the system is 2.0-3.0. Solid-liquid separation is performed to obtain a second supernatant. The second supernatant is evaporated and concentrated to obtain recovered ammonium citrate.
[0015] In some embodiments of this application, it also includes: The third supernatant obtained after adding the citric acid compound to the second solution for second precipitation and solid-liquid separation is reused in the first precipitation step; The fourth supernatant obtained after adding calcium salt to the third solution for third precipitation and solid-liquid separation is reused in the alkali dissolution step. The sixth precipitate obtained after removing arsenic from the fifth solution and separating solid and liquid is dissolved in acid and reused in the arsenic removal step.
[0016] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0017] Figure 1 This is a schematic flowchart of the method for preparing iron phosphate using sludge ash acid leaching solution and iron-containing waste liquid in the embodiments of this application.
[0018] Figure 2 This is a schematic flowchart illustrating the method for recovering copper and iodine from copper / iodine precipitates in embodiments of this application.
[0019] Figure 3 This is a schematic flowchart of the method for recovering ammonium citrate from waste liquid in the preparation process of ferric phosphate in this application embodiment. Detailed Implementation
[0020] The embodiments of this application are described in detail below by way of example, and are intended to explain this application, but should not be construed as limiting this application.
[0021] Currently, recycling phosphorus and iron components from industrial solid / liquid waste is one of the potential pathways to obtain low-cost phosphorus and iron sources, such as using sludge incineration ash to produce phosphorus sources and ferrous sulfate byproducts of titanium dioxide to produce iron sources. In the traditional approach, phosphorus source preparation and iron source preparation are two independent separation and purification processes—sludge ash needs to undergo acid leaching and purification processes to prepare phosphates or phosphoric acid, while ferrous sulfate needs to undergo dissolution and impurity removal processes to obtain an iron salt solution. Finally, the purified phosphorus and iron sources are mixed to prepare ferric phosphate. The tandem combination of phosphorus and iron source preparation processes not only makes the entire process lengthy, but also the similar or repetitive impurity removal processes for aluminum, calcium, magnesium, and heavy metals in the two processes can easily lead to the superposition and waste of equipment and reagents, as well as a multiplication of secondary waste. Therefore, if the two independent separation and purification processes of phosphorus and iron source preparation can be merged into a synergistic process, using the same system to achieve simultaneous recovery and purification of phosphorus and iron, the overall process flow will be effectively shortened, the separation and purification efficiency will be significantly improved, and the production cost of ferric phosphate will be further reduced.
[0022] Furthermore, the removal of arsenic impurities is one of the key and challenging aspects of preparing battery-grade iron phosphate from industrial waste. Due to the highly similar chemical behaviors of arsenic and phosphorus, they are extremely difficult to separate at every stage of extraction and recovery. The industry standard "Ammonium Dihydrogen Phosphate for Batteries" (HG / T 5742-2020) clearly requires that the arsenic impurity content in battery-grade ammonium dihydrogen phosphate be ≤2 ppm. However, current technical solutions for preparing battery-grade phosphorus sources from industrial waste commonly employ methods such as sulfide precipitation or heavy metal scavenging agents to remove heavy metals. However, these methods lack sufficient deep purification capabilities for arsenic impurities, often resulting in excessive arsenic content in the refined phosphorus source, failing to meet battery-grade purity requirements.
[0023] To address the above problems, this application provides the following technical solution: This application proposes a method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid. According to embodiments of this application, the method includes the following steps: The sludge ash acid leaching solution and iron-containing waste liquid are mixed, stirred, and separated into solid and liquid components to obtain the first solution; A citric acid compound was added to the first solution to induce a first precipitation and solid-liquid separation, yielding a first precipitate. The first precipitate was subjected to a first acid dissolution and solid-liquid separation to obtain a second solution; A citric acid compound was added to the second solution to induce a second precipitation and solid-liquid separation, yielding a second precipitate. The second precipitate was subjected to alkaline dissolution and solid-liquid separation to obtain a third precipitate and a third solution; The third precipitate is subjected to a second acid dissolution to obtain an iron source solution; Calcium salt is added to the third solution to perform a third precipitation and solid-liquid separation, yielding a fourth precipitate; The fourth precipitate is subjected to a third acid dissolution and solid-liquid separation to obtain a fifth solution; The fifth solution is subjected to arsenic removal and solid-liquid separation to obtain a phosphorus source solution; Ferric phosphate is prepared using the iron source solution and the phosphorus source solution as raw materials; The operating conditions for the first and second precipitates independently include: a citrate to phosphate molar ratio of 0.1-1.0 (e.g., 0.1, 0.3, 0.5, 0.8, 1.0, or any of the aforementioned values); a pH of 1.0-3.0 (e.g., 1.5, 1.8, 2.0, or any of the aforementioned values); a temperature of 15-40℃ (e.g., 20℃, 25℃, 28℃, 30℃, or any of the aforementioned values); and a stirring time of 0.5-5h (e.g., 1h, 3h, 5h, or any of the aforementioned values). The arsenic removal composition includes copper powder, iodide, and reducing agent.
[0024] The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid described in the above embodiments of this application mainly involves simultaneously recovering and purifying phosphorus and iron through steps such as precipitation of ferric phosphate in sludge ash acid leaching solution and iron-containing waste liquid with the assistance of citric acid compounds, and removing arsenic impurities through steps such as reduction with copper powder and iodide combined reduction using reducing agents such as ascorbic acid, so that the ferric phosphate product reaches the purity level of battery grade. This method achieves simultaneous recovery and purification of phosphorus and iron components from phosphorus-containing and iron-containing waste, with a shorter overall process flow and higher purification efficiency.
[0025] In addition, the method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid according to the above embodiments of this application may also have the following additional technical features: In some embodiments of this application, the pH of the first solution is 0.5-1.0 (e.g., it can be 0.5, 0.8, 1.0 or any range between the aforementioned values), ensuring that components such as phosphorus, iron, aluminum, calcium, and magnesium are in dissolved state, providing qualified feed conditions for subsequent selective precipitation of iron phosphate controlled by citrate. The concentration of phosphate in the sludge ash acid leaching solution is 0.1-2 mol / L (for example, it can be 0.1 mol / L, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L or any range between the aforementioned values), which is beneficial to improving the efficiency of the overall process. The molar ratio of ferric iron to phosphorus in the first solution is 1.0-2.0 (e.g., it can be 1.0, 1.2, 1.5 or any of the aforementioned values). The concentration of ferric ions in the iron-containing waste liquid is 0.1-2 mol / L (for example, it can be 0.1 mol / L, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, or any range between the aforementioned values). The citric acid compounds include at least one of citric acid, sodium citrate, calcium citrate, and ammonium citrate. Thus, citrate ions can effectively control the precipitation reaction process and morphology of ferric phosphate and inhibit the transport of impurities such as aluminum and calcium during the ferric phosphate precipitation process. The reducing agent includes at least one of ascorbic acid and sodium sulfite.
[0026] In some embodiments of this application, the first acid solution for the first acid dissolution, the second acid solution for the second acid dissolution, and the third acid solution for the third acid dissolution each independently comprise a sulfuric acid solution with a concentration of 4-8 mol / L (e.g., 4 mol / L, 6 mol / L, 8 mol / L, or any range between the aforementioned values). This ensures the dissolution efficiency and operational stability of the three acid dissolution steps.
[0027] In some embodiments of this application, the working conditions parameters for the first acid dissolution include: pH of 0.5-1.0, such as 0.5, 0.8, 1.0 or any of the aforementioned values; temperature of 15-40℃ (such as 20℃, 25℃, 28℃, 30℃ or any of the aforementioned values); stirring time of 0.5-5h (such as 1h, 3h, 5h or any of the aforementioned values); and liquid-solid ratio of the first precipitate to the second acid solution of (1-10):1 (such as 1:1, 3:1, 5:1 or any of the aforementioned values). The working conditions for the second acid dissolution include: pH 0.5-1.5, for example, 0.5, 0.8, 1.2, 1.5 or any of the aforementioned values; temperature 15-40℃ (for example, 20℃, 25℃, 28℃, 30℃ or any of the aforementioned values); stirring time 0.5-5h (for example, 1h, 3h, 5h or any of the aforementioned values); and the liquid-to-solid ratio of the first precipitate to the second acid solution is (1-10):1 (for example, 3:1, 5:1, 7:1 or any of the aforementioned values). The working conditions parameters for the third acid dissolution include: pH ≤ 1.0, for example, 0.2, 0.5, 1.0 or any of the aforementioned values; temperature 15-40℃ (for example, 20℃, 25℃, 28℃, 30℃ or any of the aforementioned values); stirring time 0.5-5h (for example, 1h, 3h, 5h or any of the aforementioned values); and liquid-solid ratio of the first precipitate to the second acid solution (1-10):1 (for example, 3:1, 5:1, 7:1 or any of the aforementioned values).
[0028] Therefore, acid dissolution at room temperature avoids the energy consumption of heating, while also ensuring that the acid solution and the precipitate are in full contact and completely dissolved.
[0029] In some embodiments of this application, the working conditions parameters for alkali dissolution include: pH ≥ 12.0 (e.g., 13.0, 13.5, 14.0, 14.5 or any range between the aforementioned values), temperature 15-40℃ (e.g., 20℃, 25℃, 28℃, 30℃ or any range between the aforementioned values), and stirring time 0.5-5h (e.g., 1h, 3h, 5h or any range between the aforementioned values). The operating conditions for the third precipitate include: the amount of calcium salt added is 1.5-2.0 times the amount of phosphate in the third solution (e.g., 1.6, 1.8, 2.0, or any of the aforementioned values); the temperature is 15-40℃ (e.g., 20℃, 25℃, 28℃, 30℃, or any of the aforementioned values); and the stirring time is 0.5-5h (e.g., 1h, 3h, 5h, or any of the aforementioned values). The calcium salt includes calcium hydroxide.
[0030] Therefore, alkaline dissolution phase separation is the key to achieving complete separation of the "iron phase" and "phosphorus phase", creating conditions for subsequent deep purification of iron and phosphorus sources respectively; the calcium precipitation step enriches and recovers phosphorus from the alkaline solution, and the stoichiometric ratio of calcium to phosphorus is in the range of 1.5-2.0, which not only ensures complete phosphorus precipitation, but also provides high-quality feed for subsequent calcium removal and deep arsenic removal.
[0031] In some embodiments of this application, the arsenic removal step includes the following process: adding copper powder, iodide and reducing agent to the fifth solution and stirring, controlling the pH to 0.5-1.0, the temperature to 15-40℃, and the stirring time to 0.5-5h to obtain the sixth solution; Add copper salt to the sixth solution, at a temperature of 15-40℃, and stir for 0.5-5 hours to separate the solid and liquid phases, yielding the seventh solution and the fifth precipitate. Ammonia water was added to the seventh solution to adjust the pH of the solution to 5.0-7.0, the temperature to 15-40℃, and the stirring time to 0.5-5h. Solid-liquid separation was performed to obtain the sixth precipitate and the phosphorus source solution. The amount of copper powder added is 10-500 times the total amount of arsenic in the fifth solution (e.g., 10 times, 40 times, 50 times, 100 times, 200 times, 300 times, 500 times, or any of the aforementioned values). The amount of iodide added is 5-100 times the total amount of arsenic in the fifth solution (e.g., 10 times, 40 times, 50 times, 80 times, 100 times, or any of the aforementioned values). The amount of reducing agent added is 2-20 times the amount of iodide (e.g., 2 times, 4 times, 5 times, 7 times, 9 times, 10 times, 20 times, or any of the aforementioned values). The copper salt includes at least one of copper sulfate and copper phosphate, and the amount of copper added to the copper salt is 2-20 times the total amount of iodine in the sixth solution (e.g., 2 times, 4 times, 5 times, 7 times, 9 times, 10 times, 20 times, or any of the aforementioned values). Therefore, this application adopts a synergistic system of "copper powder + iodide + reducing agent" for arsenic removal, which can not only achieve deep removal of arsenic, but also avoid the loss of iodide due to its conversion into elemental iodine, reduce the amount of iodide reagent used, and create conditions for subsequent iodide recovery.
[0032] In some embodiments of this application, the steps for preparing ferric phosphate using the iron source solution and the phosphorus source solution as raw materials include the following processes: The iron source solution and the phosphorus source solution are mixed to obtain a mixed solution with a molar ratio of iron to phosphorus of 1.0-1.1; Ammonium citrate was added to the mixture to make the molar ratio of citrate to phosphate in the mixture 0.1-0.5. The pH of the system was adjusted to 1.0-3.0 with ammonia water. Solid-liquid separation was performed to obtain the iron phosphate and the eighth solution.
[0033] In some embodiments of this application, it also includes: The fifth precipitate is mixed with sodium hydroxide solution, the system pH is 8.0-14.0, and the collected precipitate is mixed with sulfuric acid solution containing hydrogen peroxide, the system pH is ≤2.0, and solid-liquid separation is performed to obtain copper powder and a first supernatant; ammonia is added to the first supernatant to adjust the pH to 3.0-6.0, and solid-liquid separation is performed to obtain copper arsenate precipitate and copper sulfate solution. This achieves the recovery and utilization of copper powder and iodine.
[0034] In some embodiments of this application, it also includes: The eighth solution and calcium citrate are mixed, and the molar ratio of calcium to sulfate is controlled at 0.9-1.0 and the pH of the system is controlled at 2.0-3.0. Solid-liquid separation is performed to obtain a second supernatant. The second supernatant is then evaporated and concentrated to obtain recovered ammonium citrate. Thus, the recovery and utilization of ammonium citrate is achieved.
[0035] In some embodiments of this application, it also includes: The third supernatant obtained after adding the citric acid compound to the second solution for second precipitation and solid-liquid separation is reused in the first precipitation step; The fourth supernatant obtained after adding calcium salt to the third solution for third precipitation and solid-liquid separation is reused in the alkali dissolution step. The sixth precipitate obtained after removing arsenic from the fifth solution and separating solid and liquid is dissolved in acid and reused in the arsenic removal step.
[0036] Therefore, this application reduces secondary waste emissions by recycling the chemical solution through multiple process steps, which is in line with the environmental protection concept of waste resource utilization, and the overall process has industrial economic viability.
[0037] In some embodiments of this application, the method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid may include the following processes in actual operation: (1) Waste liquid mixing: Add iron-containing waste liquid to the sludge ash acid leaching solution to make the molar ratio of iron to phosphorus in the mixed solution 1.0-2.0. Add alkali (such as calcium oxide, calcium hydroxide, calcium carbonate, sodium hydroxide, sodium carbonate) to adjust the pH of the solution to 0.5-1.0. After stirring thoroughly, remove the precipitate by centrifugation or filtration and collect the supernatant. (2) Primary precipitation: Under stirring conditions, add citric acid or sodium citrate to the supernatant to make the molar ratio of citrate to phosphate in the solution 0.1-1.0. Add alkali (such as sodium hydroxide, sodium carbonate, sodium acetate, or ammonia water) to adjust the pH of the solution to 1.0-3.0. Collect the precipitate by centrifugation or filtration. (3) Precipitation acid dissolution: Gradually add sulfuric acid solution to the precipitate, stir and adjust the pH of the solution to 0.5-1.0, and collect the supernatant by centrifugation or filtration; (4) Secondary precipitation: Perform secondary precipitation according to the conditions in step (2), collect the precipitate by centrifugation or filtration, and reuse the supernatant as citric acid solution in step (2). (5) Alkali dissolution of precipitate: Mix the precipitate with sodium hydroxide solution, stir and control the pH of the mixture to ≥12.0, and collect the precipitate and supernatant by centrifugation or filtration; (6) Preparation of iron source: Dissolve the precipitate generated in step (5) with sulfuric acid solution, adjust the pH of the solution to 0.5-1.5, and detect the iron concentration; (7) Calcium precipitation: Add calcium hydroxide to the supernatant produced in step (5) so that the molar ratio of calcium to phosphate is 1.5-2.0. Separate the precipitate by stirring or centrifugation. The supernatant is concentrated and reused in step (5). (8) Calcium removal: Mix the precipitate with sulfuric acid solution, stir at room temperature, control the pH of the mixture to 0-1.0, and collect the supernatant by centrifugation or filtration; (9) Arsenic removal: Add copper powder (e.g., copper powder with a particle size of 50-500um), iodide (e.g., sodium iodide or potassium iodide) and reducing agent (e.g., sodium sulfite or ascorbic acid) to the supernatant. Stir at room temperature to remove arsenic. Then add copper salt (e.g., copper sulfate or copper phosphate, the amount added is 2-20 times the amount of iodide added to the solution) to remove iodine. Filter and collect the supernatant and precipitate. The precipitate is used for copper / iodine recovery. (10) Preparation of phosphorus source: Add ammonia water to adjust the pH of the supernatant to 5.0-7.0, collect the supernatant and precipitate by filtration, detect the phosphorus concentration of the supernatant, and reuse the precipitate as copper salt in step (9) after acid dissolution. (11) Preparation of iron phosphate: Mix the phosphorus source and the iron source to make the molar ratio of iron to phosphorus in the solution 1.0-1.1, add ammonium citrate to make the molar ratio of citrate to phosphate in the solution 0.1-0.5, adjust the pH of the solution to 1.0-3.0 with ammonia water, collect the iron phosphate precipitate and supernatant by centrifugation or filtration respectively, and recover the ammonium citrate from the supernatant; (12) Copper / iodine recovery: Mix the precipitate from step (9) with sodium hydroxide solution, stir and control the pH to 8.0-14.0, filter and collect the precipitate; mix the precipitate with sulfuric acid solution containing hydrogen peroxide (e.g., sulfuric acid concentration of 0.01-2.0 mol / L, hydrogen peroxide mass concentration of 0.1%-10%), stir and control the pH to 0-2.0, filter and collect the supernatant; add ammonia to the supernatant to adjust the pH to 3.0-6.0, filter and collect the supernatant; (13) Ammonium citrate recovery: Add calcium citrate to the supernatant of step (11) so that the molar ratio of calcium to sulfate is 0.9-1.0, stir and control the pH to 2.0-3.0, filter and collect the supernatant; evaporate and concentrate the supernatant to obtain a concentrated ammonium citrate solution; take a portion of the concentrated ammonium citrate solution, adjust the pH of the solution to 5.0-8.0 with ammonia water, add calcium chloride so that the molar ratio of calcium to citrate is 1.5-2.0, filter and collect the precipitate.
[0038] In summary, this application has at least the following beneficial effects: (1) This application can realize the simultaneous recovery and purification of phosphorus and iron components from phosphorus-containing and iron-containing waste. Compared with the traditional phosphorus source preparation + iron source preparation series process, the overall process flow is shorter, the purification efficiency is higher, and the amount of reagents consumed and secondary waste is less. (2) This application utilizes a high proportion of citric acid / sodium citrate to regulate the secondary precipitation process of ferric phosphate, which effectively reduces the carrying of impurity elements during the precipitation process of ferric phosphate, and at the same time can effectively avoid the gelation of the precipitate, reducing the difficulty of solid-liquid separation. (3) This application can deeply remove arsenic impurities, ensuring that the arsenic content in the final iron phosphate meets the battery-grade purity requirements. At the same time, it can efficiently recover and recycle the high-valence elements such as copper and iodine consumed by the arsenic removal unit, effectively reducing the reagent cost of the arsenic removal process.
[0039] The embodiments of this application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. In addition, unless otherwise specified, all reagents used in the following embodiments are commercially available or can be synthesized according to the methods described herein or known methods. For reaction conditions not listed, they are also readily available to those skilled in the art.
[0040] In the following examples, the sludge ash comes from the residue after separate incineration of sludge from municipal wastewater treatment plants, and its main chemical components are shown in Table 1; the iron-containing waste liquid is prepared from ferrous sulfate (ferrous sulfate heptahydrate content of 89%), a by-product of titanium dioxide, and sulfuric acid.
[0041] Table 1 Chemical composition of sludge incineration ash in the examples
[0042] Example 1 This embodiment provides a method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid (unless otherwise specified, the temperature conditions in the following steps are assumed to be under normal temperature conditions). Figure 1 As shown, it includes the following steps: 1) Preparation of sludge ash acid leachate: Sludge ash was mixed with acid solution (sulfuric acid concentration of 1 mol / L and hydrogen peroxide mass concentration of 0.3%) at a liquid-to-solid ratio of 5:1. After stirring for 2 hours, the mixture was filtered and the acid leachate was collected. Calcium hydroxide suspension was added to the acid leachate to adjust the pH of the solution to about 7.0. The mixture was then filtered and the precipitate was collected. The precipitate was mixed with 6 mol / L sulfuric acid solution and stirred at room temperature to completely disperse the precipitate and control the pH of the solution to 0.5. Stirring was continued for 1 hour. The mixture was then filtered and the supernatant was collected. The molar concentration ratio of phosphorus, aluminum, and iron in this solution was approximately 1:0.98:0.05, and the mass concentration ratio of arsenic to phosphorus was approximately 0.001. 2) Preparation of iron-containing waste liquid: Ferrous sulfate (ferrous sulfate heptahydrate content of 89%), a by-product of titanium dioxide production, is dissolved in dilute sulfuric acid. The iron ion concentration is controlled to be about 1 mol / L and the pH is 1.0. Hydrogen peroxide (hydrogen peroxide mass concentration of 30%) is added to make the molar concentration ratio of hydrogen peroxide to iron 0.6. The mixture is stirred for 2 hours to convert divalent iron ions to trivalent iron ions. The mixture is then filtered and the supernatant is collected. 3) Waste liquid mixing: Mix the iron-containing waste liquid with the sludge ash acid leaching solution to make the molar ratio of phosphorus to iron in the solution 1:1.5. Add calcium hydroxide to adjust the pH of the solution to 1.0, filter and collect the supernatant. 4) Primary precipitation: Sodium citrate is added to make the molar ratio of citrate to phosphate ions 0.4. The pH of the solution is adjusted to 2.0 with sodium carbonate and sulfuric acid to generate iron phosphate precipitate. The temperature is 25℃, and the mixture is stirred for 1 hour. The precipitate is collected by centrifugation. The molar ratio of aluminum to iron in the precipitate is less than 0.1, and the mass concentration ratio of arsenic to phosphorus is about 0.001. 5) Acid dissolution of precipitate: Gradually add 4 mol / L sulfuric acid solution to the precipitate, stir to disperse the precipitate and dissolve it, control the pH of the solution to 1.0, filter and collect the supernatant; 6) Secondary precipitation: Sodium citrate was added to make the molar ratio of citrate to phosphate ions 0.4. The pH of the solution was adjusted to 2.0 with sodium carbonate and sulfuric acid to generate ferric phosphate precipitate. The mixture was stirred for 1 hour, and the precipitate was collected by centrifugation. The precipitate was washed twice with 2 times the volume of dilute sulfuric acid solution (pH 2.0). The molar ratio of aluminum to iron in the precipitate was less than 0.0005, and the mass concentration ratio of arsenic to phosphorus was approximately 0.001. 7) Alkali dissolution of precipitate: Gradually add 5 mol / L sodium hydroxide solution to the precipitate, stir to disperse the precipitate and control the pH of the solution to 14.0, continue stirring for 1 hour, filter to collect the precipitate and supernatant, wash the precipitate twice with 2 times the volume of sodium hydroxide solution (pH 14.0), the precipitate is high-purity iron hydroxide, and the supernatant is a phosphorus solution containing arsenic impurities; 8) Iron source preparation: Gradually add 4 mol / L sulfuric acid solution and deionized water to the precipitate, stir to dissolve the precipitate and control the pH of the solution to 1.0, filter and collect the supernatant, which is ferric sulfate solution; 9) Calcium precipitation: Add calcium hydroxide to the supernatant collected in step 7) to make the molar ratio of calcium to phosphate in the solution 1.6. After stirring for 0.5 h, filter and collect the precipitate and supernatant. Wash the precipitate twice with 2 volumes of 1 mol / L sodium hydroxide solution. Combine the washing liquid with the supernatant. The calcium precipitate is a mixture of hydroxyapatite and calcium hydroxide. The supernatant is a sodium hydroxide solution, which can be concentrated and reused in the precipitation alkali dissolution process. 10) Calcium removal: Gradually add 4 mol / L sulfuric acid solution and deionized water to the precipitate, stir to disperse the precipitate and control the pH of the solution to about 1.0. After the pH stabilizes, continue stirring for 1 hour, filter and collect the precipitate and supernatant; the precipitate is calcium sulfate precipitate, and the supernatant is phosphorus solution; 11) Arsenic removal: Add ascorbic acid (99% purity), copper powder (250-300 mesh, 99.7% purity), and sodium iodide (99% purity) sequentially to the supernatant, so that the molar ratio of arsenic, sodium iodide, ascorbic acid, and copper powder in the solution is 1:50:200:100. Stir at room temperature for 2 hours, then add copper sulfate to make the molar ratio of added copper ions to iodide ions in the solution 2.0. Stir at room temperature for 0.5 hours, filter, and collect the supernatant and precipitate separately. The supernatant is a phosphorus solution in which the mass concentration ratio of arsenic to phosphorus is less than 0.00001. The precipitate is a mixture of copper powder and cuprous iodide containing arsenic impurities. 12) Preparation of phosphorus source: Add ammonia to the supernatant to adjust the pH of the solution to 6.0, stir for 1 hour, filter and collect the supernatant and precipitate; the supernatant is a phosphorus solution, and the precipitate is mainly composed of copper phosphate precipitate, which can be returned to the arsenic removal process as copper salt after dissolution. 13) Preparation of ferric phosphate: Mix the prepared iron source with the phosphorus source to make the molar ratio of iron to phosphorus in the solution 1.05. Add ammonium citrate to make the molar ratio of citrate to phosphate ions 0.2. Adjust the pH of the solution to 1.5 with ammonia water. Stir at room temperature (around 25℃) for 1 hour. Centrifuge to collect the precipitate and supernatant. The precipitate is ferric phosphate precipitate (the molar ratio of phosphorus to iron is 0.98).
[0043] Two verification experiments were conducted using the above method. The results showed that the overall phosphorus recovery rate of the battery-grade phosphorus source prepared from sludge ash leachate was ≥95%; the overall iron recovery rate of the battery-grade iron source prepared from iron-containing waste liquid was ≥95%; and the arsenic impurity content in the final prepared iron phosphate precipitate was less than 3 ppm, while the content of other metal impurity elements met the technical requirements of the industry standard "Iron Phosphate for Batteries" (HG / T4701-2021).
[0044] Example 2 This embodiment provides a method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater (also including the recovery of copper and iodine from arsenic removal process waste), such as Figure 1 and Figure 2 As shown, the following steps are also included in Example 1: 1) Mix the copper / iodine precipitate produced by the arsenic removal process with 1 mol / L sodium hydroxide solution at a liquid-to-solid ratio of 3:1, stir at room temperature for 0.5 h, filter and collect the precipitate and supernatant. Wash the precipitate with 2 volumes of 0.1 mol / L sodium hydroxide solution, and combine the washing liquid with the supernatant. The supernatant is an iodine-containing solution, and the precipitate is a mixture of copper powder and cuprous oxide. 2) Mix the precipitate with a 1 mol / L sulfuric acid solution (with a hydrogen peroxide mass concentration of about 1%) at a liquid-to-solid ratio of 3:1, stir at room temperature for 2 hours, filter and collect the precipitate and supernatant; the precipitate is copper powder, and the supernatant is a copper sulfate solution containing arsenic impurities; 3) Add ammonia to the supernatant to adjust the pH of the solution to 4.0, filter and collect the precipitate and supernatant; the supernatant is a copper sulfate solution with an arsenic impurity content of less than 1 ppm, which can be returned to the arsenic removal process as a copper salt; the precipitate is copper arsenate.
[0045] Two verification experiments were conducted using the above method. The results showed that the copper / iodine recovery process achieved a copper powder recovery rate of ≥90%, an iodine recovery rate of ≥98%, and an arsenic recovery rate of ≥95%.
[0046] Example 3 This embodiment provides a method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater (also including the recovery of ammonium citrate from the wastewater in the phosphate source iron preparation process), such as Figure 1 and Figure 3 As shown, the following steps are also included in Example 1: 1) Add calcium citrate to the wastewater generated from the phosphorus source preparation process to make the molar ratio of calcium to sulfate ions in the solution 0.95, control the pH of the solution to 2.0, stir for 1 hour, filter and collect the precipitate and supernatant; the supernatant is a dilute ammonium citrate solution, and the precipitate is calcium sulfate; 2) Heat the supernatant to 60℃ for evaporation and concentration so that the citrate concentration in the solution reaches about 1 mol / L, which can be reused in the iron phosphate preparation process; 3) Take a portion of the concentrated ammonium citrate solution, adjust the pH to 6.0 with ammonia, add calcium chloride to make the molar ratio of calcium to citrate ions in the solution 1.6, stir for 1 hour, filter and collect the precipitate and supernatant; the precipitate is calcium citrate, which can be reused in step 1); the supernatant is ammonium chloride.
[0047] Two verification experiments were conducted using the above method. The results showed that the ammonium citrate recovery process achieved a recovery rate of ≥95% for ammonium citrate in the wastewater from the phosphorus source iron preparation process.
[0048] Comparative Example 1 The difference between this example and Example 1 is that: (1) The parameters for the first precipitation in step 4 and the second precipitation in step 6 were adjusted as follows: the molar ratio of citrate to phosphate was 1.2, the pH was 2.0, the temperature was 25℃, and the stirring time was 1h.
[0049] Two verification experiments were conducted using the above method. The results showed that the overall phosphorus recovery rate for preparing battery-grade phosphorus sources using sludge ash leachate was <20%, and the overall iron recovery rate for preparing battery-grade iron sources using iron-containing wastewater was <15%. The recovery rates of phosphorus and iron were significantly reduced.
[0050] Comparative Example 2 The difference between this example and Example 1 is that: (1) Step 6 was not performed for secondary precipitation and step 7 was not performed for alkaline dissolution of precipitation. In step 9, the supernatant of calcium precipitation was directly obtained by acid dissolution of precipitation in step 5).
[0051] Two verification experiments were conducted using the above method. The results showed that the overall phosphorus recovery rate of preparing battery-grade phosphorus source using sludge ash leachate was <5%; the overall iron recovery rate of preparing battery-grade iron source using iron-containing waste liquid was <5%; and the arsenic impurity content in the final prepared iron phosphate precipitate was >100ppm, which did not meet the technical requirements of the industry standard "Iron Phosphate for Batteries" (HG / T4701-2021).
[0052] Comparative Example 3 The difference between this example and Example 1 is that: (1) No arsenic removal was performed in step 11, and the phosphorus source was prepared directly using the phosphorus solution obtained in step 10 in step 12.
[0053] Two verification experiments were conducted using the above method. The results showed that the arsenic impurity content in the final prepared iron phosphate precipitate was >100ppm, which did not meet the technical requirements of the industry standard "Iron Phosphate for Batteries" (HG / T4701-2021).
[0054] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0055] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.
Claims
1. A method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid, characterized in that, Includes the following steps: The sludge ash acid leaching solution and iron-containing waste liquid are mixed, stirred, and separated into solid and liquid components to obtain the first solution; A citric acid compound was added to the first solution to induce a first precipitation and solid-liquid separation, yielding a first precipitate. The first precipitate was subjected to a first acid dissolution and solid-liquid separation to obtain a second solution; The citric acid compound is added to the second solution to perform a second precipitation and solid-liquid separation, resulting in a second precipitate. The second precipitate was subjected to alkaline dissolution and solid-liquid separation to obtain a third precipitate and a third solution; The third precipitate is subjected to a second acid dissolution to obtain an iron source solution; Calcium salt is added to the third solution to perform a third precipitation and solid-liquid separation, yielding a fourth precipitate; The fourth precipitate is subjected to a third acid dissolution and solid-liquid separation to obtain a fifth solution; The fifth solution is subjected to arsenic removal and solid-liquid separation to obtain a phosphorus source solution; Ferric phosphate is prepared using the iron source solution and the phosphorus source solution as raw materials; The working conditions for the first and second precipitates are each independently defined as follows: the molar ratio of citrate to phosphate is 0.1-1.0, the pH is 1.0-3.0, the temperature is 15-40℃, and the stirring time is 0.5-5h. The arsenic removal composition includes copper powder, iodide, and reducing agent.
2. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 1, characterized in that, The pH of the first solution is 0.5-1.0; The concentration of phosphate in the sludge ash acid leaching solution is 0.1-2 mol / L; The molar ratio of ferric iron to phosphorus in the first solution is 1.0-2.0; The concentration of ferric ions in the iron-containing waste liquid is 0.1-2 mol / L; The citric acid compounds include at least one of citric acid, sodium citrate, calcium citrate, and ammonium citrate; The reducing agent includes at least one of ascorbic acid and sodium sulfite.
3. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 1, characterized in that, The first acid solution of the first acid dissolution, the second acid solution of the second acid dissolution, and the third acid solution of the third acid dissolution each independently comprise a sulfuric acid solution with a concentration of 4-8 mol / L.
4. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 1, characterized in that, The working conditions for the first acid dissolution include: pH 0.5-1.0, temperature 15-40℃, stirring time 0.5-5h, and the liquid-solid ratio of the first precipitate to the first acid solution is (1-10):
1. The working conditions for the second acid dissolution include: pH 0.5-1.5, temperature 15-40℃, stirring time 0.5-5h, and the liquid-to-solid ratio of the third precipitate to the second acid solution is (1-10):
1. The working conditions for the third acid solution include: pH ≤ 1.0, temperature 15-40℃, stirring time 0.5-5h, and the liquid-to-solid ratio of the fourth precipitate to the third acid solution is (1-10):
1.
5. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 1, characterized in that, The working conditions for alkaline dissolution include: pH ≥ 12.0, temperature 15-40℃, and stirring time 0.5-5h. The operating conditions for the third precipitate include: the amount of calcium salt added is 1.5-2.0 times the amount of phosphate in the third solution, the temperature is 15-40℃, and the stirring time is 0.5-5h. The calcium salt includes calcium hydroxide.
6. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 1, characterized in that, The arsenic removal steps include the following process: adding copper powder, iodide and reducing agent to the fifth solution, controlling the pH to 0.5-1.0, the temperature to 15-40℃, and stirring for 0.5-5h to obtain the sixth solution; Add copper salt to the sixth solution, at a temperature of 15-40℃, and stir for 0.5-5 hours to separate the solid and liquid phases, yielding the seventh solution and the fifth precipitate. Ammonia water was added to the seventh solution to adjust the pH of the solution to 5.0-7.0, the temperature to 15-40℃, and the stirring time to 0.5-5h. Solid-liquid separation was performed to obtain the sixth precipitate and the phosphorus source solution. The amount of copper powder added is 10-500 times the total amount of arsenic in the fifth solution, the amount of iodide added is 5-100 times the total amount of arsenic in the fifth solution, and the amount of reducing agent added is 2-20 times the amount of iodide. The copper salt includes at least one of copper sulfate and copper phosphate, and the amount of copper added to the copper salt is 2-20 times the total amount of iodine in the sixth solution.
7. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 1, characterized in that, The steps for preparing ferric phosphate using the iron source solution and the phosphorus source solution as raw materials include the following processes: The iron source solution and the phosphorus source solution are mixed to obtain a mixed solution with a molar ratio of iron to phosphorus of 1.0-1.1; Ammonium citrate was added to the mixture to make the molar ratio of citrate to phosphate in the mixture 0.1-0.
5. The pH of the system was adjusted to 1.0-3.0 using ammonia water. Solid-liquid separation was performed to obtain the ferric phosphate and the eighth solution.
8. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing waste liquid according to claim 6, characterized in that, Also includes: The fifth precipitate was mixed with sodium hydroxide solution, and the pH of the system was 8.0-14.
0. The precipitate was collected by filtration and mixed with sulfuric acid solution containing hydrogen peroxide, and the pH of the system was ≤2.
0. Copper powder and a first supernatant were obtained by solid-liquid separation. Ammonia was added to the first supernatant to adjust the pH to 3.0-6.
0. Copper arsenate precipitate and copper sulfate solution were obtained by solid-liquid separation.
9. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 7, characterized in that, Also includes: The eighth solution and calcium citrate are mixed, and the molar ratio of calcium to sulfate is controlled at 0.9-1.0 and the pH of the system is 2.0-3.
0. Solid-liquid separation is performed to obtain a second supernatant. The second supernatant is evaporated and concentrated to obtain recovered ammonium citrate.
10. The method for preparing ferric phosphate using sludge ash acid leaching solution and iron-containing wastewater according to claim 1, characterized in that, Also includes: The third supernatant obtained after adding the citric acid compound to the second solution for second precipitation and solid-liquid separation is reused in the first precipitation step; The fourth supernatant obtained after adding calcium salt to the third solution for third precipitation and solid-liquid separation is reused in the alkali dissolution step. The sixth precipitate obtained after removing arsenic from the fifth solution and separating solid and liquid is dissolved in acid and reused in the arsenic removal step.