A self-sealing fly ash-based pressed solidified body, its preparation method and application
By synergistically combining unwashed and dechlorinated municipal solid waste incineration fly ash with carbide slag, mineral slag, etc., and through microwave-assisted wet heat treatment, a self-sealing fly ash-based pressed solidified body is formed, which solves the durability and stability problems under salt-freezing service environment, realizes pore self-sealing and heavy metal solidification, and reduces the risk of heavy metal migration.
Patent Information
- Application Number
- CN202611376057.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies, when used in salt-freezing service environments, fail to adequately address the durability and environmental stability of solidified fly ash, resulting in risks of pore structure deterioration, strength reduction, and heavy metal migration. This makes it difficult to simultaneously achieve low-cost large-scale utilization, salt solution migration inhibition, freeze-thaw damage suppression, and heavy metal migration risk control.
By using unwashed and dechlorinated municipal solid waste incineration fly ash, carbide slag, blast furnace slag, solid waste sulfate and/or solid waste aluminum silicon in a synergistic formulation, and through microwave-assisted wet heat treatment, C-(A)-SH gel, Friedel salt and other Cl-AFm and AFt phases are formed, achieving self-sealing of pores and microcracks and solidification of heavy metals.
During salt-freezing service, the self-sealing fly ash-based pressed solidified body can continuously induce the formation of a stationary phase, reduce the risk of heavy metal migration, improve the self-sealing ability of pores and the effect of freeze-thaw damage inhibition, and ensure long-term environmental stability.
Smart Images

Figure CN123106031A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical fields of harmless disposal of fly ash from municipal solid waste incineration, resource utilization of solid waste, and salt-resistant gelling materials. In particular, it relates to a self-sealing fly ash-based pressed solidified body, its preparation method, and its application. Background Technology
[0002] Fly ash from municipal solid waste incineration contains high levels of soluble chlorides, heavy metals, and small amounts of sulfates, classifying it as hazardous waste requiring strict control. Currently, commonly used fly ash disposal or pretreatment methods include cement solidification, chemical stabilization, water washing and desalination, high-temperature melting, sintering of ceramsite, geopolymer solidification, and co-preparation of solidified materials such as non-fired bricks. While these methods can reduce the risk of heavy metal leaching and achieve fly ash reduction or resource utilization to some extent, the resulting solidified materials may still experience problems such as pore structure deterioration, strength reduction, and increased risk of heavy metal migration in cold regions and service environments involving chlorides, sulfates, and freeze-thaw cycles. Long-term durability and environmental stability still have room for improvement.
[0003] To address the durability issues of solidified bodies under salt-freezing service environments, existing technologies typically follow a process of fly ash pretreatment – strong alkali / cement-based gelation and solidification – molding and curing – landfilling or low-value utilization. This involves first reducing the initial leaching risk of fly ash through water washing and desalination, chemical stabilization, or the addition of cement / strong alkali activators, followed by casting, pressing, or brick forming, and finally curing and utilization. Some solutions also require adding a protective surface coating, high-temperature heat treatment, hydrothermal treatment, or the addition of antifreeze agents after molding. However, water washing and desalination generate saline wastewater and weaken the role of endogenous chloride salts in the formation of the Cl-AFm stationary phase; strong alkali or cement-based gelation and solidification increases costs, carbon emissions, and corrosion risks; the outer surface coating is prone to interfacial debonding during freeze-thaw cycles, making it difficult to continuously seal internal microcracks; simply increasing the amount of cementitious materials or additives is insufficient to continuously induce stationary phase regeneration during salt-freezing service. Therefore, existing technologies are insufficient to simultaneously achieve low-cost large-scale utilization of unwashed high-chlorine fly ash, salt migration inhibition, freeze-thaw damage suppression, self-sealing of microcracks during service life, and control of heavy metal migration risks. Summary of the Invention
[0004] To address the shortcomings of the existing technology, the present invention aims to provide a self-sealing fly ash-based pressed solidified body, its preparation method, and its application. This allows the fly ash-based pressed solidified body to not only complete initial solidification during the preparation stage but also continue to induce the formation of stationary phases and subsequent hydration products during salt-freezing service, thereby achieving self-sealing of pores and microcracks and solidification of heavy metals, thus reducing the migration risk of heavy metals during long-term salt-freezing service.
[0005] To solve the above-mentioned technical problems, the present invention provides a method for preparing a self-sealing fly ash-based pressed and cured body, comprising the following steps: The cementitious component is added to mixing water and mixed at a water-cement ratio of 0.20–0.40 to obtain salt-containing moist granules. The salt-containing moist granules are pressed and shaped under a pressure of 5 MPa–40 MPa for 20–300 seconds to obtain a pressed green body. The cementitious component contains the following raw materials in the following mass percentages: 20%–55% unwashed and dechlorinated fly ash, 5%–25% carbide slag, 25%–70% slag, 0%–15% solid waste sulfate, and 0%–20% solid waste aluminum silicon. The sum of the mass percentages of the raw materials is 100%, and the mass percentages of solid waste sulfate and solid waste aluminum silicon are not both 0.
[0006] Microwave-assisted wet heat treatment was applied to the pressed preform at a power density of 0.1 W / g to 2.0 W / g. During the heating stage, the surface temperature of the pressed preform was increased at an average heating rate of 0.5℃ / min to 10℃ / min, and the maximum surface temperature was controlled at 45℃ to 85℃. The cumulative microwave irradiation time was 8 min to 30 min, and the mass loss rate of the treated pressed preform did not exceed 8%. Subsequently, the treated pressed preform was subjected to moist curing or standard curing to obtain a self-sealing fly ash-based pressed solidified body.
[0007] This method uses fly ash from high-chlorinated municipal solid waste incineration that has not been dechlorinated by water as the main solid waste source, combined with carbide slag, blast furnace slag, and solid waste sulfate and / or solid waste aluminum silicon. The mixture is then pressed into shape under a water-to-binder ratio of 0.20–0.40. Subsequently, the shaped green body is subjected to low-temperature microwave-assisted hydrothermal treatment at an average heating rate of 0.5℃ / min–10℃ / min and a power density of 0.1W / g–2.0W / g. The surface temperature of the green body is controlled at 45℃–85℃, with a cumulative treatment time of 8 min–30 min, and the mass loss rate after treatment is kept below 8%. The microwave-assisted hydrothermal treatment achieves a controlled increase in the internal temperature of the green body by dielectric heating the aqueous phase in the system, and causes dynamic adjustment of the state and distribution of pore liquid, thereby promoting the redistribution of soluble salts and the occurrence of early hydration reactions to a certain extent. Under conditions without melting, sintering, or high-pressure hydrothermal reactions, an initial C-(A)-SH gel, Friedel salt, and other Cl-AFm and AFt phases are formed, while retaining certain unreacted slag glass phase, aluminosilicate phase, and calcium-alkaline reaction interface. This solidified body, under subsequent chloride, sulfate, and freeze-thaw coupled service environments, exhibits exogenous Cl... - SO4 2- After water enters the pores, it can induce the regeneration of the reaction phase and the subsequent filling of hydration products, thereby achieving pore self-blocking, salt migration inhibition and heavy metal re-fixation.
[0008] The above-mentioned proportions serve the following purposes: municipal solid waste incineration fly ash provides endogenous chlorides and heavy metals, serving as the main source for Cl-AFm phase formation and fly ash disposal; calcium carbide slag provides calcium-alkaline components such as Ca(OH)2, increasing the system's alkalinity and activating the slag; the slag provides a sustainable glassy phase silica-alumina source for reaction, forming a C-(A)-SH gel framework; the selective addition of solid waste sulfate components compensates for the relative deficiency of sulfates in fly ash and promotes the appropriate generation of AFt phase or monosulfide AFm phase; the selective addition of solid waste aluminum-silicon components supplements aluminum-silicon reaction sites, enhancing the synergistic formation of Cl-AFm phase, AFt phase, and gel framework, such as Friedel salt. In summary, this provides a phase basis for pore self-sealing, salt solution migration inhibition, and heavy metal re-fixation.
[0009] A water-cement ratio of 0.20–0.40 can balance compactability, ion migration, hydration reaction, and the formation of a low-porosity structure. The reason for limiting this water-cement ratio range is that when the water-cement ratio is below 0.20, there is insufficient mixing water, making it difficult for soluble salts in fly ash to fully dissolve and redistribute, and limiting the early reactions of slag and aluminum-silicon phases. When the water-cement ratio is above 0.40, the system is prone to change from a wet particle state to a high-water-content slurry state. After pressing, the number of interconnected pores and capillaries increases, and salt solution and freeze-thaw water can more easily enter the interior of the solidified body, which is not conducive to pore self-sealing and long-term curing of heavy metals.
[0010] When the power density is below 0.1 W / g or the processing time is too short, the pressed green body is difficult to form an effective low-temperature humid heat control effect, and the redistribution of pore liquid and early hydration promotion effect are insufficient. When the power density is above 2.0 W / g or the processing time is too long, it is easy to cause local overheating, rapid surface water loss, microcrack propagation or abnormal salt enrichment, which is not conducive to subsequent pore self-blocking and heavy metal stabilization.
[0011] The reason for limiting the pressure and holding time is that when the pressure is below 5 MPa or the holding time is too short, the contact between particles is insufficient, the initial porosity is high, and it is difficult to form an effective salt-freezing resistant skeleton. When the pressure is above 40 MPa or the holding time is too long, the molding energy consumption increases, and it may lead to stress concentration at the interface of the layered preform, excessive local migration of moisture, or local dehydration cracks during subsequent microwave treatment. The pressure of 5 MPa to 40 MPa and the holding time of 20 s to 300 s can promote particle rearrangement, improve interfacial contact and initial density, and provide a stable skeleton for subsequent microwave hydrothermal control and salt-freezing induced stationary phase formation.
[0012] Limiting the average heating rate to 0.5℃ / min–10℃ / min, the maximum surface temperature of the pressed green body to 45℃–85℃, and the cumulative microwave irradiation time to 8min–30min is to ensure sufficient dielectric heating of the aqueous phase within the green body and to create a mild and controllable hygrothermal gradient without damaging the low water-to-binder ratio pressed framework. When the average heating rate is below 0.5℃ / min, the surface temperature is below 45℃, or the cumulative treatment time is less than 8min, the effects of pore fluid migration, soluble salt dissolution and redistribution, and early hydration promotion are not significant. When the average heating rate is above 10℃ / min, the surface temperature is above 85℃, or the cumulative treatment time exceeds 30min, rapid water loss, vapor pressure accumulation, non-uniform salt enrichment, and drying shrinkage or thermal stress microcracks are likely to occur on the surface or in localized areas. Therefore, the above parameter range can balance hygrothermal transfer, ion migration, early reaction promotion, and the structural integrity of the green body.
[0013] Limiting the mass loss rate of pressed green bodies after microwave-assisted hydrothermal treatment to no more than 8% is to constrain the actual heat treatment intensity under different green body sizes and equipment conditions using directly measurable quality indicators, and to control the moisture evaporation caused by microwaves within a range that does not disrupt the continuous aqueous phase. When the mass loss rate exceeds 8%, the surface of the green body is prone to excessive drying, increasing the internal and external moisture gradient and local vapor pressure, which may cause drying shrinkage microcracks, salt enrichment on the surface, and interruption of the continuous water film required for subsequent hydration. When the mass loss rate does not exceed 8%, the green body can retain sufficient pore water to maintain ion migration, subsequent curing, and the continuous generation of reactive phases, thereby reducing the risk of structural deterioration due to excessive water loss.
[0014] Preferably, the gelling component is divided into an inner gelling component and an outer gelling component, which are mixed with mixing water at a water-to-gel ratio of 0.20 to 0.40 to obtain an inner layer of salt-containing moist granules and an outer layer of salt-containing moist granules. The outer layer of salt-containing moist granules is arranged on the outer periphery of the inner layer of salt-containing moist granules and pressed in one step to obtain a pressed blank with an inner layer of load-bearing and solidified core and an outer layer of salt-freezing response layer. The pressed blank has an inner and outer gradient partition structure. The inner cementing component comprises 35%–55% untreated municipal solid waste incineration fly ash, 5%–18% calcium carbide slag, 35%–60% slag, 0%–5% solid waste sulfate components, and 0%–10% solid waste aluminum silicon; the outer cementing component comprises 10%–35% untreated municipal solid waste incineration fly ash, 10%–25% calcium carbide slag, 40%–70% slag, 3%–15% solid waste sulfate components, and 3%–20% solid waste aluminum silicon.
[0015] The reason for further limiting it to a mixture of internal and external gradient partitions is that... The inner cementitious component has a relatively high proportion of fly ash, mainly responsible for the large-volume disposal of fly ash, the fixation of heavy metals, and the load-bearing and solidification functions. The outer cementitious component has a relatively high proportion of slag, carbide slag, solid waste sulfate, and solid waste aluminum-silicon components, which can provide more calcium-alkali sources, active silica-alumina phases, and sulfate components, and preferentially react with external Cl during service. - SO4 2- Upon contact with moisture, Cl-AFm phase, AFt phase, and C-(A)-SH gel are formed, thus creating a salt-freezing-resistant protective layer on the outer layer, delaying the migration of salt solution and freeze-thaw water to the inner layer. The inner and outer layers are formed into a continuous interface through a single pressing process, avoiding the problem of easy debonding of traditional surface coatings during freeze-thaw cycles, thereby further improving the self-sealing ability of pores and microcracks and the long-term fixation effect of heavy metals. At the same time, this gradient range allows the outer layer to have a lower fly ash content and a higher content of gelling reaction components compared to the inner layer, which is conducive to the preferential formation of a dense protective layer on the outer layer; the inner layer maintains a higher fly ash content, which is beneficial to increasing the amount of hazardous waste that can be disposed of.
[0016] Preferably, the microwave-assisted wet heat treatment is either continuous or pulsed. When pulsed treatment is used, the microwave irradiation duration is 10s–180s and the interval duration is 10s–240s within each pulse cycle, and the process is repeated according to the above irradiation and interval parameters. Continuous treatment is suitable for smaller billets or billets with more uniform moisture content, while pulsed treatment can achieve a heating-uniforming-reheating process during the microwave irradiation and intermittent stop phases, reducing the risk of local overheating and facilitating moisture redistribution.
[0017] Preferably, the solid waste sulfate is one or more of the following: desulfurized gypsum, phosphogypsum, titanium gypsum, fluorogypsum, desulfurized ash, circulating fluidized bed solidified ash, or sulfur-containing slag; all of the above solid waste sulfate components can provide SO4. 2- Or a sulfur-containing calcium phase, which participates in the formation of AFt phase such as ettringite, monosulfide AFm phase or other sulfur-containing aluminate hydration products in a high-calcium and high-alkali environment. This can not only compensate for the relative deficiency of sulfate in high-chlorine fly ash, but also fill the pores with an appropriate amount of sulfur-containing stationary phase and synergistically fix some heavy metal ions, thereby improving the volume stability and long-term environmental safety under salt-freezing conditions.
[0018] The solid waste aluminum-silicon is one or more of the following: red mud, fly ash, calcined coal gangue powder, aluminum ash washing slag, tailings powder, recycled brick powder, and waste ceramic powder, but does not include cement clinker, silicate cement, or cementitious materials with cement clinker as the main component. The above-mentioned solid waste aluminum-silicon components can provide active Al2O3, SiO2, or aluminosilicate phases, providing aluminum-silicon sources for the formation of Cl-AFm phases, AFt phases, and C-(A)-SH gels such as Friedel salt; at the same time, the limitation that it does not include cement clinker or silicate cement highlights the technical route of this invention, which utilizes solid waste aluminum-silicon for compensation rather than traditional cement clinker reinforcement.
[0019] Preferably, the water-cement ratio is 0.20–0.30, resulting in salt-containing moist granules that are compactable and exhibit no significant free water precipitation. This method also achieves better results in terms of compactability, ion migration, hydration reaction, and the formation of a low-porosity structure.
[0020] Preferably, the pressing method is one of unidirectional pressing, bidirectional pressing, compression molding, or vibration pressing. The reason for choosing these pressing methods is that they are all suitable for wet granules with low water-to-binder ratios, can provide adjustable molding pressure and holding time without introducing significant free water, and form a continuous, dense granular skeleton. Among these, unidirectional pressing equipment is simple and suitable for regular small products; bidirectional pressing can reduce the density gradient in the thickness direction; compression molding facilitates obtaining specific shapes and sizes; and vibration pressing is beneficial for improving particle rearrangement and mold filling uniformity. All of the above methods can be integrated with internal and external gradient zoning and subsequent microwave-assisted hydrothermal treatment.
[0021] Preferably, the surface of the pressed green body is sprayed with water, coated with a film for moisturizing, or placed in an environment with a relative humidity of not less than 80% to maintain the moisture required for the dissolution-redistribution and hydration reactions of soluble salts. The reason for further limiting moisturizing measures is that microwave-assisted humid heat treatment can cause moisture migration and localized evaporation in the green body. If spraying with water, coating with a film for moisturizing, or high-humidity environment control is not performed, the surface layer is prone to rapid water loss and the formation of microcracks due to shrinkage, which weakens the self-sealing effect of pores. By maintaining a humid heat environment with a relative humidity of not less than 80% during or after treatment, a continuous water film required for the dissolution-redistribution and early hydration reactions of soluble salts can be maintained, promoting the continuous formation of Cl-AFm phase, AFt phase, and C-(A)-SH gel.
[0022] Preferably, after microwave-assisted hydrothermal treatment, the product is cured for 3 to 28 days at a temperature of 18℃ to 22℃ and a relative humidity of not less than 95%, or first sealed and cured for 6 to 48 hours, followed by standard curing to the specified age. The reason for further limiting the subsequent curing regime is that microwave-assisted hydrothermal treatment mainly serves as a low-temperature pre-regulation, and does not mean that the gelation reaction is complete. Continued curing at 18℃ to 22℃ and a relative humidity of not less than 95% provides a stable moisture environment for the subsequent hydration of the slag glass phase, fly ash active aluminosilicate phase, and calcium-alkali components of carbide slag, allowing the C-(A)-SH gel, Friedel salt, and other Cl-AFm and AFt phases to continue developing. First, sealed curing for 6 to 48 hours reduces early water loss and stabilizes the internal ionic environment, followed by standard curing, which is conducive to further forming a dense skeleton, thereby continuously improving the self-sealing ability of pores and microcracks and the fixation effect of heavy metals.
[0023] The present invention also provides a method for preparing a self-sealing fly ash-based pressed solidified body.
[0024] This invention also provides the application of a self-sealing fly ash-based compressed solidified body as a pretreatment block for solid waste-based landfills, a road base block, a non-load-bearing building material, or a landfill covering material.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: By synergistically combining fly ash from municipal solid waste incineration without water washing and dechlorination, carbide slag, blast furnace slag, solid waste sulfate and / or solid waste aluminum silicon, fly ash provides endogenous chloride salts and heavy metals to be fixed, carbide slag provides calcium alkali source, solid waste aluminum silicon is selectively introduced, blast furnace slag and solid waste aluminum silicon provide active silicon aluminum phase, and solid waste sulfate is selectively introduced to compensate for the relative deficiency of sulfate in fly ash and to adjust the appropriate amount of AFt phase or monosulfide AFm phase to be generated, thus providing a phase basis for the synergistic generation of Cl-AFm phase and AFt phase such as C-(A)-SH gel and Friedel salt.
[0026] The process involves pressing the solidified body with a water-to-binder ratio of 0.20–0.40 and a pressure of 5–40 MPa to preferentially reduce the initial interconnected pores and increase particle contact density. Subsequently, low-temperature microwave-assisted hydrothermal treatment is implemented at an average heating rate of 0.5–10 °C / min, a power density of 0.1 W / g–2.0 W / g, a surface temperature of 45–85 °C, and a cumulative treatment time of 8–30 min, with a process constraint that the post-treatment mass loss rate does not exceed 8%. This process utilizes dielectric heating of the aqueous phase to promote the release of Cl from the pore liquid and its components. - SO4 2- Controlled migration and redistribution of alkaline components promote the formation of early hydration products in the particle contact area and pore walls, while avoiding excessive water loss and local thermal damage, forming a structure in which an initial dense framework and a reaction interface coexist.
[0027] During subsequent salt-freezing service, moisture and Cl- enter the residual pores or microcracks. - and SO4 2- It can continue to react with the retained glassy phase of slag, aluminosilicate phase of fly ash, and calcium alkali source of carbide slag, allowing C-(A)-SH gel, Cl-AFm phase, and AFt phase to preferentially deposit and fill pore walls, particle interfaces, and microcracks, reducing capillary channels and their connectivity; it also compresses a dense framework while reducing water saturation and frost heave, thereby achieving self-sealing of microcracks, inhibition of salt migration, and suppression of freeze-thaw damage. Heavy metals can have their migration risk reduced through gel adsorption and encapsulation, ion binding of aluminate phase, and low-permeability structural barrier. Attached Figure Description
[0028] Figure 1 To investigate the formation and salt solution migration inhibition mechanism of self-sealing fly ash-based pressed solidified bodies under microwave-assisted hygrothermal regulation.
[0029] Figure 2 This is a process flow diagram of the self-sealing fly ash-based pressed and cured body of the present invention. Detailed Implementation
[0030] The specific embodiments of the present invention are described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention. Unless otherwise specified, the experimental methods described in the embodiments of the present invention are conventional methods.
[0031] It should be noted that when numerical ranges are involved in this invention, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as in Examples 1 to 19, preferred embodiments are described in this invention to avoid redundancy. However, this invention is not limited to these, but can be implemented in other ways within the scope of the technical solutions defined in the appended claims. All raw materials, reagents, instruments, and equipment used in the following embodiments of this invention can be purchased from the market or prepared by existing methods.
[0032] The following detailed description, in conjunction with embodiments of the present invention and accompanying drawings, provides a clear and complete illustration of the technical solutions in these embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0033] The molding method provided in this invention is one of unidirectional pressing, bidirectional pressing, compression molding, or vibration pressing. In the following embodiments, unidirectional pressing is preferred.
[0034] The solid waste sulfate provided in this invention can be one or more of desulfurized gypsum, phosphogypsum, titanium gypsum, fluorogypsum, desulfurized ash, circulating fluidized bed solid sulfur ash, or sulfur-containing slag. The following related embodiments select desulfurized gypsum or desulfurized ash according to the specific formula.
[0035] The solid waste aluminum silicon provided in this invention is one or more of the following: red mud, fly ash, calcined coal gangue powder, aluminum ash washing slag, tailings powder, recycled brick powder, and waste ceramic powder, but does not include cement clinker, silicate cement, or cementitious materials with cement clinker as the main component. The following related embodiments select calcined coal gangue powder, red mud, or fly ash according to the specific formula.
[0036] In this invention, the microwave power density refers to the ratio of the set output power of the microwave equipment during microwave processing to the mass of the pressed blank before processing, and the unit is W / g.
[0037] The average heating rate refers to the heating stage of microwave-assisted wet heat treatment, determined based on the change in the surface temperature of the pressed billet with treatment time. The surface temperature of the pressed billet is continuously monitored using a non-contact infrared thermometer; for pulsed microwave treatment, the heating time includes the microwave irradiation stage and adjacent intermittent stages.
[0038] The mass loss rate is calculated according to the formula η=(m0-m1) / m0×100%, where m0 is the mass of the pressed blank before microwave-assisted damp heat treatment, and m1 is the mass of the pressed blank measured under the same weighing conditions after microwave-assisted damp heat treatment.
[0039] Example 1 A method for preparing a self-sealing fly ash-based compressed solidified body includes the following steps: Based on the total mass of the cementitious components, weigh out 35% of the fly ash from municipal solid waste incineration that has not undergone water washing and dechlorination treatment, 12% of the calcium carbide slag, 48% of the slag, and 5% of the desulfurized gypsum as raw materials. After dry mixing for 120 seconds, add mixing water, control the water-cement ratio at 0.29, and stir until a moist granular mixture is formed.
[0040] The moist granular mixture is loaded into a mold and unidirectionally pressed under a pressure of 20 MPa for 120 seconds to obtain a fly ash-based pressed blank.
[0041] The pressed green body was placed in a 2450MHz microwave processing cavity and subjected to pulsed microwave treatment, with a microwave on / off cycle of 60 seconds for a total on time of 8 minutes. Based on the green body's initial mass, the microwave power density was approximately 0.55 W / g. During the treatment, an infrared thermometer continuously monitored the surface temperature of the green body. By adjusting the microwave output power and irradiation state, the surface temperature was gradually increased to approximately 75°C, with an average heating rate of approximately 3.5°C / min during the heating phase. After microwave-assisted damp heat treatment, the mass of the pressed green body was measured, and the mass loss rate was approximately 2.8%.
[0042] Subsequently, the preform treated with microwave-assisted hydrothermal heat was cured for 28 days at a temperature of 20±2℃ and a relative humidity of not less than 95% to obtain a self-sealing fly ash-based pressed and cured body. The process flow diagram of the self-sealing fly ash-based pressed and cured body is shown below. Figure 2 As shown.
[0043] Example 2 A method for preparing a self-sealing fly ash-based compressed solidified body includes the following steps: Based on the total mass of the cementitious components, weigh out 40% of the fly ash from municipal solid waste incineration that has not undergone water washing and dechlorination treatment, 10% of the calcium carbide slag, 40% of the slag, 5% of the desulfurization ash, and 5% of the calcined coal gangue powder as raw materials. After dry mixing for 120 seconds, control the water-cement ratio to 0.3, add mixing water, and stir until a moist granular mixture is formed.
[0044] The moist granular mixture is loaded into a mold and unidirectionally pressed under a pressure of 25 MPa for 180 seconds to obtain a fly ash-based pressed blank.
[0045] The pressed preform was placed in a 2450MHz microwave processing cavity and subjected to continuous microwave processing for a total microwave on-time of 30 minutes. Based on the preform's initial mass, the microwave power density was approximately 0.32 W / g. During processing, an infrared thermometer continuously monitored the surface temperature of the pressed preform, and the microwave output power was adjusted according to the surface temperature changes to gradually raise the surface temperature to approximately 85℃, with an average heating rate of approximately 2.2℃ / min. After microwave-assisted hydrothermal treatment, the mass of the pressed preform was measured, with a mass loss rate of approximately 5.2%. It was then immediately covered with a film for moisture retention. The preform treated with microwave-assisted hydrothermal treatment was sealed and cured for 24 hours, followed by standard curing for 28 days to obtain a self-sealing fly ash-based pressed and cured body. The process flow diagram of the self-sealing fly ash-based pressed and cured body is shown below. Figure 2 As shown.
[0046] Example 3 A method for preparing a gradient fabric self-sealing fly ash-based compressed solidified body includes the following steps: The raw materials are divided into inner layer raw materials and outer layer raw materials. The inner layer raw materials, based on the total mass of the inner layer cementing components, include 45% unwashed and dechlorinated municipal solid waste incineration fly ash, 10% calcium carbide slag, and 45% slag. The outer layer raw materials, based on the total mass of the outer layer cementing components, include 25% unwashed and dechlorinated municipal solid waste incineration fly ash, 15% calcium carbide slag, 50% slag, 5% desulfurized gypsum, and 5% calcined coal gangue powder.
[0047] The inner and outer layer raw materials were mixed with mixing water at a water-to-binder ratio of 0.25 to obtain an inner layer of salt-containing moist granules 1 and an outer layer of salt-containing moist granules 2. Salt-containing moist granules 2 were first laid on the bottom and side walls of the mold, then salt-containing moist granules 1 was added, and finally salt-containing moist granules 2 were placed on top. The mold was then unidirectionally pressed under a pressure of 25 MPa and held for 180 seconds to obtain a pressed blank with an outer salt-freezing responsive protective layer and an inner load-bearing solidified core layer.
[0048] The pressed preform was placed in a 2450MHz microwave processing cavity and subjected to pulsed microwave treatment with a 60s on / off cycle for a total of 8 minutes. The microwave power density was approximately 0.50 W / g based on the preform's initial mass. During the treatment, an infrared thermometer continuously monitored the surface temperature of the preform. By adjusting the microwave output power and the microwave irradiation / intermittent state, the surface temperature was gradually increased, with the maximum surface temperature controlled within 75℃. The average heating rate during the heating phase was approximately 3.2℃ / min. After microwave-assisted hydrothermal treatment, the mass of the pressed preform was measured, with a mass loss rate of approximately 2.5%. The preform was then immediately covered with a film for moisture retention and cured for 28 days at 20±2℃ and a relative humidity of not less than 95%, yielding a self-sealing fly ash-based pressed and cured body. The process flow diagram for this self-sealing fly ash-based pressed and cured body is shown below. Figure 2 As shown.
[0049] In this gradient structure, the ratio of relatively low fly ash, high slag, and high compensating components in the outer layer is conducive to the preferential formation of a salt-freezing protective layer and provides reaction phase generation sites; the relatively high fly ash ratio in the inner layer is conducive to improving fly ash disposal capacity and load-bearing solidification capacity.
[0050] Example 4 Compared with Example 1, Example 4 differs only in the raw material ratio. The proportions of 35% fly ash from municipal solid waste incineration without water washing and dechlorination treatment, 12% calcium carbide slag, 48% slag, and 5% desulfurized gypsum by weight of cementing components in Example 1 are replaced with 20% fly ash from municipal solid waste incineration without water washing and dechlorination treatment, 25% calcium carbide slag, 40% slag, and 15% desulfurized gypsum by weight of cementing components. The rest is the same as in Example 1. After microwave-assisted wet heat treatment, the mass of the pressed green body was measured, and the mass loss rate was approximately 8%.
[0051] Example 5 Compared with Example 1, Example 5 differs only in the water-binder ratio. The water-binder ratio of 0.29 in Example 1 is replaced with 0.40. Everything else is the same as in Example 1. After microwave-assisted wet heat treatment, the mass of the pressed blank was measured, and the mass loss rate was about 5.4%.
[0052] Example 6 The only difference between Example 6 and Example 2 is the early sealing and curing time after microwave-assisted damp heat treatment. The sealing and curing time of 24 hours in Example 2 is adjusted to 48 hours before standard curing to the specified age. The other raw material composition, water-to-binder ratio, mixing method, pressing and molding conditions and microwave-assisted damp heat treatment conditions are the same as in Example 2.
[0053] Example 7 Example 7 differs from Example 2 only in that, based on the total mass of the cementitious components, it uses 35% unwashed and dechlorinated municipal solid waste incineration fly ash, 5% calcium carbide slag, 40% blast furnace slag, and 20% calcined coal gangue powder as raw materials; the water-cement ratio is adjusted to 0.20; the pressing pressure is adjusted to 40 MPa, and the holding time is adjusted to 20 s; after microwave-assisted hydrothermal treatment, it is sealed and cured for 6 hours, and then cured according to standard to the specified age. All other mixing methods and microwave-assisted hydrothermal treatment conditions are the same as in Example 2. After the microwave-assisted hydrothermal treatment, the mass of the pressed green body is measured, and the mass loss rate is approximately 3.6%.
[0054] Example 8 Example 8 differs from Example 2 only in that, based on the total mass of the cementitious components, it uses 55% unwashed and dechlorinated municipal solid waste incineration fly ash, 5% calcium carbide slag, 25% blast furnace slag, 5% desulfurization ash, and 10% calcined coal gangue powder as raw materials; the water-cement ratio is adjusted to 0.40; the pressing pressure is adjusted to 5 MPa; and the holding time is adjusted to 300 s. The remaining mixing methods, microwave-assisted hydrothermal treatment conditions, and subsequent curing regime are the same as in Example 2. After the microwave-assisted hydrothermal treatment, the mass of the pressed green body was measured, and the mass loss rate was approximately 6.1%.
[0055] Example 9 Compared with Example 2, Example 9 differs only in the raw material ratio: based on the total mass of the cementitious components, it uses 20% fly ash from municipal solid waste incineration without water washing and dechlorination treatment, 5% calcium carbide slag, 70% slag, 2% desulfurization ash, and 3% calcined coal gangue powder. The rest is the same as in Example 2. After microwave-assisted wet heat treatment, the mass of the pressed green body was measured, and the mass loss rate was about 8%.
[0056] Example 10 Compared with Example 2, Example 10 differs only in the raw material ratio: based on the total mass of the cementitious components, it uses 20% fly ash from municipal solid waste incineration without water washing and dechlorination treatment, 25% calcium carbide slag, 25% slag, 15% desulfurization ash, and 15% calcined coal gangue powder. The rest is the same as in Example 2. After microwave-assisted wet heat treatment, the mass of the pressed green body was measured, and the mass loss rate was about 5.8%.
[0057] Example 11 Compared with Example 2, Example 11 differs only in that the calcined coal gangue powder is replaced with red mud. Otherwise, it is the same as Example 2. After microwave-assisted wet heat treatment, the mass of the pressed green body is measured and the mass loss rate is about 8%.
[0058] Example 12 Compared with Example 2, Example 12 differs only in that calcined coal gangue powder is replaced with fly ash. Otherwise, it is the same as Example 2. After microwave-assisted wet heat treatment, the mass of the pressed blank is measured, and the mass loss rate is about 7.2%.
[0059] Example 13 The difference between Example 13 and Example 3 lies in the inner and outer raw materials and the processing conditions.
[0060] The raw materials are divided into inner layer raw materials and outer layer raw materials. The inner layer raw materials, based on the total mass of the inner layer cementing components, include 35% unwashed and dechlorinated municipal solid waste incineration fly ash, 5% calcium carbide slag, and 60% slag. The outer layer raw materials, based on the total mass of the outer layer cementing components, include 35% unwashed and dechlorinated municipal solid waste incineration fly ash, 10% calcium carbide slag, 40% slag, 5% desulfurized gypsum, and 10% calcined coal gangue powder.
[0061] The pressed preform was placed in a 2450MHz microwave processing cavity and subjected to pulsed microwave treatment, with a microwave on / off cycle of 10 seconds for a total on-time of 25 minutes. Based on the preform's initial mass, the microwave power density was approximately 0.10 W / g. During the treatment, an infrared thermometer continuously monitored the surface temperature of the preform. By adjusting the microwave output power and the microwave irradiation / intermittent state, the surface temperature was gradually increased, with the maximum surface temperature controlled within 45℃. The average heating rate during the heating phase was approximately 0.5℃ / min. After microwave-assisted hydrothermal treatment, the mass of the pressed preform was measured, with a mass loss rate of approximately 2.5%. The preform was then immediately covered with a film for moisture retention and cured for 28 days at a temperature of 20±2℃ and a relative humidity of not less than 95%, resulting in a self-sealing fly ash-based pressed and cured body. The process flow diagram for this self-sealing fly ash-based pressed and cured body is shown below. Figure 2 As shown.
[0062] Example 14 The difference between Example 14 and Example 3 lies in the inner and outer raw materials and the processing conditions.
[0063] The raw materials are divided into inner layer raw materials and outer layer raw materials. The inner layer raw materials, based on the total mass of the inner layer cementing components, include 47% unwashed and dechlorinated municipal solid waste incineration fly ash, 18% calcium carbide slag, and 35% slag. The outer layer raw materials, based on the total mass of the outer layer cementing components, include 10% unwashed and dechlorinated municipal solid waste incineration fly ash, 25% calcium carbide slag, 59% slag, 3% desulfurized gypsum, and 3% calcined coal gangue powder.
[0064] The pressed preform was placed in a 2450MHz microwave processing cavity and subjected to pulsed microwave treatment with a 180s on-time and 240s off-time, for a total microwave on-time of 10.5 min. Based on the preform's initial mass, the microwave power density was approximately 2 W / g. During the treatment, an infrared thermometer continuously monitored the surface temperature of the pressed preform. By adjusting the microwave output power and the microwave irradiation / intermittent state, the surface temperature was gradually increased, with the maximum surface temperature controlled within 85℃. The average heating rate during the heating phase was approximately 10℃ / min. After microwave-assisted hydrothermal treatment, the mass of the pressed preform was measured, with a mass loss rate of approximately 2.5%. It was then immediately covered with a film for moisture retention and cured for 28 days at 20±2℃ and a relative humidity of not less than 95%, yielding a self-sealing fly ash-based pressed and cured body. The process flow diagram for this self-sealing fly ash-based pressed and cured body is shown below. Figure 2 As shown.
[0065] Example 15 The difference between Example 15 and Example 3 lies in the inner and outer layer materials.
[0066] The raw materials were divided into inner layer raw materials and outer layer raw materials. The inner layer raw materials, based on the total mass of the inner layer cementing components, included 55% unwashed and dechlorinated municipal solid waste incineration fly ash, 5% calcium carbide slag, 35% blast furnace slag, and 5% desulfurized gypsum. The outer layer raw materials, based on the total mass of the outer layer cementing components, included 10% unwashed and dechlorinated municipal solid waste incineration fly ash, 14% calcium carbide slag, 70% blast furnace slag, 3% desulfurized gypsum, and 3% calcined coal gangue powder. The mass of the pressed green body was measured after microwave-assisted wet heat treatment, and the mass loss rate was approximately 2.1%.
[0067] Example 16 The difference between Example 16 and Example 3 lies in the inner and outer layer materials.
[0068] The raw materials were divided into inner and outer layers. The inner layer raw materials, based on the total mass of the inner layer cementing components, included 50% unwashed and dechlorinated municipal solid waste incineration fly ash, 5% calcium carbide slag, 35% blast furnace slag, and 10% calcined coal gangue powder. The outer layer raw materials, based on the total mass of the outer layer cementing components, included 15% unwashed and dechlorinated municipal solid waste incineration fly ash, 10% calcium carbide slag, 40% blast furnace slag, 15% desulfurized gypsum, and 20% calcined coal gangue powder. After microwave-assisted wet heat treatment, the mass of the pressed green body was measured, and the mass loss rate was approximately 2.8%.
[0069] Example 17 The difference between Example 17 and Example 3 lies in the inner and outer layer materials.
[0070] The raw materials were divided into inner layer raw materials and outer layer raw materials. The inner layer raw materials, based on the total mass of the inner layer cementing components, included 50% unwashed and dechlorinated municipal solid waste incineration fly ash, 5% calcium carbide slag, 35% blast furnace slag, 3% desulfurized gypsum, and 7% calcined coal gangue powder. The outer layer raw materials, based on the total mass of the outer layer cementing components, included 35% unwashed and dechlorinated municipal solid waste incineration fly ash, 19% calcium carbide slag, 40% blast furnace slag, 3% desulfurized gypsum, and 3% calcined coal gangue powder. After microwave-assisted wet heat treatment, the mass of the pressed green body was measured, and the mass loss rate was approximately 2.4%.
[0071] Example 18 The difference between Example 18 and Example 3 lies in the water-to-binder ratio and pressing conditions.
[0072] The inner and outer layer raw materials given in Example 3 were added to mixing water at a water-to-binder ratio of 0.25 and mixed to obtain inner layer salt-containing moist granules 1 and outer layer salt-containing moist granules 2. Salt-containing moist granules 2 were first laid on the bottom and side walls of the mold, then salt-containing moist granules 1 was added, and finally salt-containing moist granules 2 were covered. The mold was then unidirectionally pressed under a pressure of 25 MPa and held for 180 seconds to obtain a pressed blank with an outer salt-freezing responsive protective layer and an inner load-bearing solidified core layer. Alternatively, the inner and outer layer raw materials were added to mixing water at a water-to-binder ratio of 0.20 and mixed to obtain inner layer salt-containing moist granules 1 and outer layer salt-containing moist granules 2. First, salt-containing moist granules 2 are laid on the bottom and side walls of the mold, then salt-containing moist granules 1 are added, and finally salt-containing moist granules 2 are covered. The mold is unidirectionally pressed and molded under a pressure of 5 MPa and held for 300 s to obtain a pressed blank with an outer salt-freezing response protective layer and an inner load-bearing solidified core layer. After microwave-assisted damp heat treatment, the mass of the pressed blank is measured and the mass loss rate is about 3.0%.
[0073] Example 19 The difference between Example 19 and Example 3 lies in the water-to-binder ratio and pressing conditions.
[0074] The inner and outer layer raw materials given in Example 3 were added to mixing water at a water-to-binder ratio of 0.25 and mixed to obtain inner layer salt-containing moist granules 1 and outer layer salt-containing moist granules 2. Salt-containing moist granules 2 were first laid on the bottom and side walls of the mold, then salt-containing moist granules 1 was added, and finally salt-containing moist granules 2 were covered. The mold was then unidirectionally pressed under a pressure of 25 MPa and held for 180 seconds to obtain a pressed blank with an outer salt-freezing responsive protective layer and an inner load-bearing solidified core layer. Alternatively, the inner and outer layer raw materials were added to mixing water at a water-to-binder ratio of 0.40 and mixed to obtain inner layer salt-containing moist granules 1 and outer layer salt-containing moist granules 2. First, salt-containing moist granules 2 are laid on the bottom and side walls of the mold, then salt-containing moist granules 1 are added, and finally salt-containing moist granules 2 are covered. The mold is unidirectionally pressed and molded under a pressure of 40 MPa and held for 20 seconds to obtain a pressed blank with an outer salt-freezing response protective layer and an inner load-bearing solidified core layer. After microwave-assisted damp heat treatment, the mass of the pressed blank is measured, and the mass loss rate is about 2.9%.
[0075] The self-sealing fly ash-based pressed solidified bodies described in Examples 1 to 19 above were all able to be prepared. The performance of the self-sealing fly ash-based pressed solidified bodies prepared in Examples 1 to 3 is now preferred for verification.
[0076] Comparative Example 1 Comparative Example 1 used the same raw materials and pressing conditions as Example 1, but without microwave-assisted hydrothermal treatment; only standard curing was performed. This Comparative Example 1 is used to illustrate the effect of microwave-assisted hydrothermal treatment on the redistribution of pore fluid and the regulation of the degree of early hydration reaction.
[0077] Comparative Example 2 Comparative Example 2 used the same raw materials and microwave treatment method as Example 1, but increased the water-to-binder ratio to 0.55 and employed casting molding instead of compression molding. This Comparative Example 2 was used to illustrate the contribution of low water-to-binder ratio compression molding to the initial pore structure and salt freeze resistance.
[0078] Comparative Example 3 Comparative Example 3 used the same raw material pressing conditions and microwave treatment method as Example 1, but used fly ash that had been washed and dechlorinated with water as the raw material. This Comparative Example 3 is used to illustrate the effect of retaining the endogenous chloride salts in fly ash on the formation of Cl-AFm phases such as Friedel salts and the ability of chloride salts to bind.
[0079] Comparative Example 4 Comparative Example 4 used the same pressing conditions and microwave treatment as Example 1, but the mass percentage of each gelling component was different.
[0080] Based on the total mass of the cementitious components, the following were used: 10% unwashed and dechlorinated fly ash, 10% carbide slag, 30% slag, 10% desulfurization ash, and 40% calcined coal gangue powder. The rest were the same as in Example 1.
[0081] Comparative Example 5 Comparative Example 5 used the same raw materials and microwave treatment method as Example 1, but reduced the water-to-binder ratio to 0.05 for compression molding.
[0082] Comparative Example 6 Comparative Example 6 used the same raw materials and microwave treatment method as Example 1, but the pressing conditions were different, and the pressure was maintained at 100 MPa for 10 seconds.
[0083] Comparative Example 7 Comparative Example 7 used the same raw materials and microwave treatment method as Example 1, but the pressing conditions were different, and the pressure was maintained at 1 MPa for 500s.
[0084] Comparative Example 8 Comparative Example 8 used the same raw materials and pressing conditions as Example 1, but the microwave treatment method was different. Microwave-assisted wet heat treatment was applied to the pressed green body at a power density of 0.05 W / g.
[0085] Comparative Example 9 Comparative Example 9 used the same raw materials and pressing conditions as Example 1, but the microwave treatment method was different. Microwave-assisted wet heat treatment was applied to the pressed green body at a power density of 5.0 W / g.
[0086] Comparative Example 10 Comparative Example 10 used the same raw materials and pressing conditions as Example 1, but the microwave treatment method was different. Microwave-assisted wet heat treatment was applied to the pressed blank at a heating rate of 0.1℃ / min, and the treatment was carried out for a total of 100min under the condition that the surface temperature of the pressed blank was controlled at 30℃.
[0087] Comparative Example 11 Comparative Example 11 used the same raw materials and pressing conditions as Example 1, but the microwave treatment method was different. Microwave-assisted wet heat treatment was applied to the pressed blank at a heating rate of 20°C / min, and the treatment was carried out for a total of 4 minutes under the condition that the surface temperature of the pressed blank was controlled at 100°C.
[0088] Mechanism explanation of Comparative Examples 4 to 11 In Comparative Example 4, the fly ash content was lower than the lower limit of the present invention and the content of solid waste aluminum-silica material was too high. The fly ash disposal capacity and the supply of endogenous chloride salts were insufficient. At the same time, the calcium-silicon-aluminum ratio of the system deviated from the scope of the present invention, making it difficult to take into account the large-scale utilization of hazardous waste, early forming strength and continuous generation of Cl-AFm phase.
[0089] The water-cement ratio of Comparative Example 5 is only 0.05, which can be used to dissolve soluble salts in fly ash and support the early hydration of slag. However, the water content is insufficient, making it difficult for the mixture to form a uniform and continuous water film, which easily leads to dry material agglomeration, interface defects, and insufficient subsequent reactions.
[0090] Comparative Example 6, under 100MPa high pressure, only held for 10s, may cause obvious density gradient, interlayer stress and particle breakage, and cause excessive pore closure, which is not conducive to the uniform migration of pore fluid in the later stage, and at the same time significantly increases molding energy consumption.
[0091] Comparative Example 7, with only 1 MPa pressure applied, could not achieve sufficient initial density even with extended pressure holding time. The solidified body had a high interconnected porosity, making it easier for salt solution and freeze-thaw water to penetrate.
[0092] The power density of Comparative Example 8 was only 0.05 W / g, and the temperature rise of the aqueous phase and the redistribution of the pore liquid were insufficient, making it difficult to form an effective microwave-assisted hygrothermal promotion effect.
[0093] Comparative Example 9 has a power density of 5.0 W / g, which easily generates local hot spots and rapid moisture vaporization, leading to surface drying, abnormal salt enrichment, vapor pressure accumulation, and microcrack propagation.
[0094] The average heating rate and the highest surface temperature of Comparative Example 10 are both lower than the range defined in this invention. To reach the set temperature, the processing time needs to be significantly extended. It is still difficult to form an effective microwave-assisted humid heat regulation effect within a reasonable time. The effects of pore liquid migration, soluble salt redistribution and early hydration promotion are insufficient, and the processing efficiency is low.
[0095] The average heating rate and the highest surface temperature of Comparative Example 11 are both higher than the limits of this invention. Rapid microwave heating causes the pressed blank to reach a high surface temperature in a short time, which can easily lead to rapid local moisture vaporization, surface water loss, vapor pressure accumulation and increased thermal stress. It may also cause the quality loss rate to exceed the process control requirements, which is not conducive to maintaining the structural integrity of the pressed blank and subsequent continuous hydration.
[0096] Experimental Test Evaluation of freeze-thaw resistance The cured body, after being cured to the specified age, was evaluated using a slow freeze-thaw test method. The compressive strength, mass, relative dynamic elastic modulus, and apparent crack condition were tested before and after the freeze-thaw cycle. The strength retention rate, mass loss rate, relative dynamic elastic modulus retention rate, and crack grade were used as the main evaluation indicators.
[0097] It should be noted that the strength retention rate, mass loss rate, and relative dynamic elastic modulus retention rate after freeze-thaw cycles are mainly used to evaluate the freeze-thaw damage suppression ability of the cured body and cannot be equated with damage repair alone. To evaluate the self-sealing behavior after freeze-thaw damage, the initial crack width, capillary water absorption coefficient, and relative dynamic elastic modulus can be recorded after a preset freeze-thaw cycle. Then, the body can be transferred to an environment at 20±2℃ and a relative humidity of not less than 95% or a specified salt solution for curing for 7 to 28 days, and the crack closure rate, capillary water absorption coefficient recovery rate, and relative dynamic elastic modulus recovery rate can be retested. When the above recovery test is not carried out, the effect of freeze-thaw action in this invention is described as damage suppression and microcrack self-sealing, rather than complete restoration of the original performance.
[0098] Salt erosion resistance evaluation The solidified body was immersed in chloride and sulfate solutions for testing, and its compressive strength, mass change, volume stability, apparent cracks, pore structure changes, and heavy metal concentration in the immersion solution were tested periodically. Chloride corrosion mainly evaluated the binding capacity of exogenous Cl⁻ and changes in pore connectivity; sulfate corrosion mainly evaluated the appropriate formation of sulfur-containing stationary phases such as AFt, the risk of expansion and cracking, and the ability to maintain strength.
[0099] Stability evaluation of heavy metals According to GB 5085.3-2007, the leaching concentrations of heavy metals such as Pb, Zn, Cu, and Cd in the solidified body at the specified age are determined. To evaluate the migration risk after salt freezing service, leaching tests can be conducted before and after freeze-thaw cycles, NaCl immersion, and Na2SO4 immersion, and the increase in leaching concentration, cumulative release, and retention levels after environmental effects are compared. The results of a single leaching at the specified age are used to evaluate the phased stabilization effect, while long-term stability should be comprehensively judged based on continuous or phased leaching results after environmental effects.
[0100] The self-sealing performance of pores and microcracks can be comprehensively evaluated by the total porosity before and after immersion or salt freezing, the proportion of harmful pores >100nm, the capillary water absorption coefficient, and the crack filling rate in the microscopic image. The crack filling rate can be calculated based on the change in crack area or crack width before and after the reaction in the same observation area, and combined with SEM, BSE or X-ray micro-CT to observe the deposition location of the filling product on the pore wall and crack.
[0101] Table 1 shows the durability test results. Group 28-day compressive strength / MPa Strength retention rate after 100 freeze-thaw cycles / % Mass loss after 100 freeze-thaw cycles / % Strength retention rate after 90 days of NaCl immersion / % <![CDATA[Strength retention after 90 days of Na2SO4 immersion / %]]> Example 1 40.1 86 1.5 91 90 Example 2 41.2 89 1.2 93 92 Example 3 40.8 91 0.9 92 93.5 Comparative Example 1 32.5 77 3.2 81 80 Comparative Example 2 21.9 63 6.5 72 66 Comparative Example 3 25.8 74 4.0 79 75 As shown in Table 1, under the same or similar raw material conditions, Example 1, after microwave-assisted hydrothermal treatment, exhibited higher 28-day compressive strength, strength retention rate after freeze-thaw cycles, and strength retention rate after salt erosion than Comparative Example 1 without microwave-assisted hydrothermal treatment. This indicates that low-temperature microwave-assisted hydrothermal treatment is beneficial for improving the early reaction degree and durability. In Example 2, the introduction of solid waste aluminum-silicon compensating components further improved performance after freeze-thaw cycles and salt erosion, indicating that supplementing aluminum-silicon reaction sites is beneficial for the synergistic formation of Cl-AFm phase, AFt phase, and C-(A)-SH gel. In Example 3, the adoption of a gradient structure resulted in the lowest mass loss after 100 freeze-thaw cycles and a high strength retention rate after salt immersion, indicating that the outer salt-freeze response protective layer can delay the entry of external corrosive media into the inner layer, improving overall salt-freeze resistance. Comparative Example 2 had the worst durability because of its high water-cement ratio and casting process, resulting in a higher initial porosity and easier penetration of salt solution and freeze-thaw water. Comparative Example 3 had a reduced Cl-AFm phase formation ability after being washed with dechlorinated fly ash, which weakened its resistance to chloride salt corrosion and pore self-sealing ability.
[0102] Table 2. Test results of heavy metal leaching performance at the specified age (28 days) Group Pb / (mg / L) Zn / (mg / L) Cu / (mg / L) Cd / (mg / L) Example 1 0.045 0.110 0.030 0.003 Example 2 0.035 0.085 0.024 0.002 Example 3 0.028 0.070 0.020 0.002 Comparative Example 1 0.220 0.550 0.180 0.018 Comparative Example 2 0.180 0.420 0.130 0.012 Comparative Example 3 0.120 0.300 0.080 0.008 Table 2 shows that, at the specified aging period of 28 days, the leaching concentrations of Pb, Zn, Cu, and Cd in Examples 1 to 3 were all lower than those in the comparative example, indicating that low water-cement ratio pressing, microwave-assisted hydrothermal treatment, and synergistic formation of the reactive phase are beneficial for reducing the staged leaching levels of heavy metals. Among them, Example 3 had the lowest leaching concentration, indicating that the outer protective layer with a gradient structure is beneficial for reducing the entry of salt solution and the migration of heavy metals. Comparative Example 1 lacked microwave-assisted hydrothermal control, Comparative Example 2 had more interconnected pores due to high water-cement ratio casting, and Comparative Example 3 had relatively higher leaching concentrations because the fly ash was dechlorinated by water washing, which weakened the formation conditions of the Cl-AFm phase such as Friedel salt. It should be noted that Table 2 shows the results of a single leaching at the specified aging period, which can illustrate the staged stabilization effect, but cannot prove long-term stabilization on its own; the long-term migration risk should be further evaluated in conjunction with the changes in leaching concentration and cumulative release after freeze-thaw and salt erosion.
[0103] Table 3 Evaluation results of porosity and microcracks after NaCl immersion for 90 days Group Total porosity (%) after NaCl soaking for 90 days >100nm harmful pore ratio / % Capillary water absorption coefficient / (kg·m⁻²·h⁻¹ / ²) Microcrack filling rate / % Example 1 29.5 22.0 0.42 60 Example 2 28.9 19.5 0.39 65 Example 3 28.4 15.0 0.34 69 Comparative Example 1 34.8 31.0 0.57 38 Comparative Example 2 43.4 44.5 0.78 21 Comparative Example 3 35.6 35.5 0.59 35 As shown in Table 3, Examples 1-3 maintained low total porosity and harmful pore ratio after chloride salt immersion, with lower capillary water absorption coefficients and higher microcrack filling rates than the comparative example. This indicates that the reaction phase generation and subsequent hydration product filling described in this invention can form local sealing structures near pores, interfaces, and microcracks, thereby hindering salt migration. Example 3 showed the highest microcrack filling rate, indicating that the gradient structure and inner / outer layer ratio combination used in Example 3 are beneficial for improving the solidified body's response to the salt environment and its microcrack sealing ability.
[0104] Figure 1 This paper illustrates the four-stage process of self-sealing fly ash-based pressed solidified body from preparation to service response. In the first stage, unwashed dechlorinated fly ash, carbide slag, mineral slag, and solid waste sulfate / aluminosilicate materials are mixed and pressed at a low water-to-binder ratio. The particles rearrange to form an initial dense framework, while retaining the internal Cl- from the fly ash. - And some unreacted active interfaces. In the second stage, low-temperature microwave-assisted hydrothermal treatment creates a controlled temperature rise and hydrothermal gradient through dielectric heating of the aqueous phase, promoting the local migration and redistribution of pore fluid, soluble salts, and alkaline components, and facilitating the early formation of Cl-AFm and AFt phases such as C-(A)-SH gel and Friedel salt in the particle contact area. In the third stage, under salt-freezing service conditions, exogenous Cl⁻ and SO₄²⁻... 2- Moisture preferentially enters the outer response zone along residual pores and microcracks, while the low-connectivity pore structure formed by compression delays its migration to the inner layer. In the fourth stage, the brine entering the pores and microcracks continues to react with the retained slag glass phase, aluminosilicate phase, and calcium-alkali source. The secondary generated gel, Cl-AFm phase, and AFt phase are deposited and filled at the pore walls, interfaces, and cracks, narrowing the capillary channels, reducing crack connectivity, and reducing the risk of heavy metal migration through physical barriers, gel encapsulation, and ion binding. For gradient structures, the higher content of slag, carbide slag, and compensating components in the outer layer causes the above response to occur preferentially at the surface, further forming a brine migration retardation zone.
[0105] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.
Claims
1. A method for preparing a self-sealing fly ash-based compressed solidified body, characterized in that, Includes the following steps: The cementitious component is added to mixing water and mixed at a water-cement ratio of 0.20–0.40 to obtain salt-containing moist granules. The salt-containing moist granules are pressed and shaped under a pressure of 5 MPa–40 MPa for 20–300 seconds to obtain a pressed green body. The cementitious component contains the following raw materials in the following mass percentages: 20%–55% fly ash that has not been washed and dechlorinated, 5%–25% carbide slag, 25%–70% slag, 0%–15% solid waste sulfate, and 0%–20% solid waste aluminum silicon. The sum of the mass percentages of the raw materials is 100%, and the mass percentages of solid waste sulfate and solid waste aluminum silicon are not both 0. Microwave-assisted wet heat treatment was applied to the pressed preform at a power density of 0.1 W / g to 2.0 W / g. During the heating stage, the surface temperature of the pressed preform was increased at an average rate of 0.5℃ / min to 10℃ / min, and the maximum surface temperature was controlled at 45℃ to 85℃. The cumulative microwave irradiation time was 8 min to 30 min, and the mass loss rate of the treated pressed preform did not exceed 8%. Subsequently, the treated pressed preform was subjected to moist curing or standard curing to obtain a self-sealing fly ash-based pressed solidified body.
2. The method for preparing the self-sealing fly ash-based pressed and cured body according to claim 1, characterized in that, The gelling component is divided into an inner gelling component and an outer gelling component, which are mixed with mixing water at a water-to-gel ratio of 0.20 to 0.40 to obtain an inner layer of salt-containing moist granules and an outer layer of salt-containing moist granules. The outer layer of salt-containing moist granules is arranged on the outer periphery of the inner layer of salt-containing moist granules and pressed in one step to obtain a pressed blank with an inner load-bearing solidified core layer and an outer salt-freezing response layer. The pressed blank has an inner and outer gradient partition structure. The inner cementing component comprises 35%–55% untreated municipal solid waste incineration fly ash, 5%–18% calcium carbide slag, 35%–60% blast furnace slag, 0%–5% solid waste sulfate components, and 0%–10% solid waste aluminum silicon. The outer cementing component comprises 10%–35% untreated municipal solid waste incineration fly ash, 10%–25% calcium carbide slag, 40%–70% blast furnace slag, 3%–15% solid waste sulfate components, and 3%–20% solid waste aluminum silicon. The sum of the mass percentages of each component in both the inner and outer cementing components is 100%.
3. The method for preparing the self-sealing fly ash-based pressed and cured body according to claim 1, characterized in that, The microwave-assisted damp heat treatment method is either continuous treatment or pulse treatment. When pulse treatment is used, the microwave irradiation duration is 10s to 180s and the interval duration is 10s to 240s within each pulse cycle, and the process is repeated according to the above irradiation and interval parameters.
4. The method for preparing the self-sealing fly ash-based pressed and cured body according to claim 1, characterized in that, Solid waste sulfate is one or more of the following: desulfurized gypsum, phosphogypsum, titanium gypsum, fluorogypsum, desulfurized ash, circulating fluidized bed solid sulfur ash, or sulfur-containing slag. Solid waste aluminum silicon is one or more of the following: red mud, fly ash, calcined coal gangue powder, aluminum ash washing slag, tailings powder, recycled brick powder, and waste ceramic powder.
5. The method for preparing the self-sealing fly ash-based pressed and cured body according to claim 1, characterized in that, The water-to-binder ratio is 0.20 to 0.
30.
6. The method for preparing the self-sealing fly ash-based pressed and cured body according to claim 1, characterized in that, The pressing and molding method is one of unidirectional pressing, bidirectional pressing, molding, or vibration pressing.
7. The method for preparing the self-sealing fly ash-based pressed and cured body according to claim 1, characterized in that, Spray water onto the surface of the pressed blank, cover it with a film to keep it moist, or place it in an environment with a relative humidity of not less than 80% to maintain the moisture required for the dissolution-redistribution and hydration reaction of soluble salts.
8. The method for preparing a self-sealing fly ash-based pressed and cured body according to claim 1, characterized in that, After microwave-assisted damp heat treatment, cure for 3 to 28 days at a temperature of 18℃ to 22℃ and a relative humidity of not less than 95%, or first cure in a sealed container for 6 to 48 hours and then cure according to standard until the specified age.
9. The self-sealing fly ash-based pressed solidified body prepared by the preparation method of the self-sealing fly ash-based pressed solidified body according to any one of claims 1 to 8.
10. The application of the self-sealing fly ash-based compressed solidified body according to claim 9 as a solid waste-based landfill pretreatment block, road base block, non-load-bearing building material, or landfill covering material.