Cotton-based microcrystalline cellulose and preparation method and application thereof
Kapok-based microcrystalline cellulose was prepared by combining mild ethanol pretreatment, sodium hydroxide treatment, and dilute hydrochloric acid hydrolysis with freeze-drying technology. This solved the problems of high energy consumption and structural instability in traditional processes and achieved high-efficiency aqueous battery separator performance.
Patent Information
- Application Number
- CN202611245114.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to prepare microcrystalline cellulose materials with uniform pore networks and excellent hydrophilicity, which leads to the water-based battery separator easily absorbing water and swelling in the electrolyte, resulting in unstable structure. In addition, traditional processes are energy-intensive, highly corrosive to equipment, and difficult to control the pore structure.
Kapok-based microcrystalline cellulose was prepared by using a mild method of ethanol pretreatment, sodium hydroxide treatment, and dilute hydrochloric acid hydrolysis, combined with freeze-drying technology. This method preserves the natural hollow structure, forms a hierarchical porous structure and moderate hydrophilicity, and avoids swelling.
The process achieves excellent wettability and anti-swelling properties of kapok-based microcrystalline cellulose in aqueous battery separators, improving the battery's electrochemical window and cycle life. Moreover, the process is green, environmentally friendly, and low-cost.
Smart Images

Figure CN123106929A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-value utilization technology of biomass natural fibers, specifically relating to a kapok-based microcrystalline cellulose, its preparation method, and its application. Background Technology
[0002] Microcrystalline cellulose not only possesses advantages such as high purity, high crystallinity, and large specific surface area, but is also widely used as a reinforcing filler for polymer materials such as polylactic acid, polyurethane, and epoxy resin. In recent years, its application in porous membrane materials, especially in aqueous battery separators, has attracted much attention. However, aqueous separators place extremely high demands on the microstructure and physicochemical properties of the substrate: a uniform pore network is needed to homogenize ion flux and suppress metal dendrites, while excellent hydrophilicity is required to ensure rapid electrolyte wetting. Currently, conventional cellulose materials are caught in an irreconcilable technical dilemma in this field: especially traditional commercial wood pulp or cotton pulp-based microcrystalline cellulose, whose excessive hydrophilicity easily leads to catastrophic water absorption and swelling of the separator in aqueous electrolytes, resulting in the blockage of micropores inside the membrane, structural instability, and a precipitous drop in mechanical strength. Furthermore, traditional preparation processes struggle to precisely control the pore structure at the microscopic level. For instance, patent document CN 104293858A discloses a combined treatment method using bleached hardwood pulp as raw material, employing both mechanical force and biological enzymes. First, the pulp undergoes mechanical grinding to pass through a specific sieve, followed by the addition of a complex cellulase (including endoglucanase and exoglucanase) for hydrolysis. Another example is patent document CN... Patent document 102947343B discloses a method of acidifying wood pulp fiber materials, followed by washing and dehydration, and then subjecting them to deep acid hydrolysis at a high temperature of at least 120°C and high concentration conditions to obtain microcrystalline cellulose with a narrow particle size distribution. While this method, using mechanical processing and pure biological enzymes, is environmentally friendly, the mechanical pulping process is energy-intensive, and the enzyme reaction time is too long, making it difficult to control the crystallinity distribution of the product. Furthermore, this method primarily utilizes strong acids to hydrolyze wood pulp fibers at high temperatures. Strong acids not only have high corrosion resistance to equipment but also create a heavy burden for the subsequent treatment of acid waste liquid. More significantly, the aforementioned traditional high-intensity mechanical pulping or high-temperature strong acid hydrolysis processes often completely destroy the original natural three-dimensional framework of the fibers, resulting in a wide and disordered pore size distribution and severe pore structure collapse in the final product. This material, lacking a regular nanoscale mesoporous network, cannot meet the stringent requirements of functionalized membranes for structural stability and uniform ion transport. Summary of the Invention
[0003] Based on the aforementioned shortcomings and deficiencies in the prior art, one of the objectives of this invention is to at least solve one or more of the aforementioned problems in the prior art. In other words, one of the objectives of this invention is to provide a kapok-based microcrystalline cellulose, its preparation method, and its application that meet one or more of the aforementioned requirements.
[0004] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A method for preparing kapok-based microcrystalline cellulose includes the following steps: (1) Disperse natural kapok fibers in anhydrous ethanol, pretreat them by heating in a water bath at 65-70℃ for 20-40 minutes, then cool, wash and dry to obtain pretreated kapok fibers; (2) Disperse the pretreated kapok fiber in an aqueous sodium hydroxide solution and react at 80°C for 4-6 hours. Then cool, wash, and freeze dry at -80 to -50°C and a vacuum of less than 15 Pa for 24-48 hours to obtain kapok cellulose. (3) Disperse kapok cellulose in hydrochloric acid solution and react at 70-85℃ for 70-90 min. Then cool, wash, and freeze dry at freezing temperature of -80 to -50℃ and vacuum degree of less than 15 Pa for 24-48 h to obtain kapok-based microcrystalline cellulose.
[0005] As a preferred embodiment, in step (1), the mass ratio of natural kapok fiber to anhydrous ethanol is 1:(90-110).
[0006] As a preferred embodiment, in step (2), the mass ratio of pretreated kapok fiber to sodium hydroxide aqueous solution is 1:(40-60), and the concentration of sodium hydroxide aqueous solution is 2.5-3.0M.
[0007] As a preferred embodiment, in step (3), the mass ratio of kapok cellulose to hydrochloric acid aqueous solution is 1:(20-30), and the mass percentage of hydrochloric acid aqueous solution is 1.2-1.8%.
[0008] The present invention also provides kapok-based microcrystalline cellulose prepared by the preparation method described in any of the preceding embodiments.
[0009] As a preferred embodiment, the obtained kapok-based microcrystalline cellulose has a hierarchical porous structure, with the pore size distribution based on nitrogen adsorption-desorption testing concentrated between 2-10 nm, and the peak pore size between 2-4 nm.
[0010] As a preferred embodiment, the initial contact angle of the surface of the kapok-based microcrystalline cellulose with the aqueous electrolyte is 45-50°.
[0011] As a preferred embodiment, the initial thermal degradation temperature T0 of the kapok-based microcrystalline cellulose is greater than 340 °C, and the maximum thermal degradation rate temperature T0 is greater than 340 °C. max Greater than 365 ℃.
[0012] The present invention also provides the application of kapok-based microcrystalline cellulose as described in any of the preceding embodiments for the preparation of aqueous battery separators.
[0013] Compared with the prior art, the beneficial effects of this invention are: (1) This invention breaks through the traditional conventional morphology and achieves precise reconstruction of the natural hollow structure into a rigid mesoporous network: This invention utilizes the unique ultrathin cell wall and high natural hollowness of kapok, combined with mild dewaxing, controlled hydrolysis and freeze-drying processes, and uses water sublimation to completely eliminate capillary contraction force, avoiding the pore collapse commonly seen in conventional biomass (such as straw) extraction and conventional heat drying processes. The resulting kapok-based microcrystalline cellulose exhibits a highly concentrated hierarchical porous structure (peak pore size falls in the rigid mesoporous range of 2-10 nm), which completely changes the physical defects of the dense and non-porous traditional commercial microcrystalline cellulose (such as wood pulp-based), laying a unique microscopic framework for its functional applications; (2) This invention breaks the material paradox of "high hydrophilicity necessarily leads to high swelling" and establishes a balance: thanks to the specific rigid mesoporous network and appropriate amount of surface-active hydroxyl groups mentioned above, this invention exhibits a moderate initial contact angle of 40-50°. Compared with traditional high hydrophilic substrates that are extremely prone to water absorption, swelling and collapse, the material of this invention can achieve excellent instantaneous wetting of electrolyte and maintain an extremely high liquid retention rate, while using physical spatial confinement to firmly lock solvent molecules, keeping the surface swelling rate at an extremely low level, and exhibiting a significantly higher thermal degradation temperature than conventional microcrystalline cellulose; (3) This invention endows the battery separator with excellent anti-dendritic and long-term safety performance: When this material is used as the core filler of the aqueous battery separator, its uniform and abundant nanoporous network acts as an ideal ion guiding channel. This structure can not only homogenize the ion flux at the physical level and effectively suppress the growth of metal dendrites caused by excessive local ion concentration; its strong hydrogen bond network can also actively regulate the solvation sheath of ions, lock the free water in the electrolyte, reduce side reactions such as hydrogen evolution from the source, and greatly improve the electrochemical window and cycle life of aqueous secondary batteries. Attached Figure Description
[0014] Figure 1 This is a scanning electron microscope image of the kapok-based microcrystalline cellulose prepared in Example 1 of the present invention; Figure 2 The infrared spectra of the kapok-based microcrystalline cellulose K-MCC and kapok prepared in Example 1 of this invention are shown below. Figure 3 X-ray diffraction patterns of the kapok-based microcrystalline cellulose K-MCC and kapok prepared in Example 1 of this invention; Figure 4 Thermogravimetric analysis (TGA) diagrams of the kapok-based microcrystalline cellulose prepared in Example 1 of this invention and the microcrystalline cellulose of Comparative Examples 1-2 are shown. Figure 5The nitrogen adsorption-desorption isotherms and pore size distribution diagrams of the kapok-based microcrystalline cellulose prepared in Example 1 of this invention and the microcrystalline cellulose of Comparative Examples 1-2 are shown. Figure 6 This is a comparison chart of the contact angle test results of the kapok-based microcrystalline cellulose prepared in Example 1 of the present invention and the microcrystalline cellulose of Comparative Examples 1-2.
[0015] Figure 7 This is a comparison chart of the service performance of aqueous battery separators made from kapok-based microcrystalline cellulose prepared in Example 1 of the present invention and microcrystalline cellulose prepared in Comparative Examples 1-2. Detailed Implementation
[0016] The following provides a detailed description of the kapok-based microcrystalline cellulose of the present invention, its preparation method, and its applications.
[0017] The method for preparing kapok-based microcrystalline cellulose of this invention, as a high-value utilization technology of biomass-based natural fibers, is not only simple and environmentally friendly, but also produces a novel biomass microcrystalline cellulose with high purity and high crystallinity by removing hemicellulose from natural kapok through alkaline solution and constant-temperature hydrolysis with dilute hydrochloric acid. Furthermore, thanks to the extremely high natural hollowness and ultra-thin cell walls of kapok, the specific mild dewaxing and acid hydrolysis process of this invention effectively preserves and reconstructs its unique three-dimensional porous topological framework while removing non-cellulose components. This novel kapok-based microcrystalline cellulose exhibits a highly concentrated specific pore size distribution and a perfect balance of excellent electrolyte wettability and extremely low wet swelling without the need for additional modifying agents. Its moderately hydrophilic microenvironment and regular rigid framework physically prevent excessive swelling, perfectly breaking through the inherent technical bottleneck of existing aqueous membranes. It can be widely used in composite materials, battery membranes, pharmaceutical excipients, food, textiles, and other fields.
[0018] The microcrystalline cellulose prepared by this invention not only has extremely high crystallinity and excellent thermal stability, but also completely retains and reconstructs the natural three-dimensional topological framework unique to kapok, forming a micro-hierarchical porous structure with a specific mesoporous distribution range. This structure endows the material with extremely excellent liquid wetting and retention capabilities, and while achieving ultra-high hydrophilicity, it exhibits rare wet swelling resistance and mechanical stability. Moreover, the preparation process is mild and simple, green and environmentally friendly, with abundant raw material sources and low cost.
[0019] Specifically, the preparation method of the kapok-based microcrystalline cellulose of the present invention comprises the following steps: Step 1: Disperse natural kapok fibers in ethanol and pretreat them by heating in a water bath at 65-70℃ for 30 min to remove plant waxes and some lignin from the surface of the natural fibers. After the reaction is complete, remove the fibers, wash and dry them to obtain pretreated kapok fibers. Step 2: Disperse the pretreated kapok fibers in an aqueous sodium hydroxide solution and perform alkaline boiling treatment at 80-100 ℃ for 4-6 h. After the reaction is completed, cool the reaction product to room temperature, wash until neutral, and freeze-dry at a freezing temperature of -80 to -50 ℃ and a vacuum degree of less than 15 Pa for 24-48 h to obtain the secondary pretreated kapok fibers with some hemicellulose removed, namely kapok cellulose. Step 3: Mix the pretreated kapok fibers with dilute hydrochloric acid solution and place them in a reaction vessel for hydrolysis. React at 70-85℃ for 70-90 min. After the reaction is complete, cool to room temperature, wash until neutral, and freeze-dry at -80 to -50℃ and a vacuum degree of less than 15 Pa for 24-48 h to obtain high-purity kapok-based microcrystalline cellulose.
[0020] The kapok-based microcrystalline cellulose prepared by the above method uses natural kapok fiber as raw material. It innovatively introduces ethanol water bath pretreatment to efficiently remove plant waxes and other hindering substances from the fiber surface, allowing for a more thorough and complete subsequent sodium hydroxide alkaline boiling treatment. Finally, combined with controlled hydrolysis of hydrochloric acid in a reactor, a novel high-purity, high-crystallinity biomass microcrystalline material is constructed. This method effectively removes non-cellulose components from kapok, significantly improves the reaction efficiency at each stage, and solves the problem of incomplete removal of surface impurities and subsequent insufficient hydrolysis in traditional cellulose extraction processes.
[0021] In step one above, the mass ratio of natural kapok fiber to anhydrous ethanol is 1:(90-110). The specific mass ratio can be determined according to actual application requirements. In step two above, the mass ratio of pretreated kapok fiber to sodium hydroxide aqueous solution is 1:(40-60), and the concentration of sodium hydroxide aqueous solution is 2.5-3.0 M. The specific mass ratio and concentration can be determined according to the actual application requirements. In step three above, the mass ratio of the pretreated kapok cellulose to the hydrochloric acid aqueous solution is 1:(20-30), and the mass percentage of hydrochloric acid in the hydrochloric acid aqueous solution is 1.2-1.8%; the specific mass ratio and mass percentage can be determined according to the actual application requirements. The kapok-based microcrystalline cellulose prepared by this invention has a hierarchical porous structure. Based on nitrogen adsorption-desorption testing, its mesopores are located between 2-10 nm, with a peak pore size between 2-4 nm. The pore volume of the mesopores accounts for 60-80% of the total volume. Furthermore, the initial thermal degradation temperature T0 of the kapok-based microcrystalline cellulose is greater than 340 °C, and the maximum thermal degradation rate temperature T0 is greater than 340 °C. maxThe temperature is greater than 365 °C; furthermore, the initial contact angle of the surface of kapok-based microcrystalline cellulose with aqueous electrolyte is 45-50°. Based on the microscopic rod-like structure of kapok-based microcrystalline cellulose with the aforementioned specific pore characteristics, it possesses excellent thermal stability, high specific surface area, and film-forming and mechanical reinforcing properties. This expands the application of natural kapok fiber in high-performance composite materials. Furthermore, the combination of green ethanol pretreatment and efficient acid-base hydrolysis provides a new method for developing high-purity non-wood biomass microcrystalline cellulose. Therefore, the prepared kapok-based microcrystalline cellulose can be used as a high-performance green polymer functional filler or skeleton reinforcing agent, particularly in polymer composites and reinforcing materials, battery separators, biomedicine, and textiles.
[0022] The following detailed description of the kapok-based microcrystalline cellulose, its preparation method, and its application are provided through specific embodiments and comparative examples.
[0023] Example 1: The preparation method of kapok-based microcrystalline cellulose in this embodiment is as follows: (1) Disperse 1 part by mass of natural kapok fiber in 100 parts by mass of anhydrous ethanol, react at 70°C for 30 min, and after the reaction is completed, cool to room temperature, wash and dry to obtain pretreated kapok fiber; (2) Disperse 1 part by mass of pretreated kapok cellulose in 50 parts by mass of sodium hydroxide aqueous solution (concentration of 2.5M), and react in a water bath at 100℃ for 4 hours under magnetic stirring. After the reaction is completed, cool to room temperature, wash, and freeze dry at -50℃ and vacuum degree below 15 Pa for 48 hours to obtain kapok cellulose. (3) Add 1 part by mass of kapok cellulose to 25 parts by mass of hydrochloric acid aqueous solution (1.8 wt%), place in a reaction vessel, react at 75°C for 80 min, after the reaction is completed, cool to room temperature, centrifuge, wash, freeze dry at -50°C and vacuum degree below 15 Pa for 48 h to obtain kapok-based microcrystalline cellulose, denoted as K-MCC.
[0024] The following tests and characterizations were performed on the kapok-based microcrystalline cellulose K-MCC of this embodiment: like Figure 1 As shown, the kapok-based microcrystalline cellulose treated with sodium hydroxide and hydrochloric acid is rod-shaped; like Figure 2 As shown, natural kapok fiber has a thickness of 1700~1750cm. -1A distinct C=O absorption peak appears nearby, which is mainly attributed to the vibration of oxygen-containing groups in substances such as hemicellulose and pectin. However, the C=O absorption peak almost completely disappears in the infrared spectrum of kapok-based microcrystalline cellulose (K-MCC). Meanwhile, a distinct CO absorption peak appears near 1250 cm⁻¹ (dashed line position) in natural kapok fiber, which mainly originates from the aryl ether bond in the lignin structure. In the K-MCC spectrum, this CO absorption peak is also significantly weakened or disappears. This indicates that the preparation process in this embodiment can efficiently remove plant waxes, hemicellulose, and lignin, obtaining microcrystalline cellulose with extremely high purity. like Figure 3 As shown, X-ray powder diffraction comparison indicates that compared with natural kapok fiber, kapok-based microcrystalline cellulose (K-MCC) has significantly improved crystallinity. The intensity of its main diffraction peak on the 002 crystal plane is significantly enhanced and the peak shape is sharper. This is because during the ethanol pretreatment, alkali boiling, and dilute hydrochloric acid hydrolysis, a large amount of amorphous hemicellulose, lignin, and non-crystalline regions of cellulose in natural kapok fiber are hydrolyzed and removed, resulting in a significant increase in the proportion of the remaining regularly arranged crystalline regions. On the other hand, the spectrum shows that K-MCC still has absorption peaks at approximately 16° (110), 22° (002), and 34° (004) at 2θ. Compared with the original natural kapok sample, the diffraction peak intensity of K-MCC is significantly increased, and the half-peak width is narrowed. This indicates that the chemical treatment removes the amorphous regions and significantly improves the crystallinity of the material. This highly crystalline rigid skeleton is the structural basis for K-MCC to play an excellent mechanical support and anti-swelling role in composite materials and membranes.
[0025] Comparative Example 1: The preparation process of the wood pulp-based microcrystalline cellulose (W-MCC) in this comparative example is as follows: (1) Add 25 parts of hydrochloric acid aqueous solution (1.8 wt%) to 1 part by mass of wood pulp, place it in a reaction vessel, react at 75 ℃ for 80 min, after the reaction is completed, cool to room temperature, centrifuge, wash, freeze dry at -50 ℃ and vacuum degree less than 15 Pa for 48 h to obtain the finished product.
[0026] Comparative Example 2: The preparation process of the straw-based microcrystalline cellulose (S-MCC) in this comparative example is as follows: (1) Disperse 1 part by mass of natural straw fiber in 100 parts by mass of anhydrous ethanol solution, react at 65-70℃ for 30 min, and after the reaction is completed, cool to room temperature, wash and dry to obtain pretreated straw fiber.
[0027] (2) Disperse 1 part by mass of pretreated straw cellulose in 50 parts by mass of sodium hydroxide solution (concentration of 2.5M), react in a water bath at 100℃ for 4 hours under magnetic stirring, and after the reaction is completed, cool to room temperature, wash, freeze dry at -50℃ and vacuum degree below 15 Pa for 48 hours to obtain secondary pretreated straw fiber. (3) 1 part by mass of secondary pretreated straw fiber was added to 25 parts by mass of hydrochloric acid aqueous solution (1.8 wt%), placed in a reaction vessel, reacted at 75 ℃ for 80 min, and after the reaction was completed, cooled to room temperature, centrifuged, washed, and freeze-dried at a freezing temperature of -50 ℃ and a vacuum degree of less than 15 Pa for 48 h to obtain the finished product.
[0028] Thermogravimetric analysis (TGA) was used to evaluate the thermal stability of the products. The results were obtained by comparing Example 1 (K-MCC, kapok-based), Comparative Example 1 (W-MCC, wood pulp-based), and Comparative Example 2 (S-MCC, straw-based). max A comprehensive comparison of (maximum thermal degradation rate temperature) and carbon residue, such as Figure 4 As shown: Example 1 is more effective, T max The thermal degradation temperature increased significantly from 335.0℃ in Comparative Example 2 and 355.0℃ in Comparative Example 1 to 368.0℃ in Example 1; secondly, the initial thermal degradation temperature T0 was as high as 345.0℃ in Example 1, while it was 320.0℃ in Comparative Example 1 and only 300.0℃ in Comparative Example 2; regarding the carbon residue at 600℃, Comparative Example 2 had approximately 15%, Example 1 had approximately 11%, and Comparative Example 1 had the lowest carbon residue at 600℃, approximately 8%; the purpose of comparing microcrystalline cellulose materials from different biomass sources was to verify the influence of the microstructure of different natural raw materials on the thermal stability of the final product. Figure 4 As can be seen, thanks to the unique ultrathin cell wall of kapok and its highly crystalline rigid skeleton reconstructed after de-impregnation and hydrolysis, the thermal degradation resistance of Example 1 is optimal. Therefore, the kapok-based microcrystalline cellulose of Example 1 achieves the optimal thermal safety margin when facing harsh working environments such as aqueous battery separators.
[0029] The specific surface area and pore size of the products were evaluated using a BELSORP-max (MicrotracBEL) surface area and pore size analyzer. A comprehensive comparison of nitrogen adsorption / desorption capacity and pore size distribution was conducted using Example 1 (kapok-based, K-MCC), Comparative Example 1 (wood pulp-based, W-MCC), and Comparative Example 2 (straw-based, S-MCC). Figure 5As shown: Comparative Example 2 exhibits a larger absolute pore volume, with a maximum nitrogen adsorption capacity of approximately 3.3 cm³ / g. It also shows the highest peak pore size distribution (dV / dD) at 2–3 nm, approximately 0.0042 cm³ / g / nm. Example 1 is second, with a maximum nitrogen adsorption capacity of approximately 3.0 cm³ / g. Comparative Example 1 shows the worst nitrogen adsorption capacity (below 0.5 cm³ / g in most relative pressure ranges, indicating severe pore structure collapse). Example 1 shows a peak pore size distribution at 2–3 nm of approximately 0.003 cm³ / g / nm, while Comparative Example 1's peak is only approximately 0.0014 cm³ / g / nm. The comparison of microcrystalline cellulose materials from different natural biomass sources aims to verify whether different precursors can retain and reconstruct an ideal three-dimensional mesoporous network and achieve optimal membrane application performance after undergoing de-impurification hydrolysis. Figure 5 As can be seen, the pores of Comparative Example 1 were damaged, while the pores of Comparative Example 2 were extremely developed, but the excessive pore volume would lead to excessive swelling after liquid absorption. The mesoporous network of Example 1 was concentrated in 2~10nm and had a moderate pore volume, which made the wetting dynamics and skeleton rigidity optimal. Therefore, Example 1 (kapok-based microcrystalline cellulose) achieved a relatively balanced optimal state between "ultra-high hydrophilicity and liquid retention" and "anti-swelling structural stability".
[0030] like Figure 6 As shown, kapok-based microcrystalline cellulose K-MCC exhibits a more moderate interfacial tension when in contact with aqueous electrolytes, effectively balancing rapid wetting of the electrolyte with the anti-swelling properties of the physical framework. This avoids structural collapse caused by excessive hydrophilicity, as seen in commercial wood pulp microcrystalline cellulose, thus achieving excellent membrane stabilization.
[0031] like Figure 7 As shown, five core physical and interfacial dimensions that determine the service performance of aqueous battery separators are extracted to more intuitively demonstrate the adaptability of this invention for battery separator applications. Existing technologies, in developing novel biomass battery separators, often fall into the trap of pursuing extreme values for a single indicator, such as achieving extremely high porosity or superhydrophilic surfaces through drastic modification. However, such one-dimensional breakthroughs often come at the cost of sacrificing the structural strength and wet dimensional stability of the material, leading to swelling and collapse of the separator during long-term service, thus failing to meet the requirements of aqueous battery separators. This invention does not blindly pursue extreme values for a single physicochemical parameter, but rather, based on the systemic requirements of the separator under complex electrochemical environments, exhibits excellent application adaptability.
[0032] In summary, the preparation method of this invention can produce kapok-based microcrystalline cellulose with excellent thermal stability and abundant mesoporous structure. The preparation process is simple, environmentally friendly, and low in cost, and has broad application prospects in composite materials, pharmaceutical excipients, food packaging, textiles and other fields.
[0033] Given that there are numerous embodiments of the present invention, and the raw materials and quantities involved can be selected within a limited range according to actual needs, and that the experimental data for each embodiment are extensive and numerous, it is not suitable to list and describe them one by one here. However, the content to be verified and the final conclusions obtained in each embodiment are similar. Therefore, the verification content of each embodiment will not be described one by one here.
[0034] It should be noted that the above embodiments can be freely combined as needed. The above description is only a detailed explanation of the preferred embodiments and principles of the present invention. For those skilled in the art, there will be changes in the specific implementation methods based on the ideas provided by the present invention, and these changes should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing kapok-based microcrystalline cellulose, characterized in that, Includes the following steps: (1) Disperse natural kapok fibers in anhydrous ethanol, pretreat them by heating in a water bath at 65-70℃ for 20-40 minutes, then cool, wash and dry to obtain pretreated kapok fibers; (2) Disperse the pretreated kapok fiber in an aqueous sodium hydroxide solution and react at 80-100℃ for 4-6 hours. Then cool, wash, and freeze dry at a freezing temperature of -80 to -50℃ and a vacuum degree of less than 15 Pa for 24-48 hours to obtain kapok cellulose. (3) Disperse kapok cellulose in hydrochloric acid solution and react at 70-85℃ for 70-90 min. Then cool, wash, and freeze dry at freezing temperature of -80 to -50℃ and vacuum degree of less than 15 Pa for 24-48 h to obtain kapok-based microcrystalline cellulose.
2. The preparation method according to claim 1, characterized in that, In step (1), the mass ratio of natural kapok fiber to anhydrous ethanol is 1:(90-110).
3. The preparation method according to claim 1, characterized in that, In step (2), the mass ratio of pretreated kapok fiber to sodium hydroxide aqueous solution is 1:(40-60), and the concentration of sodium hydroxide aqueous solution is 2.5-3.0M.
4. The preparation method according to claim 1, characterized in that, In step (3), the mass ratio of kapok cellulose to hydrochloric acid aqueous solution is 1:(20-30), and the mass percentage of hydrochloric acid aqueous solution is 1.2-1.8%.
5. Kapok-based microcrystalline cellulose prepared by the preparation method according to any one of claims 1-4.
6. The kapok-based microcrystalline cellulose according to claim 5, characterized in that, The obtained kapok-based microcrystalline cellulose has a hierarchical porous structure. The pore size distribution based on nitrogen adsorption-desorption test is concentrated between 2-10 nm, and the peak pore size is between 2-4 nm.
7. The kapok-based microcrystalline cellulose according to claim 5, characterized in that, The initial contact angle of the surface of the kapok-based microcrystalline cellulose with the aqueous electrolyte is 45-50°.
8. The kapok-based microcrystalline cellulose according to claim 5, characterized in that, The initial thermal degradation temperature T0 of the kapok-based microcrystalline cellulose is greater than 340 °C, and the maximum thermal degradation rate temperature T0 is greater than 340 °C. max Greater than 365 ℃.
9. The application of kapok-based microcrystalline cellulose as described in any one of claims 5-8, characterized in that, Used to prepare separators for aqueous batteries.
Citation Information
Patent Citations
Manufacture of Microcrystalline Cellulose
CN102947343B
Preparation method for nano-microcrystalline cellulose
CN104293858A