Chromium-free composite treatment process for surface treatment of stainless steel bearings
By employing a multi-step process involving light leveling, composite alkaline degreasing, composite pickling, composite activation, chromium-free passivation, and silane sealing, the problems of incomplete carbide removal and difficulty in breaking inert oxide films in the surface treatment of stainless steel bearings have been solved. This process achieves chromium-free composite treatment with high corrosion resistance and dimensional accuracy, making it suitable for high-end precision bearings in aerospace, marine equipment, and AI robotics.
Patent Information
- Application Number
- CN202611463658.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing surface treatment processes for stainless steel bearings suffer from problems such as incomplete removal of carbides, difficulty in breaking down inert oxide films, insufficient corrosion resistance, and high environmental risks, making it difficult to meet the corrosion resistance and dimensional accuracy requirements of high-end precision bearings.
A multi-step process is adopted, including light leveling, composite alkaline degreasing, composite pickling, composite activation, chromium-free passivation, and silane sealing. Through physical and chemical treatment, surface carbides and oxide films are removed to form a double-layer protective film, ensuring the uniformity and corrosion resistance of the bearing surface.
It significantly improves the corrosion resistance of bearings, with a rust-free time of over 72 hours in neutral salt spray tests, representing a 3-fold improvement in corrosion resistance. Furthermore, the process is environmentally friendly and chromium-free, meeting the requirements of green manufacturing.
Smart Images

Figure CN123108548A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a chromium-free composite treatment process for the surface treatment of stainless steel bearings. Background Technology
[0002] G65Cr14Mo and 65Cr13 are new types of high-carbon, high-chromium martensitic stainless steels. After heat treatment, they possess excellent hardness, wear resistance, and load-bearing capacity, making them core candidate materials for high-precision bearings in aerospace, marine equipment, and AI robotics. However, after quenching and tempering, these materials exhibit a large precipitation of Cr7C3 carbides and free carbon on their surface. The hard carbides form a significant corrosion micro-cell effect with the substrate, easily inducing pitting and crevice corrosion defects, severely reducing bearing service life. Simultaneously, the high-chromium substrate readily self-passivates in atmospheric environments, forming a dense and stable Cr2O3 inert oxide film. Conventional surface pretreatment processes cannot effectively remove this inert layer, resulting in uneven passivation film formation, high porosity, and poor film-substrate adhesion, making effective protection difficult to achieve. Existing surface treatment processes for stainless steel bearings have significant shortcomings: traditional strong acid pickling processes are prone to causing over-corrosion of the substrate, making it difficult to meet the micron-level dimensional tolerance requirements of precision bearings; the protective film formed by ordinary single chromium-free passivation processes has limited protective capabilities, with rust-free time in neutral salt spray tests typically less than 24 hours, making it unsuitable for harsh and highly corrosive service environments such as marine and aerospace applications; while chromium-containing passivation processes can improve corrosion resistance, they generate a large amount of chromium-based hazardous waste, posing high environmental risks and incurring high wastewater treatment costs, which is inconsistent with the trend of green manufacturing development. Summary of the Invention
[0003] To address the shortcomings of existing technologies, this invention provides a chromium-free composite treatment process for the surface treatment of stainless steel bearings. This process can efficiently remove surface carbides and break down inert oxide films, significantly improving corrosion resistance while ensuring the dimensional accuracy of the bearings. Furthermore, the process is chromium-free, environmentally friendly, and easily industrialized.
[0004] To achieve the above objectives, the present invention provides a chromium-free composite treatment process for the surface treatment of stainless steel bearings, comprising the following steps: Step 1, Light-drilling: The stainless steel bearing parts are subjected to light-drilling treatment. The stainless steel bearing parts are made of G65Cr14Mo or 65Cr13 high carbon chromium martensitic stainless steel. This weakens the surface carbide protrusions and burr defects, and obtains a uniform reactive substrate. Step 2, alkaline degreasing: Immerse the polished bearing parts in a composite alkaline degreasing solution to remove surface oil and impurities; Step 3, composite pickling: The degreased bearing parts are pickled using a nitric acid-hydrofluoric acid composite pickling solution to remove the Cr7C3 carbides, free carbon and iron-rich phases precipitated on the surface. Step 4, Composite Activation: The pickled bearing parts are activated using a hydrochloric acid-organic acid composite activation solution to break the surface Cr2O3 inert oxide film and inhibit secondary passivation. Step 5, Chromium-free passivation: The activated bearing parts are passivated using a chromium-free passivation solution to form a manganese-nickel composite phosphate inorganic passivation film on the surface; Step 6, silane sealing: The passivated bearing parts are sealed with silane sealant and baked to cure, forming an organic silicon sealing layer on the outside of the inorganic passivation film, and finally constructing a double-layer protective film system.
[0005] The beneficial effects of this setup are as follows: This setup addresses the material characteristics of new high-carbon chromium stainless steel, which exhibits Cr7C3 carbide precipitation and spontaneous Cr2O3 inert oxide film formation after heat treatment. The processes are seamlessly integrated, functionally complementary, and synergistically enhanced: Light filtering physically homogenizes the surface morphology, providing a uniform reaction substrate for subsequent chemical treatment; degreasing, pickling, and activation progressively purify the surface, removing oil and impurities, stripping precipitated carbides, and breaking down the inert oxide film, thus eliminating the root cause of corrosion micro-cell hazards and passivation film formation interface barriers; chromium-free passivation and silane sealing together construct a dual-layer protection system, balancing the wear resistance and support of the film layer with its dielectric shielding properties. Through the coordinated efforts of the entire process, it can be implemented directly on existing bearing surface treatment production lines without the need for additional large-scale specialized equipment. It solves the problems of poor corrosion resistance caused by incomplete removal of carbides and difficulty in breaking the inert film in conventional processes, while avoiding dimensional deviations caused by strong corrosion processes. At the same time, the entire process adopts a chromium-free system, eliminating the generation of chromium-based hazardous waste from the source. It combines technical performance, environmental benefits and industrial adaptability, and can increase the neutral salt spray rust-free time of bearing parts to more than 72 hours, with corrosion resistance more than 3 times higher than that of traditional single passivation processes.
[0006] As a further feature of the present invention, the light-passing leveling in step one adopts a two-stage process of rough polishing and fine polishing, with the rough polishing time being 30 minutes and the fine polishing time being 20 minutes.
[0007] The beneficial effects of this setup are as follows: The large amount of grinding in the rough polishing stage rapidly weakens the raised morphology of Cr7C3 carbides on the surface of G65Cr14Mo and 65Cr13 stainless steel, while effectively removing machining defects such as tool marks and burrs from complex structures like bearing chamfers, sealing grooves, and raceways, significantly reducing the macroscopic surface roughness. Then, the fine polishing stage further homogenizes the surface micromorphology, smoothing out the fine scratches left by the rough polishing, resulting in a highly smooth and consistent reaction substrate surface. This two-stage parameter combination ensures sufficient removal of surface defects while avoiding dimensional deviations and surface deformation damage caused by over-grinding. After this process, the surface roughness fluctuation of the bearing can be controlled within 0.05μm, effectively preventing localized current concentration and over-corrosion caused by uneven surfaces during subsequent pickling. It also reduces the retention and accumulation of corrosive media in surface pits under salt spray conditions, lowering the probability of corrosion from a physical morphology perspective and providing a stable and uniform reaction interface for subsequent chemical treatment processes.
[0008] As a further feature of the present invention, the composite alkaline degreasing solution in step two comprises, by mass percentage: 10%~30% potassium carbonate, 2%~5% ethylenediaminetetraacetic acid, 2%~5% C9-C11 alkyl alcohol polyether, with the remainder being deionized water; the degreasing temperature is 50~60℃, and the soaking time is 10~12 minutes; after degreasing, the solution is rinsed twice with tap water.
[0009] The beneficial effects of this setup are as follows: Through the synergistic effect of potassium carbonate, ethylenediaminetetraacetic acid (EDTA), and C9-C11 alkyl alcohol polyethers, highly efficient and thorough removal of various types of contaminants from the bearing surface is achieved. Potassium carbonate provides a strongly alkaline environment, removing animal and vegetable oil stains through saponification. EDTA, as a metal complexing agent, can complex residual metal powder and free metal ions on the surface, preventing them from adhering to the surface and interfering with subsequent film-forming reactions. C9-C11 alkyl alcohol polyethers, as nonionic surfactants, have excellent emulsifying and penetrating capabilities, quickly penetrating to the interface between the oil stains and the substrate, and stripping away mineral oil contaminants such as cutting oil, polishing paste, and residual polishing fluid through emulsification. Combined with a treatment temperature of 50-60℃ and a soaking time of 10-12 minutes, the rate and thoroughness of the degreasing reaction are ensured, while avoiding slight oxidation and alkaline corrosion of the substrate surface caused by excessively high temperatures or prolonged soaking times. After treatment, the workpiece is soaked and cleaned twice with tap water to ensure that the water film on the surface is continuous, without film breakage or water residue, providing a clean reaction interface for subsequent pickling and activation processes, and avoiding defects such as pinholes in the passivation film and poor adhesion caused by impurities.
[0010] As a further feature of the present invention, the nitric acid-hydrofluoric acid composite pickling solution in step three comprises, by mass percentage: 2%~15% nitric acid, 0.1%~1.0% hydrofluoric acid, 1%~6% corrosion inhibitor, and the remainder is deionized water; the pickling temperature is 25~35℃, and the treatment time is 0.5~1.0 min; after pickling, the solution is rinsed twice with tap water.
[0011] The beneficial effects of this setup are: nitric acid, as an oxidizing acid, can preferentially etch the interface between the carbide and the substrate, oxidizing and loosening the carbide structure, while simultaneously dissolving the iron-rich phase on the surface, creating conditions for carbide exfoliation; the F produced by the dissociation of hydrofluoric acid... - Can react with dissolved Cr 3+ Fe 3+ A stable complex is formed, disrupting the dissolution equilibrium at the interface and promoting the overall detachment of Cr7C3 carbides and free carbon from the substrate surface. The carbide removal rate can reach over 85%, eliminating the potential for corrosion micro-cells formed by carbides and the substrate at the source. Simultaneously, 1%–6% corrosion inhibitor is added to the system, selectively adsorbing onto the substrate surface and inhibiting excessive dissolution of the substrate. Combined with a temperature of 25–35°C and a short treatment time of 0.5–1.0 min, the dimensional corrosion rate in a single process is controlled at the sub-micron level. This ensures both sufficient carbide removal and effective control of overall dimensional changes, meeting the micron-level dimensional tolerance requirements of precision bearings.
[0012] As a further feature of the present invention, in step four, the hydrochloric acid-organic acid composite activation solution comprises, by mass percentage: 2%~18% hydrochloric acid, 2%~5% organic acid, and the remainder is deionized water; the activation treatment temperature is 25~35℃, and the treatment time is 0.5~1.0 min; after activation, the solution is rinsed twice with tap water.
[0013] The beneficial effects of this setup are: Addressing the characteristic of high-chromium stainless steel that readily and rapidly regenerates a Cr2O3 inert oxide film after pickling, homogeneous and gentle activation is achieved through the combination of hydrochloric acid and organic acids: hydrochloric acid provides a high concentration of H+. +This process can rapidly etch away thin oxide films and floating rust on the surface, breaking down the inert oxide film barrier and exposing fresh and uniform active sites on the substrate surface. The organic acid acts as a pH buffer, smoothing acidity fluctuations and slowing the etching rate to prevent surface roughness deterioration and dimensional deviations caused by localized over-etching. Furthermore, it acts as a complexing agent, complexing free chromium ions on the surface, reducing the chromium ion concentration at the interface, inhibiting rapid secondary passivation after activation, and ensuring uniform and stable surface activity before passivation. Combined with a temperature of 25–35°C and processing parameters of 0.5–1.0 min, uniform surface activation can be achieved with minimal etching, eliminating the obstruction of the inert film to subsequent passivation film formation and providing a consistent active substrate for uniform passivation film growth. This effectively avoids defects such as uneven passivation film formation, high porosity, and poor adhesion.
[0014] As a further feature of the present invention, the chromium-free passivation solution in step five comprises, by mass percentage: 5%~10% orthophosphoric acid, 5%~10% manganese dihydrogen phosphate, 3%~8% nickel sulfate, with the remainder being deionized water; the passivation treatment temperature is 90~95℃, and the treatment time is 10~12 min; after passivation, the solution is rinsed twice with tap water.
[0015] The beneficial effects of this setup are as follows: A composite system of orthophosphoric acid, manganese dihydrogen phosphate, and nickel sulfate is used to construct a chromium-free manganese-nickel composite phosphate passivation film, completely replacing traditional chromate passivation and preventing the generation of chromium-based pollutants such as hexavalent chromium from the source. Orthophosphoric acid provides the acidic environment required for passivation film formation, promoting the micro-dissolution of the base metal and the deposition of phosphate film, ensuring the adhesion between the film and the substrate. Manganese dihydrogen phosphate provides manganese ions, serving as the main metal source for film formation and constructing the main framework of the phosphate film, forming an inorganic protective layer with a certain thickness and hardness, providing basic wear-resistant and corrosion-resistant support for bearings. Nickel sulfate introduces nickel ions, which can participate in the film formation process to refine the film grains, fill micropores and gap defects in the film, and significantly improve the film density, film-substrate adhesion, and pitting corrosion resistance. With a film-forming temperature of 90~95℃ and a processing time of 10~12min, a continuous, dense, and strongly bonded manganese-nickel composite phosphate inorganic passivation film can be formed on the activated uniform substrate surface, serving as the inorganic anti-corrosion substrate for the entire protection system.
[0016] As a further provision of the present invention, the silane sealing agent in step six comprises, by mass percentage: 2.0%~20.0% carboxylic acid amine salt, 2.0%~10.0% sodium sulfonate, 1.0%~5.0% vinyltrimethoxysilane, with the balance being deionized water; the sealing treatment involves immersing at room temperature for 2~3 minutes, draining, and then baking for curing at a temperature of 80~90℃ for 10~15 minutes.
[0017] The beneficial effects of this setup are as follows: Through the synergistic effect of carboxylic acid amine salt, sodium sulfonate, and vinyltrimethoxysilane, a dense organic sealing layer is formed on the outside of the inorganic passivation film, constructing a composite protective structure of inorganic anti-corrosion substrate combined with organic sealing barrier. Vinyltrimethoxysilane, as the core film-forming substance, can hydrolyze to produce silanol groups, which form hydrogen bonds with the hydroxyl groups on the surface of the passivation film and further dehydrate and crosslink to form a three-dimensional network of organosilicon film, effectively sealing the micropores, gaps, and other defects of the passivation film and blocking the penetration path of corrosive media. Carboxylic acid amine salt and sodium sulfonate, as additives, can improve the stability and wettability of the silane solution, promote the uniform spreading and adhesion of silane on the surface of the passivation film, and enhance the uniformity and bonding force of the sealing layer. Combined with an adsorption process of immersion at room temperature for 2-3 minutes and a baking and curing process at 80-90℃ for 10-15 minutes, the silane can be fully cross-linked and cured to form a firmly bonded and highly shielding organic sealing layer. This layer works synergistically with the inner inorganic passivation film to significantly improve the film's resistance to salt spray and media penetration, ultimately achieving a multiple-fold improvement in the corrosion resistance of bearing parts. Attached Figure Description
[0018] Figure 1 This is a flowchart illustrating the routes of three embodiments of the present invention; Figure 2 The surface morphology of the part after a 0-hour neutral salt spray test following conventional environmentally friendly passivation process. Figure 3 The surface morphology of the part after a 24-hour neutral salt spray test following conventional environmentally friendly passivation process. Figure 4 These are surface morphology images of parts after 0 hours of neutral salt spray testing following treatment in three embodiments of the present invention. Figure 5 The images show the surface morphology of parts after 72 hours of neutral salt spray testing following treatment in three embodiments of the present invention. Detailed Implementation
[0019] The first embodiment of the chromium-free composite treatment process for stainless steel bearing surface treatment of the present invention includes the following steps. This embodiment deals with bearing ring parts made of G65Cr14Mo material, and performs the following steps in sequence: Step 1, Polishing and Leveling: A two-stage polishing process of 30 minutes of rough polishing and 20 minutes of fine polishing is used to grind the bearing rings.
[0020] Step 2, alkaline degreasing: Immerse the parts after polishing in a composite alkaline degreasing solution. The degreasing solution consists of the following components by mass percentage: 20% potassium carbonate, 3% EDTA, 3% C9-C11 alkyl alcohol polyether, and the remainder is deionized water. The treatment temperature is 55℃, and the soaking time is 11 minutes. After treatment, rinse twice with tap water.
[0021] Step 3, composite pickling: Use nitric acid-hydrofluoric acid composite pickling solution, which is composed of 8% nitric acid, 0.5% hydrofluoric acid, 3% imidazoline corrosion inhibitor, and the remainder is deionized water by mass percentage; the treatment temperature is 30℃, and the pickling time is 0.8min; after treatment, soak and rinse twice with tap water.
[0022] Step 4, Composite Activation: Use hydrochloric acid-organic acid composite activation solution, which is: 10% hydrochloric acid, 3% citric acid, and the remainder is deionized water by mass percentage; the treatment temperature is 30℃ and the activation time is 0.8min; after treatment, soak and rinse twice with tap water.
[0023] Step 5, Chromium-free passivation: The chromium-free passivation solution consists of the following components by mass percentage: 8% phosphoric acid, 7% manganese dihydrogen phosphate, 5% nickel sulfate, and the remainder is deionized water; the treatment temperature is 92℃, and the passivation time is 11 minutes; after treatment, the sample is rinsed twice with tap water.
[0024] Step 6, Silane sealing: The silane sealing agent is composed of the following by mass percentage: 10% carboxylic acid amine salt, 5% sodium sulfonate, 3% vinyltrimethoxysilane, and the remainder is deionized water; soak at room temperature for 2.5 minutes, drain, and then bake at 85°C for 12 minutes to cure.
[0025] The performance of the parts processed in this embodiment was tested: the removal rate of Cr7C3 carbides on the surface was 88%; the total dimensional change of the entire process was 0.7μm, and the roughness fluctuation was 0.03μm; the neutral salt spray test according to GB / T10125 showed that the rust-free time was 78h, and there was no pitting corrosion on the surface.
[0026] A second embodiment of the chromium-free composite treatment process for the surface treatment of stainless steel bearings of the present invention includes the following steps: Step 1, Light Leveling: A two-stage light leveling process is adopted, consisting of 30 minutes of rough polishing and 20 minutes of fine polishing.
[0027] Step 2, alkaline degreasing: The degreasing solution consists of the following components by mass percentage: 10% potassium carbonate, 2% EDTA, 2% C9-C11 alkyl alcohol polyether, and the remainder is deionized water; the treatment temperature is 50℃, and the soaking time is 10 minutes; after treatment, the product is rinsed twice with tap water.
[0028] Step 3, composite pickling: The pickling solution consists of the following components by mass percentage: 2% nitric acid, 0.1% hydrofluoric acid, 1% thiourea corrosion inhibitor, and the remainder is deionized water; the treatment temperature is 25℃, and the pickling time is 0.5 min; after treatment, the solution is rinsed twice with tap water.
[0029] Step 4, Composite Activation: The activation solution consists of 2% hydrochloric acid and 2% tartaric acid by mass percentage, with the remainder being deionized water; the treatment temperature is 25℃, and the activation time is 0.5 min; after treatment, the solution is rinsed twice with tap water.
[0030] Step 5, Chromium-free passivation: The passivation solution consists of the following components by mass percentage: 5% orthophosphoric acid, 5% manganese dihydrogen phosphate, 3% nickel sulfate, with the remainder being deionized water; the treatment temperature is 90℃, and the passivation time is 10 minutes; after treatment, the sample is rinsed twice with tap water.
[0031] Step 6, Silane sealing: The sealing agent by mass percentage is: 2.0% carboxylic acid amine salt, 2.0% sodium sulfonate, 1.0% vinyltrimethoxysilane, and the balance is deionized water; soak at room temperature for 2 minutes, drain, and then bake at 80℃ for 10 minutes to cure.
[0032] The performance of the parts processed in this embodiment was tested: the removal rate of Cr7C3 carbides on the surface was 86%; the total dimensional change of the entire process was 0.5μm, the roughness fluctuation was 0.02μm; the rust-free time in the neutral salt spray test was 75h, and there was no pitting corrosion on the surface.
[0033] The third embodiment of the chromium-free composite treatment process for stainless steel bearing surface treatment of the present invention includes the following steps: Step 1, Light Leveling: A two-stage light leveling process is adopted, consisting of 30 minutes of rough polishing and 20 minutes of fine polishing.
[0034] Step 2, alkaline degreasing: The degreasing solution consists of the following components by mass percentage: 30% potassium carbonate, 5% EDTA, 5% C9-C11 alkyl alcohol polyether, and the remainder is deionized water; the treatment temperature is 60℃, and the soaking time is 12 minutes; after treatment, the product is rinsed twice with tap water.
[0035] Step 3, composite pickling: The pickling solution consists of the following components by mass percentage: 15% nitric acid, 1.0% hydrofluoric acid, 6% imidazoline corrosion inhibitor, and the remainder is deionized water; the treatment temperature is 35℃, and the pickling time is 1.0 min; after treatment, the solution is rinsed twice with tap water.
[0036] Step 4, Composite Activation: The activation solution consists of 18% hydrochloric acid, 5% citric acid, and the remainder is deionized water by mass percentage; the treatment temperature is 35℃, and the activation time is 1.0 min; after treatment, the solution is rinsed twice with tap water.
[0037] Step 5, Chromium-free passivation: The passivation solution consists of the following components by mass percentage: 10% phosphoric acid, 10% manganese dihydrogen phosphate, 8% nickel sulfate, and the remainder is deionized water; the treatment temperature is 95℃, and the passivation time is 12 minutes; after treatment, the sample is rinsed twice with tap water.
[0038] Step 6, Silane sealing: The sealing agent by mass percentage is: 20.0% carboxylic acid amine salt, 10.0% sodium sulfonate, 5.0% vinyltrimethoxysilane, and the balance is deionized water; soak at room temperature for 3 minutes, drain, and then bake at 90℃ for 15 minutes to cure.
[0039] The performance of the parts processed in this embodiment was tested: the removal rate of Cr7C3 carbides on the surface was 90%; the total dimensional change of the entire process was 0.9μm, the roughness fluctuation was 0.04μm; the rust-free time in the neutral salt spray test was 82h, and there was no pitting corrosion on the surface.
[0040] In comparison, the same batch of G65Cr14Mo bearing ring parts were treated using a conventional single environmentally friendly chromium-free passivation process, which only involved degreasing, conventional pickling, activation, and a single chromium-free passivation step, without any light leveling or silane sealing treatment.
[0041] Testing revealed that the removal rate of Cr7C3 carbides on the surface of the parts was 52%; the total dimensional change over the entire process was 1.8 μm; and obvious rust and pitting defects appeared on the surface of the parts after 22 hours of neutral salt spray testing.
[0042] As can be seen from the comparison of the embodiments and comparative examples, the chromium-free composite treatment process of the present invention can significantly improve the carbide removal effect, accurately control the dimensional accuracy of bearing parts, and improve the corrosion resistance by more than 3 times compared with conventional processes, thus possessing excellent comprehensive protection performance and industrial application value.
[0043] The above examples are merely one preferred embodiment of the present invention. Ordinary variations and substitutions made by those skilled in the art within the scope of the technical solution of the present invention are all included within the protection scope of the present invention.
Claims
1. A chromium-free composite treatment process for stainless steel bearing surface treatment, characterized by, Includes the following steps: Step 1, Light-drilling: The stainless steel bearing parts are subjected to light-drilling treatment. The stainless steel bearing parts are made of G65Cr14Mo or 65Cr13 high carbon chromium martensitic stainless steel. This weakens the surface carbide protrusions and burr defects, and obtains a uniform reactive substrate. Step 2, alkaline degreasing: Immerse the polished bearing parts in a composite alkaline degreasing solution to remove surface oil and impurities; Step 3, composite pickling: The degreased bearing parts are pickled using a nitric acid-hydrofluoric acid composite pickling solution to remove the Cr7C3 carbides, free carbon and iron-rich phases precipitated on the surface. Step 4, Composite Activation: The pickled bearing parts are activated using a hydrochloric acid-organic acid composite activation solution to break the surface Cr2O3 inert oxide film and inhibit secondary passivation. Step 5, Chromium-free passivation: The activated bearing parts are passivated using a chromium-free passivation solution to form a manganese-nickel composite phosphate inorganic passivation film on the surface; Step 6, silane sealing: The passivated bearing parts are sealed with silane sealant and baked to cure, forming an organic silicon sealing layer on the outside of the inorganic passivation film, and finally constructing a double-layer protective film system.
2. A chromium-free composite treatment process for stainless steel bearing surface treatment as claimed in claim 1, wherein: In step one, the light-passing leveling adopts a two-stage process of rough polishing and fine polishing, with the rough polishing time being 30 minutes and the fine polishing time being 20 minutes.
3. A chromium-free composite treatment process for stainless steel bearing surface treatment as claimed in claim 1, wherein: In step two, the composite alkaline degreasing solution consists of the following components by mass percentage: 10%~30% potassium carbonate, 2%~5% ethylenediaminetetraacetic acid, 2%~5% C9-C11 alkyl alcohol polyether, and the remainder is deionized water; the degreasing temperature is 50~60℃, and the soaking time is 10~12 minutes; after degreasing, the product is rinsed twice with tap water.
4. A chromium-free composite treatment process for stainless steel bearing surface treatment as claimed in claim 1, wherein: In step three, the nitric acid-hydrofluoric acid composite pickling solution consists of the following components by mass percentage: 2%~15% nitric acid, 0.1%~1.0% hydrofluoric acid, 1%~6% corrosion inhibitor, and the remainder is deionized water; the pickling temperature is 25~35℃, and the treatment time is 0.5~1.0 min; after pickling, the solution is rinsed twice with tap water.
5. A chromium-free composite treatment process for stainless steel bearing surface treatment as claimed in claim 1, wherein: In step four, the hydrochloric acid-organic acid composite activation solution consists of the following components by mass percentage: 2%~18% hydrochloric acid, 2%~5% organic acid, and the remainder is deionized water; the activation temperature is 25~35℃, and the treatment time is 0.5~1.0 min; after activation, the solution is rinsed twice with tap water.
6. A chromium-free composite treatment process for stainless steel bearing surface treatment as claimed in claim 1, wherein: In step five, the chromium-free passivation solution consists of the following components by mass percentage: 5%~10% orthophosphoric acid, 5%~10% manganese dihydrogen phosphate, 3%~8% nickel sulfate, with the remainder being deionized water; the passivation temperature is 90~95℃, and the treatment time is 10~12 minutes; after passivation, the sample is rinsed twice with tap water.
7. A chromium-free composite treatment process for stainless steel bearing surface treatment as claimed in claim 1, wherein: In step six, the silane sealing agent, by mass percentage, comprises: 2.0%~20.0% carboxylic acid amine salt, 2.0%~10.0% sodium sulfonate, 1.0%~5.0% vinyltrimethoxysilane, with the balance being deionized water; the sealing treatment involves immersing at room temperature for 2~3 minutes, draining, and then baking for curing at a temperature of 80~90℃ for 10~15 minutes.