Preparation method of phosphogypsum-based recycled aggregate from solid waste

The method of preparing phosphogypsum by mixing calcination and non-calcination treatment solves the problem of additive dependence in phosphogypsum-based recycled aggregates, realizes efficient and environmentally friendly preparation of phosphogypsum-based recycled aggregates, improves the removal rate and utilization rate of phosphogypsum, and ensures the performance and environmental friendliness of the products.

CN123106145APending Publication Date: 2026-11-17HUBEI JUHAI ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611540841.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing phosphogypsum-based recycled aggregates involve additive-dependent processes, which limit the amount of phosphogypsum that can be disposed of, result in high production costs and environmental pollution risks. Furthermore, exogenous chemical agents can easily introduce impurities, affecting the performance of the products.

Method used

A one-step preparation method is adopted, which uses calcined phosphogypsum and non-calcined modified phosphogypsum mixed together and processed by high-temperature calcination and non-calcination process to achieve homogeneous integration of the cementing component and the cemented component, avoiding the addition of external chemical additives. Based on the cementing activity and modification characteristics of phosphogypsum itself, a whole solid waste gypsum-based recycled aggregate is prepared.

Benefits of technology

This method achieves efficient removal and comprehensive utilization of phosphogypsum, avoids impurities introduced by exogenous chemical agents, improves the removal rate and comprehensive utilization rate of phosphogypsum, reduces preparation costs, and ensures the performance stability and environmental friendliness of the products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106145A_ABST
    Figure CN123106145A_ABST
Patent Text Reader

Abstract

This invention relates to the field of building materials technology, and provides a method for preparing a fully solid waste phosphogypsum-based recycled aggregate, comprising the following steps: calcined phosphogypsum is obtained by calcining and modifying phosphogypsum, and non-calcined modified phosphogypsum is obtained by phosphogypsum through processes such as water washing, neutralization, and flotation without calcination; calcined phosphogypsum and non-calcined modified phosphogypsum are mixed in a certain proportion to obtain a mixture; the mixture is stirred; the mixed mixture is granulated to obtain a preliminary recycled aggregate blank; the preliminary recycled aggregate blank is cured to obtain recycled aggregate; or the mixed mixture is pressed into a parent rock and then crushed and screened into recycled aggregate. This invention uses the byproducts of different harmless treatment of phosphogypsum as raw materials, relying on the inherent cementitious activity of calcined phosphogypsum and the homologous characteristics of attached water and hydrated cementitious materials in non-calcined modified phosphogypsum, to prepare a fully solid waste phosphogypsum-based recycled aggregate without adding any external chemical additives throughout the process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, and in particular to a method for preparing whole solid waste phosphogypsum-based recycled aggregate. Background Technology

[0002] Phosphogypsum is an industrial byproduct produced during the wet-process phosphoric acid production process, with calcium sulfate dihydrate (CaSO4·2H2O) as its main component. Statistics show that approximately 4-5 tons of phosphogypsum are generated for every ton of phosphoric acid produced. my country's annual phosphogypsum emissions have long remained at 70-80 million tons, with historical stockpiles exceeding 800 million tons. However, the comprehensive utilization rate has consistently hovered around 50%. The large-scale stockpiling of phosphogypsum not only occupies significant land resources, but also poses a significant environmental risk, as soluble phosphorus, fluorine, and heavy metals can leach into the soil and groundwater through rainwater. Therefore, improving the disposal and comprehensive utilization rate of phosphogypsum has become a crucial issue urgently needing to be addressed by the phosphorus chemical industry.

[0003] Converting phosphogypsum into lightweight building aggregate is considered a core direction for large-scale utilization, but current processes suffer from common defects when adapting to this type of raw material. In conventional large-scale preparation systems of recycled aggregate and gypsum-based aggregate, to ensure particle integrity, control setting and hardening rate, and optimize granulation effect, the process requires the addition of binders and setting-regulating admixtures (accelerators and retarders). This admixture-dependent process route has three limitations: First, the actual utilization amount of phosphogypsum per unit product is limited, and there is a hidden ceiling to improving the utilization rate. Second, the procurement and formulation of multiple types of chemical admixtures directly increases the overall cost of raw material preparation. Third, exogenous chemical agents can easily introduce impurities such as soluble salts and organic additives, leading to environmental risks such as deterioration of product performance and secondary pollution from solid waste resource recovery products. Summary of the Invention

[0004] This invention aims to at least solve one of the technical problems existing in related technologies. To this end, this invention proposes a method for preparing homogeneous phosphogypsum-based recycled aggregate from solid waste, aiming to prepare homogeneous phosphogypsum-based recycled aggregate from solid waste in a one-step process without adding external chemical additives.

[0005] The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to an embodiment of the present invention includes the following steps: Calcined phosphogypsum and non-calcined modified phosphogypsum are provided. The calcined phosphogypsum is obtained by calcining phosphogypsum at high temperature to achieve the crystal transformation of dihydrate calcium sulfate to hemihydrate calcium sulfate or anhydrous calcium sulfate. The non-calcined modified phosphogypsum is obtained by a non-calcining process from phosphogypsum. The calcined phosphogypsum and the non-calcined modified phosphogypsum are mixed in a certain proportion to obtain a mixture, wherein no chemical additives are added. The mixture is stirred together; The mixed material is granulated to obtain a preliminary recycled aggregate blank, which is then cured to obtain recycled aggregate; or, the mixed material is pressed into parent rock and then crushed and screened to obtain recycled aggregate.

[0006] The method for preparing homogeneous all-solid waste phosphogypsum-based recycled aggregate according to embodiments of the present invention uses bulk solid waste as the sole raw material to achieve homogeneous integration of the cementing component and the cemented component. Relying on the cementing activity of calcined phosphogypsum itself and the water-adhering characteristics of non-calcined modified phosphogypsum, no external chemical additives are added throughout the process, and homogeneous all-solid waste phosphogypsum-based recycled aggregate is prepared in one step.

[0007] According to one embodiment of the present invention, the calcination-free process includes at least one of water washing, neutralization, and flotation.

[0008] According to one embodiment of the present invention, the calcined phosphogypsum accounts for 20% to 99% of the mass of the mixture.

[0009] According to one embodiment of the present invention, the non-calcined modified phosphogypsum is obtained by homogenizing phosphogypsum with an alkaline substance accounting for 0.1% to 10% of the dry weight of phosphogypsum and then aging for ≥4.5 hours.

[0010] According to one embodiment of the present invention, the alkaline substance is selected from at least one of slag powder, carbide slag, calcium oxide, sodium hydroxide, and calcium hydroxide.

[0011] According to one embodiment of the present invention, the non-calcined modified phosphogypsum meets the following indicators: 100% passing rate through a 2.36mm square sieve, pH value ≥ 3.0, water-soluble phosphorus pentoxide ≤ 0.3%, water-soluble fluoride ion ≤ 0.2%, and 7-day compressive strength ≥ 0.5MPa.

[0012] According to one embodiment of the present invention, after the step of mixing the mixture, the mixture is loaded into the feeding silo, and when the feeding silo is full, the mixture reaches the initial setting stage.

[0013] According to one embodiment of the present invention, the total time from the start of mixing to the end of granulation is controlled between the initial setting time and the final setting time of the mixture.

[0014] According to one embodiment of the present invention, the curing time does not exceed 2 hours; The recycled aggregate has a 2-hour compressive strength ≥ 2.0 MPa, an initial water absorption rate ≤ 15% after 2 hours, and a softening coefficient ≥ 0.5 after 2 hours.

[0015] According to one embodiment of the present invention, the mixture is supplied to the granulation equipment using an intermittent continuous feeding method with a single or dual feeding bins; The intermittent continuous feeding method with dual feeding hoppers includes: feeding material into the first feeding hopper, and when the material in the first feeding hopper is full, the mixture just reaches the initial setting stage; while the first feeding hopper discharges material to the downstream granulation equipment for granulation, it feeds material into the second feeding hopper, and the first feeding hopper and the second feeding hopper intermittently and alternately feed material to the granulation equipment.

[0016] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the drawings used in the description of the embodiments or related technologies will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a schematic flowchart of the preparation method of the all-solid waste phosphogypsum-based recycled aggregate provided in the embodiments of the present invention.

[0019] Figure 2 This is a flowchart illustrating the phosphogypsum treatment process in the method for preparing all-solid-waste phosphogypsum-based recycled aggregate provided in this embodiment of the invention.

[0020] Figure 3 This is a process flow diagram of the preparation method of all-solid waste phosphogypsum-based recycled aggregate provided in the embodiments of the present invention.

[0021] Figure 4 This is a schematic diagram of the feeding structure in the preparation method of all-solid waste phosphogypsum-based recycled aggregate provided in the embodiments of the present invention. Detailed Implementation

[0022] The embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and should not be construed as limiting the scope of the invention.

[0023] In the description of the embodiments of the present invention, it should be noted that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of the present invention. In addition, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0024] In the description of the embodiments of the present invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "connected" and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of the present invention based on the specific circumstances.

[0025] In embodiments of the present invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0026] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0027] Please refer to the reference. Figure 1 , Figure 2 and Figure 3The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to an embodiment of the present invention includes the following steps: Step S1: Raw material preparation.

[0028] We offer calcined phosphogypsum and non-calcined modified phosphogypsum.

[0029] Preparation of calcined phosphogypsum: Calcination of phosphogypsum at high temperature transforms calcium sulfate dihydrate into calcium sulfate hemihydrate or anhydrous calcium sulfate crystals to obtain calcined phosphogypsum. The calcined phosphogypsum obtained after calcination meets the requirements of the "Building Gypsum" standard.

[0030] Preparation of non-calcined modified phosphogypsum: Phosphogypsum is treated with non-calcined processes such as water washing, neutralization, and flotation to obtain non-calcined modified phosphogypsum. Preferably, the non-calcined modified phosphogypsum is obtained by neutralization. Specifically, phosphogypsum is homogenized with an alkaline substance accounting for 0.1%~10% of the dry weight of the phosphogypsum, and then aged for ≥4.5 hours, i.e., after chemical modification and harmless treatment, non-calcined modified phosphogypsum is obtained. The alkaline substance is selected from at least one of slag powder, carbide slag, calcium oxide, sodium hydroxide, and calcium hydroxide. The obtained non-calcined modified phosphogypsum meets the following indicators: 100% passing rate through a 2.36mm square sieve, pH value ≥3.0, water-soluble phosphorus pentoxide ≤0.3%, water-soluble fluoride ion ≤0.2%, and 7-day compressive strength ≥0.5MPa.

[0031] Understandably, calcined phosphogypsum contains ≥60% hemihydrate / anhydrous gypsum and has a pH ≥6.0; non-calcined modified phosphogypsum is obtained from phosphogypsum through non-calcination processes such as water washing, neutralization, and flotation, and contains ≥60% dihydrate gypsum and a pH ≥3.0, with the difference in attached water content between the phosphogypsum before and after modification being ≤10%.

[0032] Step S2: Mix the ingredients.

[0033] Calcined phosphogypsum and non-calcined modified phosphogypsum are mixed in a certain proportion to obtain a mixture. The mass percentage of calcined phosphogypsum in the mixture is 20% to 99%. For example, if the calcined phosphogypsum accounts for 20%, then the non-calcined modified phosphogypsum accounts for 80%; or, if the calcined phosphogypsum accounts for 99%, then the non-calcined modified phosphogypsum accounts for 1%. No chemical additives are added during this mixing process.

[0034] Step S3: Mix.

[0035] The mixture is stirred to ensure thorough homogeneous mixing of calcined phosphogypsum and non-calcined modified phosphogypsum. During the stirring process, the calcined phosphogypsum begins a hydration reaction upon contact with water, and the system gradually acquires the driving force for hydration and gelation.

[0036] Step S4: Feeding and granulation.

[0037] The mixed material is loaded into the feeding silo and fed to the downstream granulation equipment for granulation and molding to obtain the initial blank of recycled aggregate.

[0038] The total time from mixing to granulation is controlled between the initial and final setting times of the mixture to ensure that the granules are formed in a state with sufficient plasticity, while utilizing the mixture's own coagulation and hardening process to achieve initial solidification of the granules.

[0039] Step S5: Maintenance.

[0040] The recycled aggregate blanks are cured for no more than 2 hours to obtain the finished recycled aggregate product.

[0041] The method for preparing solid waste-based recycled aggregate according to embodiments of the present invention uses bulk solid waste as raw material to achieve homogeneous integration of the cementing component and the cemented component. Relying on the cementing activity of calcined phosphogypsum itself and the high water content of non-calcined modified phosphogypsum, no external chemical additives are added throughout the process, thus rapidly and efficiently preparing solid waste-based recycled aggregate.

[0042] like Figure 4 As shown, in a preferred embodiment of the present invention, a dual-feeding silo intermittent continuous feeding method is used to supply the mixture to the granulation equipment.

[0043] Specifically, the system uses a belt conveyor to feed material into the first feeding hopper. When the first feeding hopper is full, the mixture has just reached the initial setting stage. At this point, the first feeding hopper discharges material to the downstream granulation equipment for granulation.

[0044] During the synchronous phase of unloading and granulating material from the first feeding silo to the downstream granulating equipment, the belt conveyor system simultaneously completes the filling operation to the second feeding silo.

[0045] The first and second feeding bins supply material to the granulator unit intermittently. That is, when the first feeding bin finishes unloading, the feeding switch to the second feeding bin, while the first feeding bin is re-feeded. Relying on the process layout of intermittently feeding the granulator unit from the two bins, the granulator equipment can be guaranteed to operate continuously without interruption. This feeding configuration can fully release the equipment's maximum capacity under large-scale production conditions.

[0046] Example 1: Calcined phosphogypsum and non-calcined modified phosphogypsum were measured and proportioned at a mass ratio of 90%:10%, and then mixed and granulated according to the above process route. After curing for 2 hours, recycled aggregate was obtained.

[0047] The recycled aggregate obtained in this embodiment has a 2-hour compressive strength of 5.7 MPa, an initial water absorption rate of 10.4% and an initial softening coefficient of 0.75, as tested.

[0048] Example 2: Calcined phosphogypsum and non-calcined modified phosphogypsum were measured and proportioned at a mass ratio of 80%:20%, and then mixed and granulated according to the above process route. After curing for 2 hours, recycled aggregate was obtained.

[0049] The recycled aggregate obtained in this embodiment has a 2-hour compressive strength of 4.9 MPa, an initial water absorption rate of 11.0% after 2 hours, and a softening coefficient of 0.71 after 2 hours, as tested.

[0050] Example 3: Calcined phosphogypsum and non-calcined modified phosphogypsum were measured and proportioned at a mass ratio of 70%:30%, and then mixed and granulated according to the above process route. After curing for 2 hours, recycled aggregate was obtained.

[0051] The recycled aggregate obtained in this embodiment has a 2-hour compressive strength of 4.2 MPa, an initial water absorption rate of 11.8% after 2 hours, and a softening coefficient of 0.68 after 2 hours, as tested.

[0052] Example 4: Calcined phosphogypsum and non-calcined modified phosphogypsum were measured and proportioned at a mass ratio of 60%:40%, and then mixed and granulated according to the above process route. After curing for 2 hours, recycled aggregate was obtained.

[0053] The recycled aggregate obtained in this embodiment has a 2-hour compressive strength of 3.4 MPa, an initial water absorption rate of 12.5% ​​after 2 hours, and a softening coefficient of 0.61 after 2 hours, as tested.

[0054] Example 5: Calcined phosphogypsum and non-calcined modified phosphogypsum were measured and proportioned at a mass ratio of 50%:50%, and then mixed and granulated according to the above process route. After curing for 2 hours, recycled aggregate was obtained.

[0055] The recycled aggregate obtained in this embodiment has a 2-hour compressive strength of 2.5 MPa, an initial water absorption rate of 14.2% after 2 hours, and a softening coefficient of 0.53 after 2 hours, as tested.

[0056] Example 6: Calcined phosphogypsum and non-calcined modified phosphogypsum were measured and proportioned at a mass ratio of 90%:10%, and then subjected to pressure pressing, curing, crushing and screening to obtain recycled aggregate.

[0057] The recycled aggregate obtained in this embodiment has a 2-hour compressive strength of 5.2 MPa, an initial water absorption rate of 11.2% after 2 hours, and a softening coefficient of 0.71 after 2 hours, as tested.

[0058] As can be seen from the above examples, with the increase of the content of non-calcined modified phosphogypsum (i.e., the proportion of calcined phosphogypsum decreases), the compressive strength and softening coefficient of the recycled aggregate show a decreasing trend, while the water absorption rate shows an increasing trend. In the mixture of calcined phosphogypsum and non-calcined modified phosphogypsum, when the mass ratio of calcined phosphogypsum is in the range of 70% to 90%, the recycled aggregate has better comprehensive performance—2-hour compressive strength ≥ 4.2 MPa, 2-hour water absorption rate ≤ 11.8%, and 2-hour softening coefficient ≥ 0.68.

[0059] The technical solution of the present invention has the following beneficial effects: All solid waste, zero additives: This process system uses bulk solid waste (phosphogypsum) as the sole raw material, achieving homogeneous integration of the cementing component and the cemented component. Relying on the inherent gelling activity of calcined phosphogypsum and the high water content of non-calcined modified phosphogypsum, no external chemical additives are added throughout the process. This allows for the rapid and efficient preparation of solid waste-based recycled aggregates, avoiding the risk of product performance degradation and secondary pollution caused by the introduction of soluble salts, organic additives, and other impurities from external chemical agents. Simultaneously, utilizing the homogeneous and recyclable characteristics of gypsum-based materials, it achieves green and circular full utilization. Furthermore, the all-solid waste phosphogypsum-based materials represent a significant innovation in terms of phosphogypsum removal rate and comprehensive utilization. The calcined phosphogypsum used in this technology is obtained through high-temperature calcination, during which adhering water is evaporated and crystal water is removed. The mass of the calcined phosphogypsum is approximately 60%–70% of that of the undiluted phosphogypsum. Therefore, when the calcined phosphogypsum content in the product is 60%~70%, it is equivalent to absorbing 100% of the original phosphogypsum. If the content of non-calcined modified phosphogypsum is also taken into account, the unit product can absorb more than 100% of the original phosphogypsum, which significantly improves the removal rate and comprehensive utilization rate of phosphogypsum.

[0060] Short curing cycle and high production efficiency: Relying on the physical and chemical properties of the raw materials and the rapid setting and hydration characteristics of calcined phosphogypsum, the total time from mixing to granulation is strictly controlled between the initial setting and the final setting. The granulation time is short and curing can be completed in just 2 hours, which greatly shortens the curing cycle of traditional gypsum granulation process and improves the turnover efficiency of single-line production.

[0061] The production process is stable and controllable: Since it does not involve fluctuations in the dosage of external additives, the solidification behavior of the system is stable, the key performance indicators such as mechanical strength and stability of the finished aggregate have small fluctuations, and the quality uniformity of the production process is easy to control.

[0062] Full release of equipment capacity: Through intermittent alternating feeding from dual feeding hoppers, a high material supply rate can be achieved, and the granulation equipment can operate continuously without interruption, fully releasing the equipment's maximum capacity under large-scale production conditions.

[0063] Finally, it should be noted that the above embodiments are only for illustrating the present invention and not for limiting the present invention. Although the present invention has been described in detail with reference to the embodiments, those skilled in the art should understand that various combinations, modifications, or equivalent substitutions of the technical solutions of the present invention do not depart from the spirit and scope of the technical solutions of the present invention and should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a whole solid waste phosphogypsum-based recycled aggregate, characterized in that, Includes the following steps: Calcined phosphogypsum and non-calcined modified phosphogypsum are provided. The calcined phosphogypsum is obtained by calcining phosphogypsum at high temperature to achieve the crystal transformation of dihydrate calcium sulfate to hemihydrate calcium sulfate or anhydrous calcium sulfate. The non-calcined modified phosphogypsum is obtained by a non-calcining process from phosphogypsum. The calcined phosphogypsum and the non-calcined modified phosphogypsum are mixed in a certain proportion to obtain a mixture, wherein no chemical additives are added. The mixture is stirred together; The mixed material is granulated to obtain a preliminary recycled aggregate blank, which is then cured to obtain recycled aggregate; or, the mixed material is pressed into parent rock and then crushed and screened to obtain recycled aggregate.

2. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 1, characterized in that, The calcination-free process includes at least one of water washing, neutralization, and flotation.

3. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 1, characterized in that, In the mixture, the calcined phosphogypsum accounts for 20% to 99% of the mass.

4. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 1, characterized in that, The non-calcined modified phosphogypsum is obtained by homogenizing phosphogypsum with 0.1% to 10% of an alkaline substance by dry weight of phosphogypsum and then aging for ≥4.5 hours.

5. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 4, characterized in that, The alkaline substance is selected from at least one of slag powder, carbide slag, calcium oxide, sodium hydroxide, and calcium hydroxide.

6. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 1, characterized in that, The non-calcined modified phosphogypsum meets the following indicators: 100% passing rate through a 2.36mm square sieve, pH value ≥ 3.0, water-soluble phosphorus pentoxide ≤ 0.3%, water-soluble fluoride ion ≤ 0.2%, and 7-day compressive strength ≥ 0.5MPa.

7. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 1, characterized in that, After the mixing step, the mixture is loaded into the feeding silo. When the feeding silo is full, the mixture reaches the initial setting stage.

8. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 1, characterized in that, The total time from the start of mixing to the end of granulation is controlled between the initial setting time and the final setting time of the mixture, and the aggregate forming or parent rock forming time is ≤10min.

9. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to claim 1, characterized in that, The curing time shall not exceed 2 hours; The recycled aggregate has a 2-hour compressive strength ≥ 2.0 MPa, an initial 2-hour water absorption rate ≤ 15%, and an initial 2-hour softening coefficient ≥ 0.

5.

10. The method for preparing all-solid waste phosphogypsum-based recycled aggregate according to any one of claims 1 to 9, characterized in that, The mixture is supplied to the granulation equipment using an intermittent continuous feeding method with a single or dual feeding bins. The time from the start of mixing to the completion of molding in each bin is precisely controlled to be before the final setting time, and there is no leakage. The intermittent continuous feeding method of the dual feeding silos includes: feeding material into the first feeding silo, and when the material in the first feeding silo is full, the mixture just reaches the initial setting stage; While the first feeding hopper discharges material to the downstream granulation equipment for granulation, it feeds material to the second feeding hopper. The first feeding hopper and the second feeding hopper intermittently and alternately feed material to the granulation equipment.