Methods for activating room-temperature superelasticity in NiTi alloys, NiTi alloys and their applications
By subjecting NiTi alloy samples to cold and hot cycling treatment, geometrically necessary dislocations are accumulated, the phase transformation temperature is reduced, and the alloy exhibits stable superelasticity at room temperature. This solves the problem that superelasticity of NiTi alloy at room temperature is difficult to achieve, with a recovery rate of 95%.
Patent Information
- Application Number
- CN202611237221.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing NiTi alloys are difficult to exhibit superelasticity at room temperature due to their high phase transformation temperature. Therefore, it is necessary to develop methods to reduce the phase transformation temperature in order to achieve room temperature superelasticity.
By subjecting NiTi alloy samples to thermal cycling treatment, including holding at temperatures above the austenitic phase transformation end temperature and then holding at temperatures below the martensitic phase transformation end temperature, and repeating this process multiple times, geometrically necessary dislocations are accumulated in the alloy samples, the phase transformation characteristic temperature is reduced, and the alloy is made to stably maintain the austenitic phase at room temperature.
The method achieves stable superelastic behavior of NiTi alloy at room temperature with a recovery rate of over 95%, and is simple to operate, making it suitable for shape memory alloy components with complex structures.
Smart Images

Figure CN123108450A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of shape memory alloy technology, specifically to a method for activating the room temperature superelasticity of NiTi alloy, NiTi alloy and its applications. Background Technology
[0002] NiTi alloys, due to their excellent superelasticity, have wide applications in biomedicine, aerospace, and solid-state thermoelastic refrigeration. Superelasticity refers to the property of NiTi alloys undergoing a phase transformation to martensite under stress loading in the austenitic state, and then reverting to austenite after the external force is unloaded, thus achieving reversible strain recovery. In practical applications, most scenarios require NiTi alloys to exhibit excellent superelastic behavior at room temperature (approximately 25 °C).
[0003] However, the NiTi alloy samples prepared by various techniques in related technologies exhibit high phase transformation temperatures, meaning they only display superelastic behavior at relatively high temperatures. Therefore, developing an effective method to reduce the phase transformation temperature of NiTi alloys and restore their room-temperature superelasticity is currently one of the challenges.
[0004] Application content This application aims to at least partially address one of the technical problems in the related art. Therefore, one objective of this application is to provide a method for activating room-temperature superelasticity in NiTi alloys, NiTi alloys themselves, and their applications, wherein the NiTi alloys treated by this method exhibit superelastic behavior at room temperature.
[0005] The first aspect of this application proposes a method for activating room-temperature superelasticity in NiTi alloys, comprising: The NiTi alloy sample was held at a first temperature for a first time, and then held at a second temperature for a second time. Repeat the above steps 200-500 times; Wherein, the first temperature is higher than the austenitic phase transformation end temperature of the NiTi alloy sample, and the second temperature is lower than the martensitic phase transformation end temperature of the NiTi alloy sample.
[0006] In this application, the NiTi alloy sample is held at a temperature higher than the austenitic transformation end temperature for a first time to ensure that the entire NiTi alloy sample is transformed into austenite with no residual martensite. Then, the austenite is held at a temperature lower than the martensitic transformation end temperature for a second time to further transform the austenite into martensite, and finally, a second transformation back into austenite occurs. During the austenite-to-martensite transformation, large-scale shear distortion occurs inside the NiTi alloy sample, resulting in the formation of numerous martensite / austenite phase interfaces. To accommodate this shear distortion, a large number of geometrically necessary dislocations are generated at the phase interfaces. However, when the martensite transforms back into austenite, the original martensite / austenite phase interfaces completely annihilate, while the large number of geometrically necessary dislocations remain inside the NiTi alloy sample.
[0007] Furthermore, by repeating the above steps, the accumulation of geometrically necessary dislocations in the NiTi alloy sample is achieved, thereby enabling the process of overcoming this resistance to complete the martensitic phase transformation at a lower temperature. Ultimately, the overall characteristic temperature of the martensitic and austenitic phase transformation of the material is reduced, allowing the alloy to stably maintain the austenitic phase at room temperature, thus exhibiting stable superelasticity.
[0008] In some embodiments, at least one of the following conditions is met: The first temperature is 50℃~200℃; The second temperature is ≤0℃.
[0009] In some embodiments, at least one of the following conditions is met: The step of keeping the NiTi alloy sample at a first temperature includes: placing the NiTi alloy sample in a first heat exchange medium at the first temperature, wherein the first heat exchange medium includes at least one of water and oil. The step of keeping the NiTi alloy sample at a second temperature includes: placing the NiTi alloy sample in a second heat exchange medium at the second temperature, wherein the second heat exchange medium includes at least one of liquid nitrogen and liquid helium.
[0010] In some embodiments, the first time and the second time are satisfied independently: ; in, ρ The density of the NiTi alloy sample is expressed in kg / m³. 3 , c p The specific heat capacity of the NiTi alloy sample is expressed in J / (kg). K), V represents the volume of the NiTi alloy sample, in m³. 3 h represents the heat transfer coefficient of the heat transfer medium, with units of W / (m³).2 K), A represents the surface area of the NiTi alloy sample, in m². 2 T0 represents the initial temperature of the NiTi alloy sample, in °C. t The target temperature of the NiTi alloy sample is represented in °C. This represents the constant temperature of the heat exchange medium, expressed in °C.
[0011] In some embodiments, before holding the NiTi alloy at a first temperature for a first time, the method further includes: The NiTi alloy was held at a third temperature for a third time, followed by quenching.
[0012] In some embodiments, at least one of the following conditions is met: The third temperature is 250℃~450℃; The third time period is 1 hour to 24 hours.
[0013] In a second aspect, this application proposes a NiTi alloy obtained by the aforementioned method for activating the room-temperature superelasticity of NiTi alloys. Consequently, this NiTi alloy exhibits stable and excellent superelastic behavior at room temperature.
[0014] In some embodiments, the NiTi alloy exhibits a superelastic recovery rate of ≥95% at room temperature.
[0015] In a third aspect of this application, an application of the aforementioned NiTi alloy in the fields of biomedicine, aerospace, and solid-state thermo-elastic refrigeration is proposed.
[0016] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0017] Figure 1 This is a morphological diagram of the NiTi alloy sample in Example 1 of this application.
[0018] Figure 2 This is a schematic diagram of the hot and cold alternation in Embodiment 1 of this application.
[0019] Figure 3 The superelasticity test curves of Examples 1 and 2 of this application at room temperature are shown.
[0020] Figure 4 The graphs show the stress plateau values and strain recovery rates of Examples 1 and 2 of this application.
[0021] Figure 5The diagram shows the phase transition behavior of Embodiment 1 and Comparative Examples 1-2 of this application. Detailed Implementation
[0022] The embodiments of this application are described in detail below. The embodiments described below are exemplary and intended to explain this application, and should not be construed as limiting this application.
[0023] Based on the preceding description, the inventors considered forming a large network of dislocations within the NiTi alloy sample. The long-range elastic stress field generated by these dislocations would increase the resistance to martensite nucleation and phase interface migration, thereby increasing the critical driving force required for phase transformation. In other words, if the original NiTi alloy sample is initially martensitic at room temperature and therefore cannot exhibit superelasticity, the overall characteristic temperature of the martensitic-austenitic phase transformation can be lowered by introducing a large number of dislocations, allowing the alloy to stably maintain the austenitic phase at room temperature and thus exhibit stable superelasticity.
[0024] Furthermore, considering that NiTi alloy samples can undergo reversible phase transformations under drastic temperature changes, and that this process accumulates geometrically necessary dislocations within the NiTi alloy samples, thereby forming a large number of dislocation networks.
[0025] In view of this, a first aspect of this application proposes a method for activating the room-temperature superelasticity of NiTi alloys, comprising: S10: Hold the NiTi alloy sample at a first temperature for a first time, and then hold it at a second temperature for a second time.
[0026] In this step, the first temperature is higher than the austenitic phase transformation end temperature (A) of the NiTi alloy sample. f The second temperature is lower than the martensitic phase transformation end temperature (M) of the NiTi alloy sample. f By holding the NiTi alloy sample at a temperature higher than the end temperature of the austenitic phase transformation of the NiTi alloy sample for a first time, it can be ensured that the NiTi alloy sample is completely transformed into austenite with no residual martensite. Furthermore, by holding the austenite at a temperature lower than the end temperature of the martenitic phase transformation of the NiTi alloy sample for a second time, it can be ensured that the austenite is completely transformed into martensite, and finally undergoes a phase transformation to transform into austenite again.
[0027] During the austenite-to-martensite transformation process, large-scale shear distortion occurred inside the NiTi alloy sample, resulting in the formation of a large number of martensite / austenite phase interfaces. To accommodate the shear distortion, a large number of geometrically necessary dislocations were generated at the phase interfaces. However, when the martensite transformed back into austenite, the original martensite / austenite phase interfaces were completely annihilated, while the large number of geometrically necessary dislocations remained inside the NiTi alloy sample.
[0028] In some embodiments, the first temperature is 50°C to 200°C, specifically, it can be 50°C, 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, etc. A of the NiTi alloy sample. f Depending on the specific composition of the NiTi alloy sample, the first temperature within the above range can basically guarantee that the NiTi alloy sample will achieve the transformation from martensite to austenite.
[0029] Furthermore, the type of medium used to achieve the first temperature is not limited; for example, it includes, but is not limited to, media such as water and oil. That is, the NiTi alloy sample can be placed in water at a certain temperature to achieve the phase transformation process.
[0030] In some embodiments, the second temperature is ≤0℃, specifically, it can be 0℃, -20℃, -40℃, -60℃, -80℃, etc. As described above, the M of the NiTi alloy sample... f The specific composition of the NiTi alloy sample is related to the second temperature. Within the above range, the transformation of the NiTi alloy sample from austenite to martensite can be basically guaranteed.
[0031] Furthermore, the type of medium used to achieve the second temperature is not limited; for example, it includes, but is not limited to, liquid nitrogen. That is, the NiTi alloy sample can be placed in liquid nitrogen to achieve the phase transition process.
[0032] In some embodiments, the first and second times mentioned above can both be calculated using the following formula: ;in, ρ The density of the NiTi alloy sample is expressed in kg / m³. 3 , c p The specific heat capacity of the NiTi alloy sample is expressed in J / (kg). K), V represents the volume of the NiTi alloy sample, in m³. 3 h represents the heat transfer coefficient of the heat transfer medium, with units of W / (m³). 2 K), A represents the surface area of the nickel-titanium alloy sample, in m². 2 T0 represents the initial temperature of the NiTi alloy sample, in °C. t The target temperature of the NiTi alloy sample is represented in °C. The constant temperature of the heat transfer medium is represented by °C. The heat transfer time calculated using the above formula can basically ensure that the NiTi alloy sample fully completes the phase transformation.
[0033] In some embodiments, before subjecting the NiTi alloy sample to alternating hot and cold treatment, that is, before holding the NiTi alloy sample at a first temperature for a first time, the process further includes: aging the NiTi alloy sample (holding the NiTi alloy at a third temperature for a third time, followed by quenching). Specifically, the NiTi alloy sample can be held at 250°C to 450°C for 1 hour to 24 hours, and then placed in water at room temperature. This aging treatment can precipitate strengthening phases such as Ni4Ti3, which helps improve the superelasticity of the NiTi alloy.
[0034] For example, laser powder bed melting (LPBF) technology can fabricate NiTi alloy samples with complex geometries. However, the inherent rapid non-equilibrium solidification characteristics of the LPBF process lead to a series of microstructural defects in the printed NiTi alloy samples, including large residual stress, significant columnar grain structure, and severe microstructural compositional segregation. These defects significantly deteriorate the superelasticity of the NiTi alloy samples. The aforementioned aging treatment can improve the internal defects of NiTi alloy samples to some extent and promote the precipitation of second phases, thereby giving the NiTi alloy excellent and stable superelasticity. Specifically, the aforementioned aging treatment precipitates nanoscale Ni4Ti3 strengthening phases in the NiTi alloy samples. These precipitated phases can effectively pin dislocations and strengthen the matrix, while the aging process can also release residual stress, thereby significantly improving the superelasticity of the NiTi alloy.
[0035] S20: Repeat the above steps 10 to 500 times.
[0036] In this step, by repeating step S10, the accumulation of geometrically necessary dislocations in the NiTi alloy sample is achieved. This accumulation allows the material to overcome the resistance to martensitic transformation at a lower temperature, ultimately lowering the overall characteristic temperature of the martensitic and austenitic phase transformation. This enables the alloy to stably maintain the austenitic phase at room temperature, thus exhibiting stable superelasticity. For example, the hot and cold cycles in S10 can be 200, 250, 300, 350, 400, 450, and 500 cycles. Different cycle counts determine the number of dislocations introduced, thus determining the magnitude of the downward change in the characteristic temperature of the phase transformation. Generally, cycle counts within the above range can effectively introduce a large number of dislocations, ensuring the NiTi alloy exhibits stable superelasticity at room temperature. 500 cycles are sufficient to saturate the internal dislocations.
[0037] In a second aspect, this application proposes a NiTi alloy obtained by the aforementioned method for activating the room-temperature superelasticity of NiTi alloys. Consequently, this NiTi alloy exhibits stable and excellent superelastic behavior at room temperature.
[0038] In some embodiments, the NiTi alloy exhibits a superelastic recovery rate of ≥95% at room temperature.
[0039] The method for activating room-temperature superelasticity in NiTi alloys, or the resulting NiTi alloys, in this application have at least the following beneficial effects: 1. This application successfully addresses the problem of high phase transformation temperature in the initial printed state of NiTi alloy samples or the issue of Ni element depletion in the matrix and phase transformation temperature rising above room temperature after aging treatment due to Ni4Ti3 precipitates by subjecting NiTi alloy samples to thermal cycling, thereby restoring the room-temperature superelastic behavior of NiTi alloys. This application first introduces Ni4Ti3 precipitates through aging treatment to fully strengthen the matrix and stimulate potential superelasticity. Then, it utilizes thermal cycling to accumulate dislocations in the matrix. Leveraging the resistance effect of the dislocation network on phase transformation, the characteristic phase transformation temperature is effectively lowered back to below room temperature. This process can restore the room-temperature superelastic properties of NiTi alloys without altering the macroscopic shape of the sample or introducing mechanical damage. Experiments show that the strain of samples treated by this method can be completely recovered under the same conditions, achieving a significant transformation from martensitic detwinning behavior to fully austenitic superelasticity.
[0040] 2. The process of this method only involves conventional heating and insulation and immersion in liquid medium. It is simple to operate and has a simple process. Moreover, the fundamental principle adopted is to achieve repeated temperature-induced phase transformation through hot and cold cycles. This strategy is not only applicable to NiTi shape memory alloys, but also applicable to other complex shape memory alloy components that have been prepared by additive manufacturing technology. Therefore, it has extremely high engineering applicability and promotion value.
[0041] A third aspect of this application proposes an application of the aforementioned NiTi alloy in the fields of biomedicine, aerospace, and solid-state thermo-elastic cooling. For example, in the biomedical field, it can be used in vascular stents, orthodontic nickel-titanium wires, orthopedic internal fixation implants, and minimally invasive interventional devices; in the aerospace field, it can be applied to adaptive intelligent structures for aircraft, release and locking components for aerospace mechanisms, vibration damping and sealing assemblies for aviation pipelines, and vibration damping bushings for engines.
[0042] The present application will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present application in any way. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in the art or in accordance with the product manual.
[0043] Example 1 Preparation of NiTi alloy samples: Commercially available nickel-rich NiTi pre-alloyed powder was selected, with a composition of Ni 51 Ti 49(at.%) Particles with a diameter of 15 μm to 53 μm were printed using an AMC-M150B system (Guangdong, China). During printing, an alternating X / Y scanning strategy was employed, with a scanning rotation angle of 67°. Specific process parameters were: laser power 225 W, scanning speed 833 mm / s, powder layer thickness 30 μm, scanning spacing 90 μm, and substrate preheating temperature 100 ℃. An equiatomic NiTi alloy was used as the printing substrate, and the printing atmosphere was protected with high-purity argon, with oxygen content strictly controlled below 30 ppm. The printed size was 15 × 6 × 7 mm. 3 cuboid blocks such as Figure 1 As shown in (a), a dog-bone shaped tensile specimen with a gauge length of 5 mm and a thickness of 1 mm was then cut out by wire cutting in a plane perpendicular to the printing direction. Figure 1 (b) and (c) in the text. Figure 1 The unit (c) in the text is mm.
[0044] Aging treatment: The NiTi alloy sample was placed in a muffle furnace for aging treatment, heated to 350℃, held for 1 h, and then cooled in water at room temperature.
[0045] Thermal cycling treatment: The aged samples were subjected to thermal cycling treatment, alternately immersing them in a hot medium (90℃ constant-temperature hot water) and a cold medium (liquid nitrogen). Specifically, the samples were first placed in 90℃ hot water and held for 30 seconds, at which point the alloy samples completely transformed into austenite (B2 phase). They were then rapidly transferred to liquid nitrogen and held for 30 seconds. During the rapid cooling process, the alloy samples underwent a temperature-induced martensitic transformation, completely transforming into martensite (B19' phase). The alloy samples were then transferred back to 90℃ hot water and held for 30 seconds, allowing for a reverse phase transformation back to austenite. One complete bidirectional phase transformation process is recorded as one complete thermal cycle. A schematic diagram of the specific cycle process is shown below. Figure 2 Repeat the above cycle a total of 500 times to obtain the final NiTi alloy.
[0046] In the above-mentioned hot and cold cycling treatment, to ensure that the sample undergoes a sufficient phase change, it is necessary to maintain the sample at a certain temperature in each medium for a sufficient time to achieve complete thermal equilibrium. The specific time for achieving thermal equilibrium depends on... Calculations were performed, including the density of the NiTi alloy sample. ρ =6500kg / m 3 Specific heat capacity c p Approximately 275 J / (kg) K), when the heat transfer medium is liquid nitrogen, take the heat transfer coefficient. h =100W / (m 2 K), when the heat transfer medium is hot water, take the heat transfer coefficient. h =500W / (m 2 K), the sample volume V is approximately 57.43 mm. 3 The surface area A of the sample is 174 mm². 2 The initial temperature T0 of the sample is 25℃, and the temperature at thermal equilibrium is T t It is 90℃. The temperature is 90℃; during the cooling process, T t -196℃ (The actual temperature is -196℃). It should be noted that in reality, T... t It cannot be completely equal to However, it can approach the value infinitely. Therefore, when using this formula for calculations, if the medium is cold, T t Substitute any value between the end temperature of the martensitic phase transformation and the temperature of the cold medium; if it is a hot medium, T t Simply substitute any value between the end temperature of the austenitic phase transformation and the temperature of the heat transfer medium.
[0047] Example 2 Same as Example 1, the main difference is that the number of hot and cold alternation cycles is 200.
[0048] Example 3 Same as Example 1, the main difference is that the number of hot and cold alternation cycles is 300.
[0049] Example 4 Same as Example 1, the main difference is that the heat medium used during the alternation of hot and cold is 50°C constant temperature hot water.
[0050] Example 5 Same as Example 1, the main difference is that the heat medium used during alternating hot and cold is 200°C constant temperature oil.
[0051] Example 6 Same as Example 1, the main difference is that the heat preservation time during alternating hot and cold is 60 s.
[0052] Comparative Example 1 Same as Example 1, the main difference is that no aging treatment and hot-cold cycle treatment were performed.
[0053] Comparative Example 2 Same as Example 1, the main difference is that no hot and cold cycling treatment was performed.
[0054] Detection methods Hyperelasticity test curve (stress-strain curve): Quasi-static uniaxial tensile tests were performed on the specimens using a universal testing machine at room temperature (25℃). Specifically, the strain rates for loading and unloading were both 5 × 10⁻⁶. 4 s -1 The specimen was stretched to 4% strain and then unloaded. The strain of the gauge length section of the specimen was monitored in real time throughout the process using digital image correlation technology.
[0055] Phase transition temperature test: Differential scanning calorimetry (DSC) was used to characterize the phase transition behavior of the sample. The specific test conditions were: heating and cooling rate of 10 ℃ / min, and temperature range of -90 ℃ to 90 ℃.
[0056] Test results The samples from Examples 1-6 and Comparative Examples 1-2 were polished to a mirror finish and then subjected to superelasticity and phase transition temperature tests.
[0057] Specifically, the hyperelasticity test curves of Example 1, Comparative Example 1, and Comparative Example 2 are shown in [reference needed]. Figure 3 Meanwhile, the corresponding stress plateau values and strain recovery rates of each specimen were statistically analyzed, see [see details]. Figure 4 It can be seen that the sample of Comparative Example 1 exhibits certain room-temperature hyperelastic characteristics. After being stretched to 4% and unloaded, the residual strain is about 0.8%, which indicates that the printing process and nickel-rich powder used can successfully prepare samples with room-temperature hyperelasticity. However, the printed sample cannot exhibit perfect hyperelastic recovery due to the large internal residual stress and low matrix yield strength. After stretching the sample of Comparative Example 2 to 4% strain and unloading, the residual strain is as high as 3.2%. At the same time, the plateau stress value drops from 300 MPa to about 200 MPa. This mechanical behavior of low plateau stress is a typical martensitic detwinning characteristic, and the hyperelasticity is basically lost. This indicates that the initial microstructure of the sample in Comparative Example 2 is no longer a completely austenitic state. After stretching the sample of Example 1 to 4% and unloading, the strain can be almost completely recovered, and the stress plateau value also recovers to about 300 MPa in the initial printed state. The results show that the hot and cold cycling treatment not only preserves the matrix strengthening effect brought about by the aging treatment and promotes perfect superelastic recovery, but also reactivates the stress-induced martensitic phase transformation ability of NiTi alloy by lowering the phase transformation temperature, thus restoring the superelastic behavior of NiTi alloy at room temperature.
[0058] Figure 5 The heat flow and temperature curves of DSC tests for Example 1, Comparative Example 1, and Comparative Example 2 are shown. The results indicate that the martensitic phase transformation initiation temperature of the sample in Comparative Example 2 ( M s The temperature was significantly higher than room temperature, approximately 43.7℃. This is because the formation of the Ni4Ti3 precipitate led to a decrease in the Ni content of the matrix, thus increasing the phase transition temperature. Figure 5As can be seen, the cooling peak during the cooling process (the upper half of the red curve) is clearly located to the right of the dashed line at 25 ℃ (room temperature). This indicates that under room temperature conditions, the initial microstructure of the Comparative Example 2 sample was almost entirely martensite, which is the direct cause of its loss of room temperature superelasticity. Example 1 sample... M s The temperature dropped significantly to approximately 28.1℃. It can also be seen that the cooling peak is located to the left of the dashed line at 25℃ (room temperature), indicating that under room temperature conditions, the initial microstructure of the Example 1 sample was predominantly austenite. Figure 4 The mechanical properties show that the dislocations introduced by the hot and cold cycling process play a key role in increasing the phase transition resistance and thus reducing the phase transition temperature. This is the direct reason why it can promote room temperature hyperelastic recovery.
[0059] In the description of this application, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0060] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0061] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.
Claims
1. A method for activating room-temperature superelasticity in NiTi alloys, characterized in that, include: The NiTi alloy sample was held at a first temperature for a first time, and then held at a second temperature for a second time. Repeat the above steps 200-500 times; Wherein, the first temperature is higher than the austenitic phase transformation end temperature of the NiTi alloy sample, and the second temperature is lower than the martensitic phase transformation end temperature of the NiTi alloy sample.
2. The method for activating room-temperature superelasticity of NiTi alloy according to claim 1, characterized in that, At least one of the following conditions must be met: The first temperature is 50℃~200℃; The second temperature is ≤0℃.
3. The method for activating room-temperature superelasticity of NiTi alloy according to claim 2, characterized in that, At least one of the following conditions must be met: The step of keeping the NiTi alloy sample at a first temperature includes: placing the NiTi alloy sample in a first heat exchange medium at the first temperature, wherein the first heat exchange medium includes at least one of water and oil. The step of keeping the NiTi alloy sample at a second temperature includes: placing the NiTi alloy sample in a second heat exchange medium at the second temperature, wherein the second heat exchange medium includes at least one of liquid nitrogen and liquid helium.
4. The method for activating room-temperature superelasticity of NiTi alloy according to claim 3, characterized in that, The first time and the second time are satisfied independently: ; in, ρ The density of the NiTi alloy sample is expressed in kg / m³. 3 , c p The specific heat capacity of the NiTi alloy sample is expressed in J / (kg). K), V represents the volume of the NiTi alloy sample, in m³. 3 h represents the heat transfer coefficient of the heat transfer medium, with units of W / (m³). 2 K), A represents the surface area of the NiTi alloy sample, in m². 2 T0 represents the initial temperature of the NiTi alloy sample, in °C. t The target temperature of the NiTi alloy sample is represented in °C. This represents the constant temperature of the heat exchange medium, expressed in °C.
5. The method for activating room-temperature superelasticity of NiTi alloy according to claim 1, characterized in that, Before holding the NiTi alloy at the first temperature for the first time, the method further includes: The NiTi alloy was held at a third temperature for a third time, followed by quenching.
6. The method for activating room-temperature superelasticity of NiTi alloy according to claim 5, characterized in that, At least one of the following conditions must be met: The third temperature is 250℃~450℃; The third time period is 1 hour to 24 hours.
7. A NiTi alloy, characterized in that, It is obtained by the method of activating the room temperature superelasticity of NiTi alloy as described in any one of claims 1 to 6.
8. The NiTi alloy according to claim 7, characterized in that, The NiTi alloy exhibits a superelastic recovery rate of ≥95% at room temperature.
9. An application of the NiTi alloy as described in any one of claims 7 to 8 in the fields of biomedicine, aerospace, and solid-state thermo-elastic cooling.