Negative electrode binder, negative electrode sheet and secondary battery

By combining a quaternary graft copolymer negative electrode binder with a dynamic crosslinking agent, a multi-layer dynamic crosslinking network is formed, which solves the shortcomings of existing negative electrode binders in terms of strength, buffering capacity and interfacial compatibility, and improves the electrode structure stability and performance of the battery.

CN123107589APending Publication Date: 2026-11-17SHENZHEN HAODYNE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611240999.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing negative electrode binders are insufficient in balancing high bonding strength, dynamic buffering capacity, interfacial compatibility, and electrolyte resistance, and have poor adaptability to coating processes, resulting in poor battery performance.

Method used

The quaternary graft copolymer negative electrode binder contains lignin sulfonate structural units, disulfide bond structural units, acrylic structural units, and polycarboxylic acid structural units. Combined with a dynamic crosslinking agent, it forms a multi-layer dynamic crosslinking network, which enhances the cohesive strength, self-healing ability, and interfacial compatibility of the binder.

Benefits of technology

It improves the battery's long-cycle stability, cycle life, and rate performance, reduces the electrode defect rate, and enhances coating yield and electrode structure integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This application discloses a negative electrode binder, a negative electrode sheet, and a secondary battery. The negative electrode binder comprises a copolymer and a dynamic crosslinking agent. The copolymer includes lignin sulfonate structural units and disulfide bond-containing structural units, acrylic structural units, and polycarboxylic acid structural units. The dynamic crosslinking agent includes catechol groups and borate ester groups. The negative electrode binder of this application combines high adhesive strength, excellent dynamic buffering capacity, good interfacial compatibility, and electrolyte resistance. It is also suitable for aqueous coating processes, especially for hard carbon negative electrodes in sodium-ion batteries, effectively buffering the deformation during the sodium intercalation / deintercalation process of hard carbon, improving long-cycle stability and battery cycle life and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of battery materials technology, specifically relating to a negative electrode binder, a negative electrode sheet, and a secondary battery. Background Technology

[0002] As a key component of secondary batteries, binders play a crucial role in bonding active materials, conductive agents, and current collectors, maintaining the integrity of the electrode structure, and directly affecting the battery's cycle life, rate performance, and safety performance. Currently, commercially available negative electrode binders still face several bottlenecks: Traditional oil-based binders, such as polyvinylidene fluoride (PVDF), require the use of toxic N-methylpyrrolidone (NMP) solvents, resulting in high costs, poor environmental performance, limited adhesive strength, insufficient resistance to electrolyte swelling, and easy shedding of active materials during cycling. Mainstream water-based binders, such as carboxymethyl cellulose / styrene-butadiene rubber (CMC / SBR) systems, while environmentally friendly and low-cost, suffer from poor intrinsic elasticity and insufficient cohesive strength, making it difficult to buffer volume changes during the sodium intercalation / deintercalation process of hard carbon; furthermore, their weak interfacial adhesion makes them prone to interfacial debonding and electrode pulverization during long cycles, leading to rapid capacity decay. Pure polyacrylic acid binders are brittle, have limited functional groups, low crosslinking site density, and lack dynamic elasticity, failing to continuously buffer electrode cyclic deformation; moreover, polyacrylic acid binders rely solely on molecular entanglement and a small number of hydrogen bonds to maintain their structure, exhibiting poor resistance to electrolyte swelling and easy relaxation and failure at high temperatures. Existing modified bio-based binders (such as lignin and starch-based binders) generally suffer from low mechanical strength, poor electrolyte resistance, and limited functionality. Many self-healing adhesives that introduce dynamic bonds adopt a single dynamic cross-linking system, which has an inherent contradiction between the coupling of cohesive strength and interfacial adhesion performance and the difficulty in improving them simultaneously. It cannot achieve both high bonding strength and dynamic buffering performance.

[0003] In terms of performance control, existing binders generally suffer from strong performance coupling issues, such as mutual constraints between cohesive strength, interfacial adhesion, slurry stability, and swelling resistance. Regarding process adaptability, the excessively rapid evaporation rate during aqueous coating processes can easily lead to poor slurry stability, electrode cracking, and agglomeration defects. Existing binders lack optimization for adaptability to coating processes.

[0004] Existing binder modifications have failed to simultaneously address multiple functions, including self-healing, volume buffering, slurry water retention, and compatibility with coating processes. Therefore, developing a bio-based anode binder that combines high adhesive strength, excellent dynamic buffering capacity, good interfacial compatibility, and electrolyte resistance, while also being compatible with aqueous coating processes, is a key requirement for improving the overall performance of batteries. Summary of the Invention

[0005] In order to overcome the defects of existing negative electrode binders in secondary batteries, this application provides a negative electrode binder, a negative electrode sheet, and a secondary battery.

[0006] The purpose of this application is to achieve the following technical solution.

[0007] In a first aspect, this application provides a negative electrode binder comprising a copolymer and a dynamic crosslinking agent, wherein the copolymer comprises lignin sulfonate structural units and disulfide bond-containing structural units, acrylic structural units and polycarboxylic acid structural units; and the dynamic crosslinking agent comprises catechol groups and borate ester groups.

[0008] Furthermore, the mass ratio of the copolymer to the dynamic crosslinking agent is 100:(5~20).

[0009] Furthermore, the mass ratio of lignin sulfonate structural units to acrylic structural units, polycarboxylic acid structural units and disulfide bond-containing structural units in the copolymer is 1:(0.4~1.0):(0.2~0.6):(0.3~1.0); and / or, the disulfide bond-containing structural units are graft copolymerized onto the lignin sulfonate structural units, and the grafting rate of the copolymer is 52%~68%.

[0010] Furthermore, the lignin sulfonate structural unit includes at least one of sodium lignin sulfonate structural unit, calcium lignin sulfonate structural unit, enzymatically hydrolyzed lignin sulfonate structural unit, and magnesium lignin sulfonate structural unit.

[0011] Furthermore, the disulfide-containing structural unit includes at least one of the following: thioctic acid structural unit, thiocamide structural unit, cystine diacrylate structural unit, 2,2'-dithiobisbenzimidazole diacrylate structural unit, diphenyl disulfide diacrylate structural unit, and 1,3-adamantane dithiol diacrylate structural unit.

[0012] Furthermore, the disulfide-containing structural unit includes a flexible structural unit containing disulfide bonds; and / or, the disulfide-containing structural unit includes a thioctic acid structural unit or a thiocamide structural unit.

[0013] Furthermore, the acrylic structural unit includes at least one of acrylic acid structural unit and methacrylic acid structural unit; and / or, the polycarboxylic acid structural unit includes at least one of itaconic acid structural unit, citraconic acid structural unit, mesocarboxylic acid structural unit, and fumaric acid structural unit.

[0014] Furthermore, the dynamic crosslinking agent includes at least one of borate ester-functionalized dopamine crosslinking agent, gallic acid-modified phenylboronic acid ester, L-DOPA-modified phenylboronic acid, and tannic acid-borate complex; and / or, the molar ratio of borate ester groups to catechol groups in the dynamic crosslinking agent is (1~3):(1~3).

[0015] Secondly, this application provides a negative electrode sheet, including a current collector and a coating on the surface of the current collector, the coating including a negative electrode active material, a conductive agent and a negative electrode binder as described in the first aspect.

[0016] Thirdly, this application provides a secondary battery, including the negative electrode sheet as described in the second aspect.

[0017] Compared with the prior art, this application has the following advantages: The quaternary graft copolymer of this application constructs a molecular structure combining a lignin sulfonate backbone with mono- and poly-carboxyl composite polar adhesive side chains and dynamic polydisulfide side chains. This structure, combined with a dynamic crosslinking agent containing catechol and borate ester groups, creates multiple synergistic effects and forms a dual dynamic crosslinking network. The negative electrode binder of this application possesses high adhesive strength and cohesive strength, excellent dynamic self-healing and volume buffering, good interfacial compatibility and resistance to electrolyte swelling, and good compatibility with coating processes.

[0018] The matrix structure of the quaternary graft copolymer can simultaneously improve thermodynamic stability, mechanical strength, and water compatibility. At the same time, the synergistic effect of the triple hydrophilic groups of sulfonic acid group, monocarboxyl group, and polycarboxyl group significantly improves the water dispersibility and dissolution rate of the binder, resulting in a significant improvement in the stability of the negative electrode slurry and the coating yield.

[0019] The high-density cross-linking sites of the polycarboxylic acid group form a highly dense and uniform cross-linking network by multi-point complexation and hydrogen bonding with the hydroxyl groups of the borate ester group and the catechol group. This effectively blocks the penetration of small molecules in the electrolyte and reduces the swelling rate in the electrolyte.

[0020] A triple dynamic crosslinking network consisting of dynamic covalent bonds of polydisulfide, dynamic complex bonds of borate esters, and multi-level hydrogen bonds of single / multi-carboxyl groups is constructed. Under external deformation, this network effectively dissipates mechanical energy through reversible breaking and recombination of dynamic bonds, and achieves autonomous reconstruction of dynamic bonds after stress removal, thereby endowing the electrode with room-temperature self-healing capability. This dynamic crosslinking system can well adapt to the reversible deformation of hard carbon anodes during sodium ion intercalation and deintercalation, maintaining the integrity of the electrode structure and interfacial stability, thus significantly improving the long-cycle stability, cycle life, and rate performance of the battery.

[0021] When the negative electrode binder of this application is applied to the negative electrode sheet, the obtained negative electrode sheet is basically free of cracks, pinholes and powder defects, the surface flatness and density are significantly improved, the electrode sheet defect rate is significantly reduced, and high-yield production can be achieved. Detailed Implementation

[0022] To make the technical problems, technical solutions, and beneficial effects solved by this application clearer, the following detailed description is provided in conjunction with specific embodiments. It should be understood that the embodiments described herein are only a part of the embodiments of this application, not all of them, and are merely used to explain this application and are not intended to limit it. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the protection scope of this application.

[0023] In a first aspect, this application provides a negative electrode binder comprising a copolymer and a dynamic crosslinking agent, wherein the copolymer comprises lignin sulfonate structural units and disulfide bond-containing structural units, acrylic structural units and polycarboxylic acid structural units; and the dynamic crosslinking agent comprises catechol groups and borate ester groups.

[0024] The negative electrode binder of this application is a quaternary graft copolymer, which has greater advantages. Using lignin sulfonate structural units as a rigid macromolecular backbone, acrylic structural units, polycarboxylic acid structural units, and disulfide bond-containing structural units are simultaneously covalently grafted onto the lignin sulfonate backbone through a controlled aqueous-phase free radical graft copolymerization reaction, forming a comb-shaped copolymer molecular structure. The lignin sulfonate structural units provide rigid backbone support and anchoring; the acrylic structural units provide monocarboxyl groups, endowing the binder with good water solubility, wettability, and interfacial adhesion; the polycarboxylic acid structural units increase the density of polar sites in the molecular chain, improving the density of the crosslinking network and interfacial adhesion; and the disulfide bond-containing structural units regulate dynamic elasticity, self-healing ability, and stress relaxation characteristics.

[0025] The negative electrode binder of this application employs a bifunctional dynamic crosslinking agent containing catechol groups and borate ester groups, possessing both dynamic crosslinking and interfacial adhesion functions. Specifically, the borate ester groups can undergo multi-point complexation reactions with the phenolic hydroxyl groups in lignin sulfonate structural units, the monocarboxyl groups in acrylic structural units, and the polycarboxyl groups in polycarboxylic acid structural units, forming a second dynamic crosslinking network that regulates cohesive strength and swelling resistance. The catechol groups are used to enhance the interfacial adhesion between the binder and the active material and current collector.

[0026] The negative electrode binder of this application constructs a triple synergistic crosslinking system consisting of dynamic covalent bonds of polydisulfide, dynamic complex bonds of borate ester / boron-oxygen bonds, and a high-density multi-level hydrogen bond network. The hydrogen bond network achieves micro-deformation buffering and repair under low stress through reversible fracture-reconstruction at room temperature. Single and multiple carboxyl groups form a hydrogen bond reinforcing network, enhancing intermolecular cohesion. Furthermore, carboxyl groups form hydrogen bonds and polar interactions with oxygen-containing functional groups on the surface of the negative electrode active material (such as hard carbon), increasing interfacial anchoring points and inhibiting interfacial debonding during cycling. The dynamic covalent bonds of polydisulfide achieve deformation buffering, stress dissipation, and self-repair functions under medium to high stress through dynamic exchange at room temperature. The dynamic complex bonds of borate ester / boron-oxygen bonds provide structural support at room temperature and can undergo reversible complexation exchange under high-temperature conditions, achieving adaptive structural adjustment.

[0027] This application utilizes the synergistic effect of three types of hydrophilic functional groups—lignin sulfonate structural units, acrylic structural units, and polycarboxylic acid structural units—to form a dense hydration protective film, endowing the negative electrode slurry with excellent water retention, dispersion stability, and resistance to environmental interference. The multipolar groups synergistically bind water molecules, slowing down the rate of water evaporation and preventing microcracks caused by uneven shrinkage of the adhesive layer during drying. This results in a electrode sheet with good surface smoothness and density, and a reduced defect rate. Simultaneously, it improves the electrostatic stability and steric hindrance stability of the colloid, inhibiting the agglomeration and sedimentation of negative electrode active materials (such as hard carbon), ensuring stable rheological properties of the negative electrode slurry during standing and coating processes, with controllable viscosity fluctuations.

[0028] In some embodiments, the mass ratio of the copolymer to the dynamic crosslinking agent is 100:(5~20); specifically, the mass ratio can be 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, 100:11, 100:13, 100:14, 100:17, or 100:20; preferably, the mass ratio is 100:(9~11). Within this mass ratio range, the crosslinked network is dense, exhibiting good cohesive strength and resistance to electrolyte swelling, while ensuring that the reversible exchange reaction of dynamic bonds is not inhibited, avoiding increased material brittleness due to excessive crosslinking, and contributing to long-term structural stability.

[0029] In some specific embodiments, the mass ratio of lignin sulfonate structural units to acrylic structural units, polycarboxylic acid structural units and disulfide bond-containing structural units in the copolymer is 1:(0.4~1.0):(0.2~0.6):(0.3~1.0).

[0030] Acrylic structural units provide hydrophilic wettability and interfacial adhesion sites; polycarboxylic acid structural units increase the density of crosslinking sites through multiple carboxyl groups, improving the density of the molecular network and synergistically enhancing cohesive strength with the polar groups of acrylic structural units; disulfide bond-containing structural units provide self-healing capabilities; the rigid framework of lignin sulfonate structural units maintains the overall topology of the copolymer. When the proportion of acrylic structural units is too high, the film becomes excessively hydrophilic, reducing its resistance to electrolyte swelling; when the proportion of acrylic structural units is too low, the hydration capacity and interfacial wettability of the slurry are insufficient. When the proportion of polycarboxylic acid structural units is too high, the crosslinking density is too large, increasing the material's brittleness and reducing its deformation buffering capacity; when the proportion of polycarboxylic acid structural units is too low, the dense reinforcing effect of the multiple carboxyl groups is weakened, limiting swelling resistance. When the proportion of disulfide bond-containing structural units is too low, the self-healing ability is insufficient; when the proportion of disulfide bond-containing structural units is too high, the system rigidity decreases, and the cohesive strength weakens.

[0031] In some embodiments, the disulfide-bonded structural units are grafted copolymerized onto lignin sulfonate structural units, and the grafting rate of the quaternary graft copolymer is 52% to 68%. The four structural units are covalently bonded to the same molecular chain, avoiding the problems of phase separation, small molecule migration, and structural instability found in traditional blend systems. By controlling the grafting rate, the composition and structural uniformity of the molecular chain segments can be adjusted, improving thermodynamic stability, mechanical strength, and compatibility with aqueous processing. The resulting product is uniformly dispersed, free of agglomeration and gel particles. Preferably, the grafting rate is 55% to 64%, within which the elongation at break and tensile strength can be further improved, and the electrolyte swelling rate can be reduced.

[0032] In some specific embodiments, the lignin sulfonate structural unit includes at least one of sodium lignin sulfonate structural units, calcium lignin sulfonate structural units, enzymatically hydrolyzed lignin sulfonate structural units, and magnesium lignin sulfonate structural units. Specifically, the lignin sulfonate structural unit is derived from lignin sulfonate, and the lignin sulfonate includes at least one of sodium lignin sulfonate, calcium lignin sulfonate, enzymatically hydrolyzed lignin sulfonate, and magnesium lignin sulfonate.

[0033] In this application, sodium lignosulfonate is preferred as a rigid macromolecular backbone. Its aromatic backbone provides high cohesive strength and structural support, while high-density sulfonic acid groups and hydroxyl groups construct a hydration and water-retaining layer and cross-linking reaction sites. This provides sufficient reaction anchoring points for the simultaneous graft copolymerization of the other three structural units, ensuring the aqueous compatibility and slurry coating stability of the quaternary graft copolymer. Calcium lignosulfonate has a lower raw material cost, reducing the overall system cost. Although its solubility is slightly lower, it can be adapted through process adjustments, making it suitable for large-scale industrial production. Enzymatic hydrolysis of lignosulfonates results in lower impurity content and more uniform molecular structure, leading to better uniformity and batch-to-batch stability of the generated quaternary graft copolymer, thus meeting the high consistency requirements of high-end energy storage batteries. Magnesium lignosulfonate has milder metal ion activity, causing less interference to the electrochemical system, making it suitable for high-voltage, long-cycle battery systems. Lignosulfonates exhibit excellent compatibility with quaternary copolymerization systems and are fully adaptable to aqueous free radical graft copolymerization processes, with only minor differences in rigidity, hydrophilicity, and impurity content, allowing for customized replacement as needed.

[0034] In some specific embodiments, the disulfide-containing structural unit includes at least one selected from lipoic acid, lipoamide, cystine diacrylate, 2,2'-dithiobisbenzimidazole diacrylate, diphenyl disulfide diacrylate, and 1,3-adamantane dithiol diacrylate. Specifically, the disulfide-containing structural unit is derived from a dynamic functional monomer, which includes at least one selected from lipoic acid, lipoamide, cystine diacrylate, 2,2'-dithiobisbenzimidazole diacrylate, diphenyl disulfide diacrylate, and 1,3-adamantane dithiol diacrylate.

[0035] Preferably, the disulfide-bonded structural unit comprises a flexible structural unit containing disulfide bonds. Specifically, the disulfide-bonded structural unit comprises at least one of thioctic acid structural units and thiocamide structural units. The flexible structural unit containing disulfide bonds is polymerized to form polydisulfide flexible segments, which possess both dynamic elasticity and self-healing capabilities.

[0036] In this application, natural α-lipoic acid is preferred as the dynamic functional monomer of the flexible structural unit containing disulfide bonds. The α-lipoic acid is simultaneously grafted and copolymerized with acrylic and polycarboxylic acid structural units onto the lignin framework, forming flexible side chains containing dynamic polydisulfide bonds through ring-opening polymerization. This constitutes the first dynamic crosslinking segment in the dynamic crosslinking system, endowing the binder with reversible deformation capability, stress dissipation characteristics, and self-healing function, adapting to the volume deformation of the hard carbon anode during sodium ion intercalation / deintercalation. Furthermore, the lipoamide side chain formed after ring-opening of α-lipoic acid contains amide bonds, providing additional hydrogen bonding and synergistically enhancing interfacial adhesion and cohesive strength with the carboxyl group. The dynamic functional monomer containing disulfide bonds can be replaced individually with other monomers containing disulfide bonds or used in combination as needed, all achieving dynamic crosslinking, deformation buffering, and self-healing functions, and exhibiting good copolymerization compatibility with the quaternary copolymer system.

[0037] In some specific embodiments, the acrylic structural unit includes at least one selected from acrylic acid structural units and methacrylic acid structural units. Specifically, the acrylic structural unit is derived from an acrylic monomer, which includes at least one selected from acrylic acid and methacrylic acid.

[0038] In some specific embodiments, the polycarboxylic acid structural unit includes at least one selected from itaconic acid, citraconic acid, mesocarboxylic acid, and fumaric acid. Specifically, the polycarboxylic acid structural unit is derived from an unsaturated polycarboxylic acid monomer, which includes at least one selected from itaconic acid, citraconic acid, mesocarboxylic acid, and fumaric acid. In this application, acrylic acid and itaconic acid are preferably combined. The synergistic effect of the two unsaturated polycarboxylic acid monomers gives the adhesive good adhesion, water retention, cross-linking density, and swelling resistance.

[0039] In some specific embodiments, the dynamic crosslinking agent includes at least one of borate ester-functionalized dopamine crosslinking agents, gallic acid-modified phenylboronic acid esters, L-DOPA-modified phenylboronic acid, and tannic acid-borate complexes.

[0040] In some specific embodiments, the molar ratio of borate ester groups to catechol groups in the dynamic crosslinking agent is (1~3):(1~3). Preferably, the molar ratio of borate ester groups to catechol groups in the dynamic crosslinking agent is 1:1. The equimolar matching of borate ester crosslinking sites and catechol adhesion sites maximizes the bidirectional efficiency of crosslinking enhancement and interfacial adhesion enhancement of the adhesive.

[0041] For different preparation scenarios with varying performance focuses, bifunctional dynamic crosslinking agents such as borate-functionalized dopamine, gallic acid-modified phenylboronic acid esters, L-DOPA-modified phenylboronic acid, and tannic acid-borate complexes can be selected. This application preferably uses borate-functionalized dopamine, where the molar ratio of catechol groups to borate groups is 1:1, maximizing both crosslinking enhancement and interfacial adhesion strengthening of the binder.

[0042] The negative electrode binder in this embodiment can be prepared using the following steps: 1) Synthesis of quaternary graft copolymers: Lignosulfonate was added to deionized water and stirred at 300-500 rpm until completely dissolved, preparing a lignosulfonate solution with a mass fraction of 8%-15%. Nitrogen gas was introduced to purge oxygen for 20-30 minutes. An initiator was added, with the total amount being 1%-3% of the total monomer mass. After stirring evenly, the solution was heated to 60-65℃ for activation for 5-10 minutes. The mass ratio of lignosulfonate, acrylic monomers, unsaturated polycarboxylic acid monomers, and dynamic functional monomers was 1:(0.4-1.0):(0.2-0.6): (0.3~1.0) A premixed monomer aqueous solution of acrylic acid monomer, unsaturated polycarboxylic acid monomer, and dynamic functional monomer was added dropwise at a uniform rate. The mass fraction of the premixed monomer was 20%~30%. The dropping time was controlled at 2~4h. The temperature was maintained at 60~65℃ throughout the dropping process under nitrogen atmosphere protection. After the dropping was completed, the mixture was cured at controlled temperature in stages: 60℃ for 1h, 70℃ for 2~3h, and 75℃ for 1~3h to complete the free radical graft copolymerization reaction. After the reaction was completed, the mixture was naturally cooled to room temperature, the pH of the system was adjusted to 7.0, and the mixture was dialyzed with deionized water. After dialyzed, the mixture was freeze-dried at -40~-50℃ for 24~48h to obtain the quaternary graft copolymer solid.

[0043] 2) Add the quaternary graft copolymer to deionized water and stir at 400-600 rpm until fully dispersed to prepare a copolymer aqueous solution with a mass fraction of 6%-16%; add dilute sodium hydroxide solution to adjust the pH to 7.5-8.5; add dynamic crosslinking agent at a mass ratio of 100:(5-20) of quaternary graft copolymer to dynamic crosslinking agent, stir evenly, raise the temperature to 40-60℃, and pre-crosslink at low speed for 0.5-2 hours; cool to room temperature, filter through a 100-200 mesh filter to obtain an aqueous dispersion of dual dynamic crosslinking bio-based negative electrode binder with a solid content of 5%-15%.

[0044] In the preparation step 1) above, the initiator is ammonium sulfate-sodium bisulfite, persulfate-ascorbic acid, hydrogen peroxide-ferrous salt, potassium persulfate, sodium persulfate, etc., which can achieve stable polymerization, high monomer conversion rate and low impurity residue.

[0045] In the preparation step 2) above, the dynamic crosslinking agent can be selected from borate-functionalized dopamine crosslinking agents, gallic acid-modified phenylboronic acid esters, L-DOPA-modified phenylboronic acid, or tannic acid-borate complexes, and can be synthesized by dopamine, gallic acid, L-DOPA, tannic acid and phenylboronic acid or their derivatives or borates.

[0046] For example, borate-functionalized dopamine crosslinking agents, gallic acid-modified phenylboronic acid esters, L-DOPA-modified phenylboronic acid, or tannic acid-borate complexes can be prepared by the following methods.

[0047] Synthesis method of borate ester functionalized dopamine crosslinking agent: It is prepared by conventional amidation route, and the raw materials are all commercially available conventional reagents. 4-Carboxyphenylboronic acid pinacol ester, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC·HCl), and N-hydroxysuccinimide (NHS) were dissolved in N,N-dimethylformamide (DMF solvent) at a molar ratio of 1:1.2:1.2 to prepare a 0.05~0.1 mol / L reaction solution. The solution was activated at 20~35℃ in the dark for 30~60 min. Dopamine hydrochloride at a molar ratio of 1:1 to 4-carboxyphenylboronic acid pinacol ester was then added to the reaction solution. The pH was adjusted to 7~8 with triethylamine, and the mixture was stirred at 20~35℃ in the dark for 12~24 h under nitrogen protection throughout the reaction. After the reaction was completed, DMF was removed by vacuum distillation, and the crude product was purified by silica gel column chromatography with petroleum ether and ethyl acetate in a volume ratio of (1~2):1. The product was then dried under vacuum to obtain a solid borate ester-functionalized dopamine crosslinking agent.

[0048] Synthesis of gallic acid-modified phenylboronic acid ester: A conventional amidation route was adopted, using commercially available reagents as raw materials. Gallic acid was dissolved in anhydrous N,N-dimethylformamide with EDC·HCl and NHS in a molar ratio of 1:1.2:1.2, and activated at room temperature in the dark for 30–60 min. Then, an equimolar amount of 4-aminophenylboronic acid pinacol ester was added, and triethylamine was added dropwise to adjust the pH to 7–8. The reaction was stirred at room temperature in the dark for 12–24 h. After the reaction, the solvent was removed by vacuum distillation, and the crude product was purified by silica gel column chromatography and dried under vacuum to obtain gallic acid-modified phenylboronic acid ester solid.

[0049] Synthesis method of L-DOPA modified phenylboronic acid: 4-Carboxyphenylboronic acid pinacol ester, EDC·HCl, and NHS were dissolved in anhydrous N,N-dimethylformamide in a molar ratio of 1:1.2:1.2 and activated at room temperature in the dark for 30-60 min; then an equimolar amount of L-DOPA hydrochloride was added, and triethylamine was added dropwise to adjust the pH of the system to 7-8. The reaction was stirred at room temperature in the dark for 12-24 h; after the reaction was completed, the solvent was removed by vacuum distillation, and the crude product was purified by silica gel column chromatography and vacuum dried to obtain solid L-DOPA modified phenylboronic acid.

[0050] Synthesis method of tannic acid-borate complex: Both raw materials (tannic acid and borax / boric acid) are bulk industrial-grade reagents; when using, they can be directly mixed in the system to form a dynamic complex system in situ; according to the mass ratio, tannic acid:borax = 1:0.65 or tannic acid:boric acid = 1:0.4.

[0051] Secondly, this application provides a negative electrode sheet, including a current collector and a coating on the surface of the current collector, the coating including a negative electrode active material, a conductive agent and a negative electrode binder as described in the first aspect.

[0052] In some specific embodiments, the negative electrode active material includes a hard carbon negative electrode active material, and the mass ratio of the hard carbon negative electrode active material, the conductive agent, and the negative electrode binder is (85~92):(3~8):(5~12). Specifically, this mass ratio can be 85:3:12, 85:8:7, 86:4:10, 86:7:7, 87:4:9, 87:8:5, 88:6:6, 89:3:8, 90:4:6, 91:3:6, or 92:3:5, etc.

[0053] The mass percentage of the negative electrode binder in the coating can be finely adjusted within the range of 5% to 12% depending on the type of negative electrode. A higher addition amount is used for high specific surface area hard carbon negative electrodes to ensure interfacial bonding and structural stability, while a lower addition amount is used for low expansion commercial hard carbon negative electrodes to improve electrode energy density. The stirring, pre-dispersion, and degassing parameters of the negative electrode slurry can adapt to the dispersion characteristics of different active materials. The coating thickness, gradient drying temperature, roller pressure, and compaction density of the negative electrode sheet can be flexibly controlled, comprehensively adapting to diverse production scenarios such as precision thin-layer coating, high-load thick electrode preparation, and flexible electrode processing.

[0054] The negative electrode binder of this application, with its strong wetting properties of multi-carboxyl groups, can uniformly coat hard carbon particles and conductive agents, constructing a continuous, dense, and highly elastic adhesive network. The binder dosage is moderate, satisfying the functional requirements of particle coating, interfacial bonding, and structural buffering, while avoiding excessive binder crowding of electrode pores and reducing sodium ion transport efficiency, thus maximizing the balance between electrode structural stability and energy density. The moderate binder dosage also results in lower electrode interfacial impedance, smoother ion transport, and reduced pulverization of active material during cycling, achieving a balance between high capacity, long cycling time, and high rate performance.

[0055] The negative electrode sheet of this application is prepared by first preparing a negative electrode slurry, coating the negative electrode slurry onto a current collector, drying it, and then cutting it by rolling.

[0056] More specifically, for example, hard carbon negative electrode sheets can be prepared according to the following steps.

[0057] 1) Preparation of negative electrode slurry: Mix hard carbon negative electrode active material, conductive agent, and negative electrode binder (solid part) of this application in a mass ratio of (85~92):(3~8):(5~12), add deionized water, and adjust the solid content of the negative electrode slurry to 40%~50%; first premix at low speed for 10 min, then disperse at high speed for 30~60 min, and degas under vacuum to obtain the negative electrode slurry; 2) Coating and drying: Coat the negative electrode slurry onto the 8~12μm copper foil current collector, and use gradient drying: dry at 55~60℃ for 1~3 min, dry at 75~80℃ for 2~4 min, and dry at 100~105℃ for 3~5 min. 3) Roller pressing and cutting: Roller pressing until the compacted density is 1.0~1.2 g / cm³ 3 After cutting, the material is vacuum dried at 115~125℃ for 10~14h to obtain a hard carbon negative electrode sheet.

[0058] Thirdly, this application provides a secondary battery, including the negative electrode sheet as described in the second aspect.

[0059] The positive electrode, separator, electrolyte, etc. of the secondary battery prepared according to conventional methods in the art are stacked in sequence, and then wound to obtain the cell. The cell is placed in an aluminum-plastic film, and the electrolyte is injected into the bare cell. After vacuum sealing, standing, formation, shaping and capacity testing, the secondary battery is obtained.

[0060] More specifically, a sodium-ion secondary battery is assembled using a hard carbon negative electrode sheet prepared with the binder of this application as the negative electrode, combined with a positive electrode, electrolyte, and separator. The positive electrode material is selected from any one of Prussian blue compounds, layered oxides, and polyanionic compounds; the electrolyte is selected from a 1.0 mol / L NaClO4 or NaPF6 EC / DEC / EMC (1:1:1) solution, and FEC film-forming additives may be added; the separator is selected from a glass fiber separator or a ceramic-coated polypropylene separator; the battery form can be a button cell, pouch cell, or cylindrical cell.

[0061] The specific implementation methods of this application will be further explained and illustrated below through examples and comparative examples.

[0062] Unless otherwise specified, all reagents, materials, and instruments used in the following description are conventional reagents, materials, and instruments, all of which are commercially available. The reagents involved can also be synthesized using conventional synthetic methods. Unless otherwise specified, the methods in the examples are conventional methods in the art.

[0063] Example 1 1) Preparation of negative electrode binder: Sodium lignosulfonate was added to deionized water and stirred at 400 rpm until completely dissolved to prepare a 10% sodium lignosulfonate solution. Nitrogen gas was then introduced to purge oxygen for 25 minutes. An ammonium persulfate-sodium bisulfite redox initiator was added to the solution, with the total initiator amounting to 2% of the total monomer mass. After stirring thoroughly, the solution was heated to 60°C and activated for 10 minutes. The mass ratio of sodium lignosulfonate to acrylic acid, itaconic acid, and α-lipoic acid was 1:0.7:0.4: An aqueous solution of premixed monomers of acrylic acid, itaconic acid, and α-lipoic acid was added dropwise at a constant rate of 0.6. The mass fraction of the premixed monomers in the aqueous solution was 25%. The addition time was controlled at 2.5 h, and the entire process was maintained at 60 °C under a nitrogen atmosphere. After the addition was completed, the mixture was aged in stages at controlled temperatures: 60 °C for 1 h, 70 °C for 2.5 h, and 75 °C for 2.5 h to complete the free radical graft copolymerization reaction. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, and the pH of the system was adjusted to 7.0. The mixture was then transferred to a dialysis bag with a molecular weight cutoff of 3000~5000 Da and dialyzed with deionized water for 4 days, with the water changed every 12 h. After dialysis, the mixture was freeze-dried at -45 °C for 32 h to obtain the quaternary graft copolymer solid.

[0064] 4-Carboxyphenylboronic acid pinacol ester was dissolved in DMF with EDC·HCl and NHS in a molar ratio of 1:1.2:1.2 to prepare a 0.08 mol / L reaction solution, which was activated at room temperature in the dark for 45 min. Then, dopamine hydrochloride with a molar ratio of 1:1 to 4-carboxyphenylboronic acid pinacol ester was added to the reaction solution, and the pH was adjusted to 7.5 with triethylamine. The reaction was carried out at room temperature in the dark with stirring for 20 h under nitrogen protection. After the reaction was completed, DMF was removed by vacuum distillation, and the crude product was purified by silica gel column chromatography with petroleum ether and ethyl acetate in a volume ratio of 2:1. The product was then dried under vacuum to obtain a solid borate ester-functionalized dopamine crosslinking agent.

[0065] The quaternary graft copolymer was added to deionized water and stirred at 500 rpm until fully dispersed to prepare a 10% (w / w) copolymer aqueous solution. The pH was adjusted to 7.5 by adding 0.1 mol / L sodium hydroxide solution. Boron ester functionalized dopamine crosslinking agent was added at a mass ratio of 100:10 between the quaternary graft copolymer and the dynamic crosslinking agent. After stirring evenly, the temperature was raised to 50°C and pre-crosslinked at low speed for 1 hour. After cooling to room temperature, the mixture was filtered through a 200-mesh filter to obtain an aqueous dispersion of negative electrode binder with a solid content of 10%.

[0066] 2) Preparation of the negative electrode sheet: The obtained aqueous dispersion of the negative electrode binder was mixed with hard carbon negative electrode active material and conductive carbon black at a mass ratio of 6:90:4. Deionized water was added to adjust the solid content of the negative electrode slurry to 45%. The mixture was premixed at low speed for 10 min, then dispersed at high speed for 45 min, and degassed under vacuum to obtain the negative electrode slurry. The negative electrode slurry was coated onto a 10 μm thick copper foil current collector and subjected to gradient drying: 60℃ for 2 min, 80℃ for 3 min, and 100℃ for 5 min. The mixture was then rolled to a compaction density of 1.3 g / cm³. 3 After cutting, the material is vacuum dried at 120℃ for 12 hours to obtain a hard carbon negative electrode sheet.

[0067] 3) Preparation of secondary batteries: The prepared hard carbon negative electrode sheet was used as the negative electrode, and assembled into a coin-type sodium-ion secondary battery with a positive electrode, electrolyte, and glass fiber separator. The positive electrode material was selected from Prussian blue compounds; the electrolyte was a 1.0 mol / L NaPF6 EC / DEC / EMC (1:1:1) solution with 5% FEC additive.

[0068] Example 2 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference between this embodiment and Embodiment 1 is that the mass ratio of the four monomers in the preparation of the negative electrode binder is different. Specifically, the mass ratio of sodium lignosulfonate to acrylic acid, itaconic acid, and α-lipoic acid is 1:0.5:0.2:0.6, while the rest is the same as in Embodiment 1.

[0069] Example 3 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference between this embodiment and Embodiment 1 is that the mass ratio of the four monomers in the preparation of the negative electrode binder is different. Specifically, the mass ratio of sodium lignosulfonate to acrylic acid, itaconic acid, and α-lipoic acid is 1:1:0.6:0.6, while the rest are the same as in Embodiment 1.

[0070] Example 4 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference between this embodiment and Embodiment 1 lies in the different four monomers and their mass ratios in the preparation of the negative electrode binder. Specifically, the lignin sulfonate is magnesium lignin sulfonate, the acrylic monomer is methacrylic acid, the dynamic functional monomer is thiocamide, and the mass ratio of magnesium lignin sulfonate to methacrylic acid, itaconic acid, and thiocamide is 1:0.8:0.5:1. All other aspects are the same as in Embodiment 1.

[0071] Example 5 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference between this embodiment and Embodiment 1 lies in the different four monomers and their mass ratios in the preparation of the negative electrode binder. Specifically, the lignin sulfonate is enzymatically hydrolyzed sodium lignin sulfonate, the acrylic monomer is methacrylic acid, the unsaturated polycarboxylic acid monomer is citralic acid, and the dynamic functional monomer is lipoamide. The mass ratio of enzymatically hydrolyzed sodium lignin sulfonate to methacrylic acid, citralic acid, and lipoamide is 1:0.4:0.3:0.3, and all other parameters are the same as in Embodiment 1.

[0072] Example 6 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main differences from Embodiment 1 are the different monomers used in the preparation of the negative electrode binder, the different amounts of dynamic crosslinking agent added, and the different amounts of negative electrode binder added to the negative electrode sheet. Specifically, the lignin sulfonate is calcium lignin sulfonate, the unsaturated polycarboxylic acid monomer is methyl succinic acid, and the mass ratio of calcium lignin sulfonate to acrylic acid, methyl succinic acid, and α-lipoic acid is 1:0.7:0.4:0.6; borate ester-functionalized dopamine crosslinking agent is added at a mass ratio of 100:11 between the quaternary graft copolymer and the dynamic crosslinking agent; the mass ratio of hard carbon negative electrode active material, conductive carbon black, and negative electrode binder (solids) is 89:4:7; the rest are the same as in Embodiment 1.

[0073] Example 7 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main differences from Embodiment 1 are the different monomers used in the preparation of the negative electrode binder, the different amounts of dynamic crosslinking agent added, and the different amounts of negative electrode binder added to the negative electrode sheet. Specifically, the unsaturated polycarboxylic acid monomer is fumaric acid; the mass ratio of sodium lignosulfonate to acrylic acid, fumaric acid, and α-lipoic acid is 1:0.7:0.4:0.6; a borate ester-functionalized dopamine crosslinking agent is added at a mass ratio of 100:9 between the quaternary graft copolymer and the dynamic crosslinking agent; the mass ratio of hard carbon negative electrode active material, conductive carbon black, and negative electrode binder (solids) is 88:4:8; the rest are the same as in Embodiment 1.

[0074] Example 8 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main differences from Embodiment 1 are the different monomers and dynamic crosslinking agents used in the preparation of the negative electrode binder, and the different amounts of negative electrode binder added to the negative electrode sheet. Specifically, the lignin sulfonate is magnesium lignin sulfonate, the acrylic monomer is methacrylic acid, the unsaturated polycarboxylic acid monomer is citralic acid, and the dynamic functional monomer is thioclamamide. The mass ratio of magnesium lignin sulfonate to methacrylic acid, citralic acid, and thioclamamide is 1:0.7:0.4:0.6; the dynamic crosslinking agent is gallic acid-modified phenylboronic acid ester; the mass ratio of hard carbon negative electrode active material, conductive carbon black, and negative electrode binder (solids) is 89:4:7; the rest are the same as in Embodiment 1.

[0075] The gallic acid-modified phenylboronic acid ester was synthesized using a conventional amidation route, with all raw materials being commercially available reagents. Gallic acid, EDC·HCl, and NHS were dissolved in anhydrous N,N-dimethylformamide at a molar ratio of 1:1.2:1.2 and activated at room temperature in the dark for 40 min. Subsequently, an equimolar amount of 4-aminophenylboronic acid pinacol ester was added, and triethylamine was added dropwise to adjust the pH of the system to 7.5. The reaction was stirred at room temperature in the dark for 15 h. After the reaction was completed, the solvent was removed by vacuum distillation, and the crude product was purified by silica gel column chromatography and dried under vacuum to obtain the gallic acid-modified phenylboronic acid ester solid.

[0076] Example 9 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main differences from Embodiment 1 are the dynamic crosslinking agent and its addition amount in the preparation of the negative electrode binder, and the amount of negative electrode binder added to the negative electrode sheet. Specifically, L-DOPA-modified phenylboronic acid is added at a mass ratio of 100:20 between the quaternary graft copolymer and the dynamic crosslinking agent; the mass ratio of hard carbon negative electrode active material, conductive carbon black, and negative electrode binder (solids) is 92:3:5; the rest are the same as in Embodiment 1.

[0077] The synthesis of L-DOPA-modified phenylboronic acid involved dissolving 4-carboxyphenylboronic acid pinacol ester with EDC·HCl and NHS in an anhydrous N,N-dimethylformamide at a molar ratio of 1:1.2:1.2 and activating at room temperature in the dark for 40 min. Subsequently, an equimolar amount of L-DOPA hydrochloride was added, and triethylamine was added dropwise to adjust the pH of the system to 7.5. The reaction was stirred at room temperature in the dark for 15 h. After the reaction was completed, the solvent was removed by vacuum distillation, and the crude product was purified by silica gel column chromatography and dried under vacuum to obtain solid L-DOPA-modified phenylboronic acid.

[0078] Example 10 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main differences from Embodiment 1 are the dynamic crosslinking agent and its addition amount in the preparation of the negative electrode binder, and the amount of negative electrode binder added to the negative electrode sheet. Specifically, a tannic acid-borate complex is added in a mass ratio of 100:5 of quaternary graft copolymer to dynamic crosslinking agent; the mass ratio of hard carbon negative electrode active material, conductive carbon black, and negative electrode binder (solids) is 85:3:12; the rest are the same as in Embodiment 1.

[0079] The tannic acid-borate complex is prepared by mixing tannic acid and boric acid at a mass ratio of 1:0.4.

[0080] Example 11 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference from Embodiment 1 is that the mass ratio of the four monomers in the preparation of the negative electrode binder is not disclosed. Specifically, the mass ratio of sodium lignosulfonate to acrylic acid, itaconic acid, and α-lipoic acid is 1:0.3:0.1:0.2; all other parameters are the same as in Embodiment 1.

[0081] Example 12 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference from Embodiment 1 is that the mass ratio of the four monomers in the preparation of the negative electrode binder is not disclosed. Specifically, the mass ratio of sodium lignosulfonate to acrylic acid, itaconic acid, and α-lipoic acid is 1:1.1:0.7:1.1; all other parameters are the same as in Embodiment 1.

[0082] Example 13 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference between this embodiment and Embodiment 1 is the amount of negative electrode binder added to the negative electrode sheet. Specifically, the mass ratio of hard carbon negative electrode active material, conductive carbon black, and negative electrode binder (solid content) is 94:3:3; all other aspects are the same as in Embodiment 1.

[0083] Example 14 This embodiment provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference between this embodiment and Embodiment 1 is the amount of negative electrode binder added to the negative electrode sheet. Specifically, the mass ratio of hard carbon negative electrode active material, conductive carbon black, and negative electrode binder (solid content) is 82:3:15; all other aspects are the same as in Embodiment 1.

[0084] Example 15 This comparative example provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The main difference from Example 1 is that the quaternary graft copolymer used in the preparation of the negative electrode binder contains disulfide bonds but is not flexible. Specifically, the dynamic functional monomer is cystine diacrylate; all other aspects are the same as in Example 1.

[0085] Comparative Example 1 In this comparative example, the copolymer in the negative electrode binder is a ternary grafting system that does not contain polycarboxylic acid structural units. Specifically, the negative electrode binder is prepared using most of the steps in Example 1. Itaconic acid is not present in the premixed monomers, and the mass ratio of sodium lignosulfonate to acrylic acid and α-lipoic acid is 1:0.7:0.6. The rest is the same as in Example 1.

[0086] Comparative Example 2 In this comparative example, the copolymer in the negative electrode binder is a ternary grafting system without disulfide bond structural units. Specifically, the negative electrode binder is prepared using most of the steps in Example 1. The premixed monomer does not contain disulfide bond monomers, and the mass ratio of sodium lignosulfonate to acrylic acid and itaconic acid is 1:0.7:0.4. The rest is the same as in Example 1.

[0087] Comparative Example 3 This comparative example uses a physical blending system for the negative electrode binder. Specifically, sodium lignosulfonate, polyacrylic acid, polyitanconic acid, and sodium thiooctanoate are physically mixed in a mass ratio of 1:0.7:0.4:0.6, without pre-graft copolymerization or dynamic crosslinking agents such as borate ester functionalized dopamine. The preparation of the negative electrode sheet and the secondary battery is the same as in Example 1.

[0088] Comparative Example 4 In this comparative example, the negative electrode binder was a commercially available CMC mixed with SBR at a mass ratio of 1:1; the preparation of the negative electrode sheet and the secondary battery was the same as in Example 1.

[0089] Comparative Example 5 This comparative example provides a negative electrode binder, a negative electrode sheet containing the negative electrode binder, and a secondary battery. The difference from Example 1 is that the dynamic crosslinking agent in the negative electrode binder does not contain catechol groups. Specifically, the dynamic crosslinking agent is borax; all other aspects are the same as in Example 1.

[0090] Performance testing: To better understand this application, the negative electrode binder, negative electrode sheet and secondary battery in the above embodiments and comparative examples were characterized or tested as follows.

[0091] 1. Performance of negative electrode binder [Grafting Rate] The grafting rate of the copolymer in the negative electrode binder was determined by Soxhlet extraction and weighing method. The mass W0 of the dried crude product sample was accurately weighed; acetone / deionized water mixed solvent was used as the extraction medium, and Soxhlet extraction was performed continuously for 48 h to fully elute the free monomers and homopolymers that did not participate in the grafting reaction; the remaining solid product was vacuum dried to constant weight and weighed to obtain W1; a blank control group was set up, and pure lignin sulfonate was extracted under the same conditions, and the mass loss due to lignin dissolution was corrected; the grafting rate G (%) was calculated according to the formula: G = [(W1 - corrected lignin mass) / total mass of grafting monomers] × 100%. The test results are shown in Table 1.

[0092] [Elongation at break and tensile strength] The aqueous dispersion of the negative electrode binder in the above examples and comparative examples was first defoamed, poured into a rectangular groove mold, air-dried naturally for 24 hours, and then dried at 100℃ for 12 hours. Square films (samples) of 20mm × 20mm were then cut and subjected to tensile testing at a tensile rate of 50.00mm / min using a tensile testing machine to test the elongation at break and tensile strength of the negative electrode binder. The test results are shown in Table 1.

[0093] Apply tensile force until the sample breaks, record the length change before and after the sample breaks, and calculate the elongation at break = (gauge length after break - original gauge length) / original gauge length × 100%.

[0094] Apply tensile force until the sample breaks, record the maximum tensile force at the point of breakage, and calculate the tensile strength by combining the sample's original cross-sectional area: maximum tensile force at break / original cross-sectional area.

[0095] [Swelling Rate] The aqueous dispersion of the negative electrode binder was poured into a horizontally placed polytetrafluoroethylene mold, dried at 60℃ under normal pressure to form a film, and then vacuum dried at 100℃ for 12 hours to completely remove residual solvent and moisture. A 20mm × 20mm square film was cut as a sample, and three parallel samples were prepared for each group. The initial dry mass m0 of each sample was weighed using a 0.01% analytical balance, and the average value was recorded. The sample was completely immersed in a 1.0mol / L NaPF6 / EC:DEC:EMC=1:1:1 (volume ratio) carbonate electrolyte solution, sealed in a sealed container, and placed in a constant temperature environment at 25℃ in the dark for 7 days. The sample was removed, and the free electrolyte on the surface was quickly and gently absorbed with qualitative filter paper. The mass m1 after swelling was immediately weighed. The swelling rate was calculated using the formula SR=[(m1-m0) / m0]×100%, and the arithmetic mean of the three parallel samples was taken as the final result. The test results are shown in Table 1.

[0096] Table 1 As shown in Table 1, the negative electrode binder of this application has both high elongation at break and tensile strength and low electrolyte swelling rate, which can effectively withstand the stress generated by the volume change of the hard carbon negative electrode, avoid the binder itself from cracking, and maintain the integrity of the electrode structure.

[0097] Comparing Example 1 with Examples 11 and 12, it can be seen that when the mass ratio of copolymer to dynamic crosslinking agent is within the range disclosed in this application, the grafting rate of the quaternary graft copolymer is stably maintained at 52%~68%. If the proportion of acrylic structural units is too high, the stability of the film against electrolyte will decrease. If the proportion of polycarboxylic acid structural units is too high, the crosslinking density will be greatly increased, the adhesive will become brittle, and the deformation buffering capacity will decrease. If the proportion is too low, the core advantages of polycarboxylic acid dense reinforcement and swelling reduction cannot be exerted. If the proportion of disulfide bond structural units is too low, the dynamic self-healing ability will be insufficient. If the proportion is too high, the rigidity of the system will decrease and the cohesive strength will be weakened.

[0098] The mechanical properties and electrolyte swelling resistance of the negative electrode binder in this application are enhanced. A comparison of Example 1 with Examples 5, 9, and 10 shows that when the grafting rate and the mass ratio of the copolymer to the dynamic crosslinking agent are within the preferred ranges of this application, the elongation at break and / or tensile strength can be further improved.

[0099] Comparing Example 1 with Example 15, it can be seen that the elongation at break of the binder can be further improved because of the formation of polydisulfide flexible segments in the copolymer. When it contains disulfide bonds and is a flexible structural unit, it can simultaneously take into account tensile strength and elongation at break.

[0100] Comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the lignin-acrylic acid-lipoic acid ternary grafting system (Comparative Example 1) relies solely on the carboxyl group of single acrylic acid to participate in the borate ester complexation, resulting in a limited number of crosslinking sites and network porosity defects. In contrast, the negative electrode binder of this application, due to the high-density carboxyl groups with both single and multiple carboxyl groups forming a hydrogen bond-reinforcing network, further strengthens the molecular cohesion, significantly improving tensile strength. Moreover, relying on the high-density crosslinking sites of multiple carboxyl groups, the negative electrode binder of this application exhibits a significantly lower electrolyte swelling rate compared to the ternary grafting system. The lignin-acrylic acid-itaconic acid ternary grafting system (Comparative Example 2) lacks polydisulfide segments, resulting in a significantly reduced elongation at break and insufficient dynamic elasticity. In contrast, the negative electrode binder of this application can simultaneously maintain a high elongation at break, achieving a balance between higher strength and equal toughness.

[0101] Comparing Example 1 with Comparative Examples 3 and 4, it can be seen that, compared with the prior art, the negative electrode binder of this application can form a rigid-flexible-adhesive multi-synergistic effect through a comb-shaped topological matrix of rigid bio-based main chain + single / multi-carboxyl composite polar adhesive side chain + dynamic polydisulfide flexible side chain and dynamic crosslinking agent containing catechol groups and borate ester groups. The elongation at break and tensile strength are significantly improved. The high-density crosslinking sites of multi-carboxyl groups form multi-point complexation and hydrogen bonding with the hydroxyl groups of borate ester groups and catechol groups to form a highly dense and uniform crosslinking network, which effectively blocks the penetration of small molecules of electrolyte. The swelling rate of electrolyte is significantly reduced. After long-term immersion in electrolyte, the film structure is intact, without swelling, collapse, peeling and flaking.

[0102] Comparing Example 1 with Comparative Example 5, it can be seen that the catechol groups can undergo multi-point complexation and hydrogen bonding with the high-density cross-linking sites of the carboxyl groups to form a highly dense and uniform cross-linking network, which effectively blocks the penetration of small molecules in the electrolyte and significantly reduces the swelling rate of the electrolyte; and through the formation of a rigid-flexible-viscous multiple synergistic effect, the elongation at break and tensile strength are significantly improved.

[0103] 2. Performance of the negative electrode sheet [Initial viscosity, viscosity after 24 hours of standing, viscosity growth rate] The viscosity of the negative electrode slurry was tested using a viscometer. The testing procedure was as follows: the viscometer probe was inserted into the slurry, and the viscosity value at 25°C was recorded. The initial viscosity and the viscosity after 24 hours of standing were measured. Viscosity growth rate = (Viscosity after 24 hours of standing / Initial viscosity) × 100%.

[0104] [Peel Strength] The bonding performance of the negative electrode sheet was tested according to GB / T 2792-2014 standard. The negative electrode sheet was cut into standard strips with a width of 25 mm and a length of 150 mm. The test was carried out using an electronic universal testing machine. The peel rate was set to 100 mm / min and the effective peel length was not less than 100 mm. Each group of samples was tested in parallel 5 times, and the average value was taken as the final peel strength.

[0105] [Flexibility] Tightly wind the negative electrode sheet around cylindrical needles of different diameters and observe whether the electrode coating cracks or peels off. Record the smallest needle diameter in mm at which the electrode coating does not crack or peel off. The smaller the value, the better the flexibility of the negative electrode sheet.

[0106] The test results are shown in Table 2.

[0107] Table 2 As shown in Table 2, due to the significant improvement in elongation at break and tensile strength, the flexibility and peel strength of the negative electrode sheet in this application are also significantly improved.

[0108] The negative electrode binder of this application significantly improves the water dispersibility and dissolution rate of the binder through the synergistic effect of triple hydrophilic groups of sulfonic acid group, monocarboxyl group and polycarboxyl group, so that the rheological properties of the negative electrode slurry are stable for a long time. The viscosity growth rate of the negative electrode slurry after standing for 24 hours is significantly reduced, and there is no stratification, precipitation or gel thickening during long-term storage. The stability of the negative electrode slurry is significantly better than that of the existing physical blending system (Comparative Example 3) and commercial system (Comparative Example 4). Moreover, through the formation of a rigid-flexible-adhesive multi-synergistic effect, the negative electrode binder of this application has good interfacial bonding force and good flexibility.

[0109] Comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the triple strong hydrophilic functional groups of sulfonic acid group + monocarboxyl group + polycarboxyl group work together to construct a triple dense hydration protective film. Compared with the single acrylic acid system, it has better water retention, negative electrode slurry stability, and lower viscosity growth rate. Moreover, the high-density carboxyl groups with monocarboxyl and polycarboxyl groups coexist to construct a hydrogen bond reinforcement network, further strengthening the interfacial bonding force.

[0110] Comparing Example 1 with Comparative Example 5, it can be seen that the catechol groups enhance interfacial adhesion, and the combination with carboxyl groups significantly enhances the interfacial bonding force between the binder and the negative electrode active material particles and current collector. Furthermore, the synergistic effect of the catechol groups and carboxyl groups is beneficial to the stability of the negative electrode slurry.

[0111] 3. Electrochemical performance The electrochemical properties, such as interfacial impedance, of the secondary batteries in the above examples and comparative examples were tested to evaluate the cycle stability and rate performance of the batteries. The test results are shown in Table 3.

[0112]

Electrode Interfacial Impedance (EIS)

[0113] [Initial Reversible Specific Capacity] Perform 1-3 complete charge-discharge cycles at a selected low rate (e.g., 0.1C). Resting: After activation, allow the battery to rest for a period to stabilize. First Charge: Charge at a constant current (e.g., 0.1C) to the cutoff voltage (e.g., 4.2V), then charge at a constant voltage until the current drops to the cutoff current (e.g., 0.05C). Record the charge capacity Qcharge,1st. Resting: After charging, allow the battery to rest (e.g., 5-30 minutes). First Discharge: Discharge at the same current (0.1C) to the cutoff voltage (e.g., 3.0V). Record the discharge capacity Qdischarge,1st (i.e., the initial reversible specific capacity IRC).

[0114]

Initial Coulomb Efficiency

[0115] [Capacity Retention Rate] Under a constant temperature environment of 25℃±2℃, the Blue Electric high-precision battery testing system was used; the battery voltage range was tested from 2.75V to 4.25V, and the charge / discharge rate was 1C; the battery was first charged at a constant current of 1C to the cutoff voltage, allowed to stand for 5 minutes, and then discharged at a constant current of 1C to the cutoff voltage, completing one cycle; this was repeated for 200 cycles; the discharge capacity C1 of the first cycle and the discharge capacity C of the 200th cycle were recorded. 200 Calculate the capacity retention rate = (C 200 / C1)×100%.

[0116] Table 3 As shown in Table 3, the negative electrode binder of this application can significantly reduce the electron transport impedance of the electrode and improve the rate performance and cycle stability of the battery.

[0117] The secondary battery of this application has a certain improvement in capacity retention rate compared with the ternary graft system (Comparative Examples 1 and 2) after 200 cycles at 1C, and a significant improvement compared with the existing physical blend system (Comparative Example 3) and the commercial CMC / SBR system (Comparative Example 4). Compared with Comparative Examples 1 to 5, the electrode interface impedance is significantly reduced, ion transport is faster, and rate performance is significantly improved. After long-term cycling, the electrode structure integrity is excellent, the probability of active material shedding, pulverization, and debinding is extremely low, and the long-term service stability is greatly improved.

[0118] Comparing Example 1 with Examples 13-14, it can be seen that: the negative electrode binder of this application can uniformly coat hard carbon particles and conductive agents by virtue of the strong wetting properties of polycarboxyl groups, thus constructing a continuous, dense, and highly elastic adhesive network; the amount of binder is moderate, which not only meets the functional requirements of particle coating, interface bonding, and structural buffering, but also avoids excessive binder crowding of electrode pores and reducing sodium ion transport efficiency, thereby maximizing the balance between electrode structural stability and energy density; the moderate amount of binder can make the electrode interface impedance lower, ion transport smoother, and the active material less likely to fall off and pulverize during cycling, thus taking into account high capacity, long cycle time, and high rate performance.

[0119] Therefore, the negative electrode binder of this application solves multiple technical problems by grafting and copolymerizing four types of structural units into one, addressing the issues of high brittleness of single polyacrylic acid, weak bonding of ordinary ungrafted or unmodified lignin, poor stability of pure thioctic acid, and loose and unstable structure of physical blends. Furthermore, by controlling the grafting rate to precisely regulate the composition and structural uniformity of molecular chain segments, it achieves a multi-dimensional balance of high bonding strength, excellent swelling resistance, strong dynamic toughness, good process adaptability, and low interfacial impedance. It is especially suitable for hard carbon negative electrodes of sodium-ion batteries, effectively buffering the deformation during the sodium intercalation and deintercalation process of hard carbon, and improving long-cycle stability, battery cycle life, and rate performance.

[0120] The present application has been further described above with reference to specific embodiments. However, it should be understood that the specific descriptions herein should not be construed as limiting the substance and scope of the present application. Various modifications made by those skilled in the art to the above embodiments after reading this specification are all within the scope of protection of the present application.

Claims

1. A negative electrode binder, characterized in that, The mixture includes copolymers and dynamic crosslinking agents. The copolymers include lignin sulfonate structural units and disulfide bond-containing structural units, acrylic structural units, and polycarboxylic acid structural units. The dynamic crosslinking agents include catechol groups and borate ester groups.

2. The negative electrode binder according to claim 1, characterized in that, The mass ratio of the copolymer to the dynamic crosslinking agent is 100:(5~20).

3. The negative electrode binder according to claim 1 or 2, characterized in that, The mass ratio of lignin sulfonate structural units to acrylic structural units, polycarboxylic acid structural units, and disulfide bond-containing structural units in the copolymer is 1:(0.4~1.0):(0.2~0.6):(0.3~1.0); And / or, the disulfide bond-containing structural unit is grafted copolymerized onto the lignin sulfonate structural unit, and the grafting rate of the copolymer is 52% to 68%.

4. The negative electrode binder according to claim 3, characterized in that, The lignin sulfonate structural unit includes at least one of sodium lignin sulfonate structural unit, calcium lignin sulfonate structural unit, enzymatically hydrolyzed lignin sulfonate structural unit, and magnesium lignin sulfonate structural unit.

5. The negative electrode binder according to claim 3, characterized in that, The disulfide-containing structural unit includes at least one of the following: thioctic acid structural unit, thiocamide structural unit, cystine diacrylate structural unit, 2,2'-dithiobisbenzimidazole diacrylate structural unit, diphenyl disulfide diacrylate structural unit, and 1,3-adamantane dithiol diacrylate structural unit.

6. The negative electrode binder according to claim 5, characterized in that, The disulfide bond-containing structural unit includes a flexible structural unit containing disulfide bonds; And / or, the disulfide-containing structural unit includes a thioctic acid structural unit and a thiocamide structural unit.

7. The negative electrode binder according to claim 3, characterized in that, The acrylic structural unit includes at least one of acrylic structural units and methacrylic acid structural units; And / or, the polycarboxylic acid structural unit includes at least one of itaconic acid structural unit, citraconic acid structural unit, mesocarboxylic acid structural unit, and fumaric acid structural unit.

8. The negative electrode binder according to claim 1 or 2, characterized in that, The dynamic crosslinking agent includes at least one of the following: borate ester-functionalized dopamine crosslinking agent, gallic acid-modified phenylboronic acid ester, L-DOPA-modified phenylboronic acid, and tannic acid-borate complex; and / or, The molar ratio of borate ester groups to catechol groups in the dynamic crosslinking agent is (1~3):(1~3).

9. A negative electrode sheet, characterized in that, The negative electrode sheet includes a current collector and a coating on the surface of the current collector, the coating including a negative electrode active material, a conductive agent and a negative electrode binder as described in any one of claims 1 to 8.

10. A secondary battery, characterized in that, The secondary battery includes the negative electrode sheet as described in claim 9.