A high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod and its preparation method
By using low-temperature hot extrusion and T5 aging treatment of Mg-Gd-Y-Zn-Zr-Ag alloy, a bimodal microstructure is formed in which fine dynamic recrystallized grains and coarse non-recrystallized grains coexist. This solves the problem of difficulty in achieving both high strength and plasticity in the existing technology, and realizes the synergy of high strength and good plasticity, which is suitable for the preparation of high load-bearing components.
Patent Information
- Application Number
- CN202611419858.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to simultaneously achieve high strength, good plasticity, and process feasibility in Mg-Gd-Y-Zn-Zr magnesium alloys, especially in the preparation of high-load-bearing and high-reliability components, where existing processes suffer from microstructure coarsening and insufficient strength-plasticity synergy.
A Mg-Gd-Y-Zn-Zr-Ag hexa-element alloy system was adopted. By combining low-temperature hot extrusion at 330~380℃, a bimodal structure was formed in which non-recrystallized deformed grains and submicron dynamically recrystallized grains coexist. The LPSO phase and grain boundary migration were regulated by adding Ag. Combined with T5 aging treatment, fine and dispersed nano-precipitates were formed to achieve strengthening.
Extruded magnesium alloy bars with a tensile strength of nearly 500 MPa and an elongation of more than 10% can be obtained in the range of 330~350℃. This simplifies the process, achieves a synergy between high strength and good plasticity, meets the requirements of high load-bearing components, and further improves the strength through T5 aging.
Smart Images

Figure CN123108376A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of magnesium alloy technology, specifically to a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod and its preparation method. Background Technology
[0002] Magnesium alloys possess advantages such as low density, high specific strength and specific stiffness, good vibration damping performance, and easy recyclability, making them valuable for applications in lightweight fields such as aerospace, rail transportation, automobiles, and defense equipment. As lightweight components develop towards higher load-bearing capacity and higher reliability, materials need to possess both high yield strength, tensile strength, and sufficient plasticity to reduce the risk of early cracking during processing and service.
[0003] In Mg-Gd-Y-Zn-Zr rare earth magnesium alloys, Gd and Y provide solid solution strengthening and precipitation strengthening, Zn is conducive to the formation of strengthening structures such as LPSO, and Zr can refine the as-cast grains. After hot extrusion to refine the grains and control the second phase and texture, this type of alloy has high absolute strength potential; however, a higher degree of alloying also increases the resistance to hot deformation, and the increase in strength is often accompanied by a loss of plasticity. At the same time, appropriate low-temperature extrusion is beneficial to suppress the coarsening of recrystallized grains and dynamic precipitates, forming a bimodal structure in which fine dynamic recrystallized grains and coarse deformed grains coexist; however, excessively low temperatures will increase the resistance to deformation and reduce the forming stability. In addition, T5 treatment can directly artificially age the extruded material, retaining the extruded fine grains, dislocations and heterogeneous structures and introducing nanoprecipitate strengthening; however, if the precursor structure, aging temperature and time are not properly controlled, the problem of coarsening of the structure and the problem of increased strength accompanied by decreased plasticity can easily occur.
[0004] In the prior art, invention patent CN114908279A discloses a low-temperature extrusion and aging method for Mg-Gd-Y-Zn-Zr alloys, which focuses on the synergy of high strength and fracture toughness; invention patent CN114107849A uses hot extrusion at 300~450℃ and relies on high-pressure air for online rapid cooling to form a bimodal structure, which is complex; invention patent CN111286657A has a relatively high extrusion temperature, and the aged tensile strength is about 430~441MPa, the yield strength is about 335~338MPa, and the elongation is about 4.3~6.0%, which has limited strength-ductility synergy; invention patent CN103184379B involves biodegradable Mg-Gd-Zn-Ag-Zr alloys, but does not design for the construction of bimodal structure and the synergy of strength and ductility at T5 for high load-bearing structural bars.
[0005] In summary, although existing technologies have covered low-temperature extrusion, bimodal microstructure, artificial aging, and Ag microalloying, there is still a lack of a technical solution that integrates the design of a Mg-Gd-Y-Zn-Zr-Ag hexa-element composition, the submicron bimodal microstructure constructed by conventional low-temperature extrusion, and T5 aging strengthening. Therefore, it is urgent to develop a wrought magnesium alloy with high strength, good plasticity, and process feasibility, as well as its preparation method. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a high-strength, high-plasticity Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod and its preparation method, thereby solving the problem that it is difficult to simultaneously achieve high strength, good plasticity, and process feasibility in existing Mg-Gd-Y-Zn-Zr magnesium alloys.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] A high-strength, high-plasticity Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod, comprising, by mass fraction: Gd 9.8~10.5%, Y 1.9~2.3%, Zn 1.0~1.3%, Zr 0.4~0.6%, Ag 0.9~1.3%, with the balance being Mg and unavoidable impurities.
[0009] This invention also provides a method for preparing high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rods, comprising the following steps:
[0010] S1. Take the raw materials of each component according to the specified amount, and then melt and cast them to obtain magnesium alloy ingots;
[0011] S2. Homogenize the magnesium alloy ingot obtained in S1 to obtain magnesium alloy billet;
[0012] S3. The magnesium alloy billet obtained in S2 is hot-extruded and then water-cooled to room temperature to obtain magnesium alloy rods.
[0013] Preferably, in step S1, the Mg is made from pure Mg, the Gd is made from Mg-30%Gd master alloy, the Y is made from Mg-30%Y master alloy, the Zn is made from pure Zn, the Zr is made from Mg-30%Zr master alloy, and the Ag is made from pure Ag.
[0014] Preferably, in step S1, the specific method of smelting is as follows: the surface of each component raw material is cleaned and dried, and then pure Mg is heated to 740-760 °C and completely melted under the protection of a CO2 / SF6 mixed gas with a volume ratio of 99:1. Then, Mg-30%Gd master alloy, Mg-30%Y master alloy, pure Zn and Mg-30%Zr master alloy are added in sequence, stirred and mixed evenly and fully melted, and then pure Ag is added. The smelting is continued at 740-760 °C for 20-30 min with slow stirring to obtain magnesium alloy melt.
[0015] Preferably, the specific method of casting is as follows: the magnesium alloy melt is subjected to slag removal treatment, then poured into a preheated metal mold, allowed to stand, demolded, and cooled to room temperature to obtain a magnesium alloy ingot.
[0016] Preferably, the preheating temperature of the metal mold is 180~200℃, and the settling time is 5~10min.
[0017] Preferably, in step S2, the specific method of homogenization treatment is as follows: the magnesium alloy ingot obtained in S1 is kept at 490~510℃ for 8~10h, and then water-cooled to room temperature to obtain magnesium alloy billet.
[0018] Preferably, in step S3, before hot extrusion, the magnesium alloy billet needs to be processed into an extruded bar with a diameter of 40 mm.
[0019] Preferably, the hot extrusion temperature is 330~380℃, the extrusion ratio is 9~18:1, the extrusion speed is 0.1mm / s~0.2mm / s, and the diameter of the magnesium alloy rod after extrusion is 10mm.
[0020] Preferably, the magnesium alloy rod prepared in step S3 is artificially aged at 200°C for 24 hours, and then air-cooled to room temperature to obtain an aged magnesium alloy rod.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. This invention employs a Mg-Gd-Y-Zn-Zr-Ag hexa-element alloy system, combined with low-temperature hot extrusion at 330~380℃. Through a single extrusion, a bimodal microstructure is formed where unrecrystallized deformed grains and submicron dynamically recrystallized grains coexist, while retaining long-period ordered stacked phase (LPSO phase) and fine dynamic precipitates. The addition of an appropriate amount of Ag allows for the regulation of the morphology and distribution of the LPSO phase during homogenization, promoting the formation of lamellar LPSO phases within the grains and refining them into blocky LPSO phases, providing a suitable initial microstructure for subsequent hot deformation. During hot working, Ag reduces the alloy's hot deformation activation energy and deformation resistance, improves dynamic softening ability during low-temperature deformation, and, together with the LPSO phase and dynamic precipitation behavior, regulates the dynamic recrystallization process. Furthermore, a strong interaction exists between Ag and Gd, which can form Gd-Ag solute co-segregation at local grain boundaries, regulating grain boundary migration. Therefore, Ag does not simply increase the degree of recrystallization, but rather, by adjusting recrystallization nucleation, grain boundary migration, and LPSO phase morphology, it enables the alloy to form a heterogeneous structure during low-temperature extrusion, where fine dynamic recrystallized grains coexist with coarse, unrecrystallized grains. Through these effects, the present invention can stably form a bimodal heterogeneous structure composed of fine dynamic recrystallized grains and coarse, unrecrystallized deformed grains at a relatively low extrusion temperature of 330–380°C. Further T5 aging with Ag also enhances the age-hardening response of the alloy, leading to the formation of fine, dispersed nanoprecipitates in the matrix, thereby achieving further strengthening.
[0023] 2. Within the extrusion temperature range of 330~350℃, the extruded magnesium alloy rods of this invention can obtain a tensile strength of nearly 500MPa and an elongation of more than 10%, thus they can be used directly as high-strength and high-plasticity materials without the need for subsequent artificial aging as a necessary step to obtain high strength performance. This solves the problems of insufficient strength-plasticity synergy and unsatisfactory extruded performance of existing Ag-containing magnesium alloys.
[0024] 3. When further strength improvement is required, the present invention can directly use the bimodal structure formed by low-temperature extrusion at 330℃ as the T5 precursor state, without the need for high-temperature solidification again. Only 200℃×24h artificial aging is required to introduce nano-precipitation strengthening while retaining the fine grains, dislocations and heterogeneous structure of low-temperature extrusion, thus avoiding the problems of coarsening structure and complex process flow of the traditional T6 route.
[0025] 4. This invention adopts a conventional process route of melting and casting, homogenization, one-time low-temperature hot extrusion, and optional T5 aging. It does not require a special online rapid cooling device, secondary extrusion, multi-directional forging, or large deformation rolling and other complex processes. The process is simple, has good controllability, is easy to implement and scale up, and can achieve synergistic adjustability of high strength and good plasticity on the basis of the same alloy system and the same precursor process, so as to meet the application requirements of high load-bearing and high reliability components.
[0026] Other advantages, objectives and features of the present invention will become apparent in part from the following description, and in part from those skilled in the art through study and practice of the invention. Attached Figure Description
[0027] Figure 1 The above are statistical charts showing the dynamic recrystallization area fraction and dynamic recrystallization grain size of the magnesium alloy rods prepared in Examples 1-3 of this invention.
[0028] Figure 2 The above are statistical diagrams of LPSO phase and dynamic precipitated phase in the magnesium alloy rods prepared in Examples 1-3 of this invention.
[0029] Figure 3 The above is a statistical chart of the room temperature tensile properties of the magnesium alloy rods prepared in Examples 1-3 of this invention.
[0030] Figure 4 This is the age hardening curve of Example 4.
[0031] Figure 5 This is a comparison chart of the room temperature tensile properties of Example 1 and Example 4. Detailed Implementation
[0032] To make the technical means, creative features, objectives, and effects of this invention clearer and easier to understand, the invention will be further described below in conjunction with the accompanying drawings and specific embodiments:
[0033] Example 1
[0034] The high-strength, high-plasticity Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod provided in this embodiment comprises, by mass fraction: Gd 10.20%, Y 2.10%, Zn 1.12%, Zr 0.49%, Ag 1.13%, with the balance being Mg and unavoidable impurities.
[0035] The preparation method of the above-mentioned high-strength and high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod includes the following steps:
[0036] S1. After measuring the raw materials of each component and removing impurities and drying them, pure Mg is heated to 750 °C and completely melted under the protection of a CO2 / SF6 mixed gas with a volume ratio of 99:1. Then, Mg-30%Gd master alloy, Mg-30%Y master alloy, pure Zn and Mg-30%Zr master alloy are added in sequence. After stirring and mixing evenly and fully melting, pure Ag is added. The mixture is then kept at 750 °C for 20-30 min and slowly stirred to obtain a magnesium alloy melt. The magnesium alloy melt is then slag-removed and poured into a metal mold preheated to 200 °C. After standing for 10 min, it is demolded and cooled to room temperature to obtain a magnesium alloy ingot.
[0037] S2. The magnesium alloy ingot obtained in S1 is kept at 500℃ for 9 hours for homogenization treatment. After completion, it is cooled to room temperature by water to obtain magnesium alloy billet.
[0038] S3. The magnesium alloy billet obtained in S2 is processed into an extruded bar with a diameter of 40 mm. Then, it is hot-extruded at an extrusion temperature of 330℃, an extrusion ratio of 16:1, and an extrusion speed of 0.1 mm / s. After that, it is water-cooled to room temperature to obtain a magnesium alloy bar with a diameter of 10 mm.
[0039] Example 2
[0040] The difference compared to Example 1 is that the extrusion temperature in step S3 is 350°C.
[0041] Everything else is the same.
[0042] Example 3
[0043] The difference compared to Example 1 is that the extrusion temperature in step S3 is 380°C.
[0044] Everything else is the same.
[0045] Example 4
[0046] The magnesium alloy rod prepared in Example 1 was placed in an aging furnace at 200°C and kept at that temperature for 24 hours to obtain an aged magnesium alloy rod.
[0047] The aging parameters in Example 4 were determined as follows: the magnesium alloy rod prepared in Example 1 was machined into cylindrical aging specimens with a diameter of Φ10mm × 4mm using wire cutting. After the aging furnace was heated to 200℃ and held at a stable temperature, the specimens were placed in the furnace and aged for 8h, 16h, 24h, 32h, 40h, 48h, 56h, 64h, 72h, and 80h, respectively. The specimens were then removed and cooled to room temperature in air at room temperature.
[0048] Then, a micro Vickers hardness tester was used to test the hardness of the samples at each aging time, with a test force of 0.5 kgf and a holding time of 15 s. Figure 4 It can be seen that the alloy hardness increases rapidly from 120.0 HV at the initial 0h, reaching a peak of 133.3 HV at 24h; after further extending the aging time, the hardness gradually decreases and tends to stabilize after 48h. Therefore, 200℃×24h is determined to be the preferred aging parameter.
[0049] Subsequently, the dynamic recrystallization grain size (DRX grain size), dynamic recrystallization area fraction (DRX area fraction), LPSO phase volume fraction, and room temperature tensile properties of the magnesium alloy rods prepared in Examples 1-3 were tested, and the specific structures are shown in Table 1.
[0050]
[0051] Table 1. Results of microstructure and mechanical properties of magnesium alloy rods prepared in Examples 1-3
[0052] From Table 1 and Appendix Figure 1-3 It can be seen that as the hot extrusion temperature increases from 330℃ to 380℃, the dynamic recrystallization area fraction gradually increases, the dynamic recrystallization grain size increases, and the LPSO phase volume fraction decreases; the tensile strength (UTS) and yield strength (TYS) of the bar gradually decrease, while the elongation (elevation after fracture) increases.
[0053] Among them, under the condition of hot extrusion temperature of 330℃, the magnesium alloy rod prepared in Example 1 has a high proportion of fine dynamic recrystallized grains, while retaining more unrecrystallized deformed grains, LPSO phase and fine dynamic precipitates, thus obtaining the highest tensile strength and yield strength, and maintaining an elongation of more than 10%.
[0054] Under the condition of hot extrusion temperature of 350℃, the magnesium alloy rod prepared in Example 2 still maintains submicron dynamic recrystallized grains and obvious bimodal structure, with a tensile strength close to 500MPa and an elongation further improved, showing a good balance between strength and plasticity.
[0055] Under the condition of hot extrusion temperature of 380℃, the degree of dynamic recrystallization of the magnesium alloy rod prepared in Example 3 is further improved, the size of the dynamic recrystallized grains and dynamic precipitates increases, so the strength decreases, but the elongation is significantly improved.
[0056] In summary, the magnesium alloy bars prepared in Examples 1-3 of this invention can achieve a good balance between strength and plasticity without further artificial aging, and 330~350℃ is the preferred hot extrusion temperature range for obtaining high strength and good plasticity. When plasticity is of greater importance, the hot extrusion temperature can be appropriately increased.
[0057] In addition, the hardness and room temperature tensile properties of Examples 1 and 4 were tested, and the specific results are shown in Table 2.
[0058]
[0059] Table 2. Hardness and room temperature tensile properties of the magnesium alloy rods prepared in Examples 1 and 5.
[0060] From Table 2 and Figure 5 It can be seen that the T5 aging treatment at 200℃ for 24h increases the tensile strength (UTS) and yield strength (TYS) of magnesium alloy bars from 503±9MPa and 480±8MPa to 545±7MPa and 522±4MPa, respectively, while the elongation (elongation after fracture EL) remains above 10%.
[0061] Combination Figure 4 , Figure 5 The microstructure characterization results show that the T5 aging treatment at 200℃ for 24h can introduce nano-precipitation strengthening while basically preserving the bimodal microstructure of low-temperature extrusion. This allows the existing fine grains, non-recrystallized deformation regions, and second-phase strengthening in the extrusion state to be superimposed with the strengthening of aging precipitation, thereby achieving further strengthening without significantly sacrificing plasticity.
[0062] Therefore, this invention provides a two-level performance regulation path under the same Mg-Gd-Y-Zn-Zr-Ag alloy system: the extrusion state of Examples 1-3 can directly obtain a tensile strength of 500MPa and an elongation of more than 10%; when a higher load-bearing capacity is required, the aging treatment of Example 4 can be further adopted to increase the yield strength to more than 500MPa, while maintaining an elongation of about 10%.
[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod, characterized in that, The composition by mass fraction includes: Gd 9.8~10.5%, Y 1.9~2.3%, Zn 1.0~1.3%, Zr 0.4~0.6%, Ag 0.9~1.3%, with the balance being Mg and unavoidable impurities.
2. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 1, characterized in that, Includes the following steps: S1. Take the raw materials of each component according to the specified amount, and then melt and cast them to obtain magnesium alloy ingots; S2. Homogenize the magnesium alloy ingot obtained in S1 to obtain magnesium alloy billet; S3. The magnesium alloy billet obtained in S2 is hot-extruded and then water-cooled to room temperature to obtain magnesium alloy rods.
3. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 2, characterized in that, In step S1, the Mg is made from pure Mg, the Gd is made from Mg-30%Gd master alloy, the Y is made from Mg-30%Y master alloy, the Zn is made from pure Zn, the Zr is made from Mg-30%Zr master alloy, and the Ag is made from pure Ag.
4. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 3, characterized in that, In step S1, the specific melting method is as follows: the surfaces of each component raw material are cleaned and dried. Then, under the protection of a CO2 / SF6 mixed gas with a volume ratio of 99:1, pure Mg is heated to 740-760 °C and completely melted. Then, Mg-30%Gd master alloy, Mg-30%Y master alloy, pure Zn and Mg-30%Zr master alloy are added in sequence. After stirring and mixing evenly and fully melting, pure Ag is added. The melting is continued at 740-760 °C for 20-30 min with slow stirring to obtain magnesium alloy melt.
5. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 4, characterized in that, The specific casting method is as follows: the magnesium alloy melt is treated by slag removal, then poured into a preheated metal mold, left to stand, demolded, and cooled to room temperature to obtain a magnesium alloy ingot.
6. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 5, characterized in that, The preheating temperature of the metal mold is 180~200℃, and the settling time is 5~10min.
7. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 2, characterized in that, In step S2, the specific method of homogenization treatment is as follows: the magnesium alloy ingot obtained in S1 is kept at 490~510℃ for 8~10h, and then water-cooled to room temperature to obtain magnesium alloy billet.
8. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 2, characterized in that, In step S3, before hot extrusion, the magnesium alloy billet needs to be processed into an extruded bar with a diameter of 40mm.
9. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 2, characterized in that, The hot extrusion temperature is 330~380℃, the extrusion ratio is 9~18:1, the extrusion speed is 0.1mm / s~0.2mm / s, and the diameter of the magnesium alloy rod after extrusion is 10mm.
10. The method for preparing a high-strength, high-ductility Mg-Gd-Y-Zn-Zr-Ag magnesium alloy rod according to claim 2, characterized in that, The magnesium alloy rod prepared in step S3 was artificially aged at 200°C for 24 hours, and then air-cooled to room temperature to obtain aged magnesium alloy rod.
Citation Information
Patent Citations
Biodegradable Mg-Gd-Zn-Ag-Zr magnesium alloys and their preparation methods
CN103184379B
High-strength Mg-Gd-Zn-Zr-Ag magnesium alloy and preparation method thereof
CN111286657A
Preparation method of high-toughness Mg-Gd-Y-Zn-Zr wrought magnesium alloy
CN114107849A
Preparation method of high-strength and high-fracture-toughness Mg-Gd-Y-Zn-Zr magnesium alloy
CN114908279A