Chromium-free antioxidant composition, preparation method thereof, composite copper foil and application

Through the treatment of chromium-free antioxidant composition, the complex surface treatment and environmental pollution of traditional lithium battery copper foil are solved, and high-temperature stability and environmentally friendly antioxidant effects are achieved. It is suitable for lithium-ion batteries and printed circuit boards.

CN118996427APending Publication Date: 2024-11-22WG TECH(JIANGXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040145.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The surface treatment process of traditional lithium battery copper foil is complex and prone to quality problems. The chromium anti-oxidation liquid used is harmful to the environment and is difficult to meet the market's requirements for low chromium content and no impurity elements.

Method used

A chromium-free antioxidant composition, including non-ionic surfactants, inorganic salts, glycerin and corrosion inhibitors, is used to prepare an antioxidant layer by mixing and mixing with the copper foil to prepare a surface treatment, replacing the traditional chrome plating technology.

Benefits of technology

It achieves good anti-oxidation and discoloration ability of copper foil under high temperature conditions, reduces production costs, complies with environmental protection standards, and improves product stability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a chromium-free anti-oxidation composition and a preparation method thereof, a composite copper foil and application, the components of the chromium-free anti-oxidation composition are designed, and the proportion of the components is reasonably adjusted, so that the components synergistically play a role after reasonable compatibility; and finally, the chromium-free antioxidant composition with main raw materials including a nonionic surfactant, inorganic salt, glycerol, a corrosion inhibitor and water is prepared. Meanwhile, experimental verification shows that after the composite copper foil is treated by the chromium-free antioxidant composition, the composite copper foil still does not change color after being placed in an air circulation type high-temperature oven and continuously heated at 150 DEG C for 30 minutes, and the chromium-free antioxidant composition shows good performance stability and excellent antioxidant discoloration capability and meets the use requirements of related enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of copper foil preparation, and in particular to a chromium-free antioxidant composition and a preparation method thereof, a composite copper foil and applications. Background Art

[0002] In recent years, with the active support and promotion of the new energy industry by the state, the lithium-ion power battery industry has ushered in a booming development. As one of its key components, lithium battery copper foil has been widely used in the market as the negative electrode current collector of lithium-ion batteries. The market demand and lithium battery copper foil production capacity have both shown a trend of synchronous increase. At the same time, the market's quality standards for lithium battery copper foil are becoming increasingly stringent, with particular emphasis on the ability of lithium battery copper foil to resist oxidation and discoloration in high temperature environments.

[0003] In traditional technology, in order to improve the anti-oxidation ability of lithium battery copper foil, complex surface treatment steps are used during the anti-oxidation process: including roughening, curing, pickling, washing, galvanizing, nickel plating and other links. The surface treatment process is not only lengthy, but also prone to quality problems such as folding, bumps, and pits during the continuous winding process of surface treatment, thereby reducing production efficiency and increasing manufacturing costs. The thickness of lithium battery copper foil on the market is mainly concentrated in 6μm-8μm, and these fine products are more easily damaged during the surface treatment process.

[0004] The existing integrated foil production machines mainly use chromium liquid passivation technology, which is rolled up after drying and then cut into finished products. However, the chromium anti-oxidation liquid mainly contains hexavalent chromium, which poses a serious threat to human health and has a potential carcinogenic risk. Due to the improvement of environmental awareness and the tightening of environmental protection regulations in recent years, the emission standards of chromium liquid have become increasingly stringent. The cost of chromium-containing anti-oxidation liquid discharge and treatment is high, and it is easy to cause serious pollution to water bodies and soil. In addition, manufacturers using lithium battery copper foil have higher requirements for product quality, expecting the chromium content on the surface of the copper foil to be as low as possible, and to contain no impurity elements such as nickel and zinc. This makes it difficult for traditional chrome plating anti-oxidation technology to meet the use requirements of related companies. Summary of the invention

[0005] Based on this, it is necessary to provide a chromium-free antioxidant composition and a preparation method thereof, a composite copper foil and an application thereof. The composite copper foil treated with the chromium-free antioxidant composition has the ability to resist oxidation and discoloration.

[0006] The technical solution of this application is as follows:

[0007] In a first aspect of the present invention, a chromium-free antioxidant composition is provided, wherein raw materials thereof include a nonionic surfactant, an inorganic salt, glycerol and a corrosion inhibitor in a mass ratio of (1-10): (0.1-1): (1-2): (0.1-2).

[0008] In one embodiment, the nonionic surfactant is an alkylphenol ether surfactant;

[0009] Optionally, the alkylphenol ether surfactant includes one or more of nonylphenol polyoxyethylene ether and octylphenol polyoxyethylene ether.

[0010] In one embodiment, the corrosion inhibitor is an azole corrosion inhibitor;

[0011] Optionally, the azole corrosion inhibitor includes 5-aminotetrazodone.

[0012] In one embodiment, the inorganic salt is phosphate;

[0013] Optionally, the phosphate comprises trisodium phosphate.

[0014] In one embodiment, the raw materials of the chromium-free antioxidant composition include a non-ionic surfactant, an inorganic salt, glycerol and a corrosion inhibitor in a mass ratio of (2-7): (0.2-0.5): (1.5-1.8): (0.5-1).

[0015] The second aspect of the present invention provides a method for preparing the chromium-free antioxidant composition as described above, comprising the following steps:

[0016] The nonionic surfactant, inorganic salt, glycerin, corrosion inhibitor and water are mixed and stirred.

[0017] In one embodiment, the stirring time is 0.5h-2h; and / or

[0018] The stirring temperature is room temperature.

[0019] A third aspect of the present invention provides a method for preparing a composite copper foil, comprising the following steps:

[0020] The chromium-free antioxidant composition as described above is mixed with water and stirred, and a copper foil is immersed in the obtained mixed solution to prepare an antioxidant layer on the surface of the copper foil, which is then taken out and blown dry.

[0021] A fourth aspect of the present invention provides a composite copper foil prepared according to the method for preparing the composite copper foil as described above.

[0022] A fifth aspect of the present invention provides use of the composite copper foil as described above in the preparation of lithium-ion batteries or printed circuit boards.

[0023] Compared with the prior art, this application has the following beneficial effects:

[0024] The present application designs the components of the chromium-free antioxidant composition and reasonably adjusts the proportions of the components so that the components can work synergistically after reasonable compatibility, and finally obtains a chromium-free antioxidant composition whose main raw materials include non-ionic surfactants, inorganic salts, glycerin, corrosion inhibitors and water. At the same time, it was found through experimental verification that the composite copper foil treated with the chromium-free antioxidant composition of the present application did not change color when placed in an air-circulating high-temperature oven and continuously heated at 150°C for 30 minutes, showing good performance stability, excellent anti-oxidation and discoloration ability, and meeting the use requirements of relevant companies. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] Figure 1 The process flow chart of composite copper foil in one embodiment is shown in FIG. DETAILED DESCRIPTION

[0027] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0029] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0030] As used herein, "one or more" refers to any one, any two, or any two or more of the listed items.

[0031] Herein, the optional scope of "and / or", "or / and", and "and / or" includes any one of two or more relevant listed items, and also includes any and all combinations of the relevant listed items, wherein said any and all combinations include any two relevant listed items, any more relevant listed items, or a combination of all relevant listed items. (It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in the present application, the technical solution undoubtedly includes technical solutions that are all connected by "logical AND", and also undoubtedly includes technical solutions that are all connected by "logical OR". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For another example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, technical solutions that are all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, a combination of any two or any three of A, B, C, and D, and also includes a combination of four items of A, B, C, and D (that is, a technical solution that is all connected by "logical AND").)

[0032] Herein, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0033] Herein, "first aspect", "second aspect", "third aspect", "fourth aspect", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. In addition, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0034] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0035] Specifically, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each individually disclosed point or single value itself can be combined with any other point or single value as a lower limit or upper limit or with other lower limits or upper limits to form an undefined range. The use of numerical ranges represented by endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0036] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.

[0037] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.

[0038] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±2°C, ±1°C, ±0.5°C, ±0.4°C, ±0.3°C, ±0.2°C, and ±0.1°C are allowed. Normal temperature or room temperature in this application refers to no temperature control operation, generally 4°C~35°C, preferably 20±5°C.

[0039] At present, in the market, most of the preparation process of lithium batteries uses electrolytic copper foil. As a functional key basic raw material in the electronic information industry, the application scope of electrolytic copper foil is mainly concentrated in the manufacture of lithium-ion batteries and printed circuit boards (PCBs). However, there is a significant problem with electrolytic copper foil: it is very easy to undergo oxidation reaction when exposed to air at high temperature or for a long time, which directly affects the performance and stability of the product. Therefore, it is particularly important to carry out necessary antioxidant treatment on electrolytic copper foil. Traditional antioxidant methods mostly rely on chromium plating technology, that is, chromium-plated metal is used during treatment. The dichromium anti-oxidation liquid mainly contains hexavalent chromium, which poses a major threat to the human body, water bodies and soil environment. Its high toxicity has aroused widespread environmental protection concerns. In addition, in order to achieve the standard emission of hexavalent chromium, enterprises need to bear relatively high treatment costs, which not only increases production costs, but also limits the wide application of electrolytic copper foil in many industries. More importantly, even if the emission treatment is carried out, it is difficult to fully meet the strict requirements of many industries for product safety and environmental protection standards.

[0040] Based on this, the first aspect of the present invention provides a chromium-free antioxidant composition, whose raw materials include a non-ionic surfactant, an inorganic salt, glycerol and a corrosion inhibitor in a mass ratio of (1-10): (0.1-1): (1-2): (0.1-2).

[0041] In some examples, the nonionic surfactant is an alkylphenol ether surfactant.

[0042] In some specific examples, the alkylphenol ether surfactant includes one or more of nonylphenol polyoxyethylene ether and octylphenol polyoxyethylene ether.

[0043] In some of the examples, the corrosion inhibitor is an azole corrosion inhibitor.

[0044] In some specific examples, the azole corrosion inhibitor includes 5-aminotetrazodone.

[0045] In some examples, the inorganic salt is a phosphate.

[0046] In some specific examples, the phosphate includes trisodium phosphate.

[0047] In some of the examples, the raw materials of the chromium-free antioxidant composition include a non-ionic surfactant, an inorganic salt, glycerin and a corrosion inhibitor in a mass ratio of (2-7): (0.2-0.5): (1.5-1.8): (0.5-1).

[0048] Specifically, the present application designs the components of the chromium-free antioxidant composition and reasonably adjusts the proportions of the components so that the components work synergistically after reasonable compatibility, and finally obtains a chromium-free antioxidant composition whose main raw materials include non-ionic surfactants, inorganic salts, glycerol, corrosion inhibitors and water. Further, alkylphenol ether surfactants are non-ionic surfactants, and their hydrophilic groups are mainly composed of ether groups with a certain number of oxygen-containing groups. It is this point that determines that non-ionic surfactants are superior to ionic surfactants in some aspects; because they are not in an ionic state in the solution, they have high stability, are not easily affected by the presence of strong electrolyte inorganic salts, are not easily affected by pH values, and have low costs. The phosphorus element in trisodium phosphate reacts chemically with copper metal, loosening and falling off the dirt attached to it, and is used to clean the dirt of composite copper foil, etc. Glycerol has good stability: Glycerol has good chemical stability in metalworking fluids, will not decompose or deteriorate over time, and can maintain stable and consistent performance. More importantly, it has excellent antioxidant properties: glycerol can inhibit the occurrence of metal oxidation reactions, prevent oxidation, corrosion and other phenomena, thereby maintaining the smoothness of the metal surface and the quality of metal products. Azole corrosion inhibitors are mainly 5-aminotetrazolyl, which adsorbs on the copper surface through the N atoms on the tetrazole ring and the N atoms on the amino group to achieve organic coordination, thereby forming a protective film.

[0049] The second aspect of the present invention provides a method for preparing the chromium-free antioxidant composition as described above, comprising the following steps:

[0050] The nonionic surfactant, inorganic salt, glycerin, corrosion inhibitor and water are mixed and stirred.

[0051] In some of these examples, the stirring time is 0.5h-2h. It can be understood that the stirring time includes but is not limited to 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, 2h.

[0052] In some of these examples, the stirring temperature is room temperature. It is understandable that the stirring temperature includes but is not limited to 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C.

[0053] A third aspect of the present invention provides a method for preparing a composite copper foil, comprising the following steps:

[0054] The chromium-free antioxidant composition as described above is mixed with water and stirred, and a copper foil is immersed in the obtained mixed solution to prepare an antioxidant layer on the surface of the copper foil, which is then taken out and blown dry.

[0055] In some specific examples, the method for preparing the composite copper foil comprises the following steps:

[0056] The chromium-free antioxidant composition as described above is mixed with water to prepare a chromium-free antioxidant liquid, the obtained chromium-free antioxidant liquid is mixed with water, stirred, and a copper foil is immersed in the obtained mixed liquid to prepare an antioxidant layer on the surface of the copper foil, which is taken out and blown dry.

[0057] In some examples, the raw materials of the chromium-free antioxidant solution include the following components by mass percentage:

[0058] Non-ionic surfactant 1%-10%, inorganic salt 0.1%-1.0%, glycerin 1.0%-2.0%, corrosion inhibitor 0.1%-2%, and the rest is water.

[0059] In some specific examples, the raw materials of the chromium-free antioxidant solution include the following components by mass percentage:

[0060] Non-ionic surfactant 2%-7%, inorganic salt 0.2%-0.5%, glycerin 1.5%-1.8%, corrosion inhibitor 0.5%-1%, and the rest is water.

[0061] In some examples, the volume ratio of the chromium-free antioxidant solution to water is (50-100) mL: 1 L. It can be understood that the volume ratio of the chromium antioxidant solution to water includes but is not limited to 50 mL: 1 L, 52 mL: 1 L, 54 mL: 1 L, 56 mL: 1 L, 58 mL: 1 L, 60 mL: 1 L, 62 mL: 1 L, 64 mL: 1 L, 66 mL: 1 L, 68 mL: 1 L, 70 mL: 1 L, 72 mL: 1 L, 74 mL: 1 L, 76 mL: 1 L, 78 mL: 1 L, 80 mL: 1 L, 82 mL: 1 L, 84 mL: 1 L, 86 mL: 1 L, 88 mL: 1 L, 90 mL: 1 L, 92 mL: 1 L, 94 mL: 1 L, 96 mL: 1 L, 98 mL: 1 L, 100 mL: 1 L.

[0062] In some examples, in the method for preparing the composite copper foil, the stirring time is 3 minutes to 10 minutes. It is understandable that in the method for preparing the composite copper foil, the stirring time includes but is not limited to 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes, 5.5 minutes, 6 minutes, 6.5 minutes, 7 minutes, 7.5 minutes, 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes, and 10 minutes.

[0063] In some examples, in the method for preparing the composite copper foil, the immersion time is 5s-20s. It can be understood that in the method for preparing the composite copper foil, the immersion time includes but is not limited to 5s, 5.5s, 6s, 6.5s, 7s, 7.5s, 8s, 8.5s, 9s, 9.5s, 10s, 10.5s, 11s, 11.5s, 12s, 12.5s, 13s, 13.5s, 14s, 14.5s, 15s, 15.5s, 16s, 16.5s, 17s, 17.5s, 18s, 18.5s, 19s, 19.5s, and 20s.

[0064] The fourth aspect of the present invention provides a composite copper foil prepared according to the preparation method of the composite copper foil as described above. Composite copper foil refers to a new type of material made by first using vacuum sputtering to make a metal conductive layer on the surface of a plastic film such as PET, PP, PI, and then using aqueous electroplating or other methods to thicken the copper layer to a thickness of 1 micron or more. The weight of composite copper foil is relatively light compared to electrolytic copper foil, which can improve the energy density of the battery, improve the safety of the battery and reduce the material cost. These advantages make composite copper foil expected to become the main material for the negative electrode current collector of lithium batteries in the future.

[0065] A fifth aspect of the present invention provides use of the composite copper foil as described above in the preparation of lithium-ion batteries or printed circuit boards.

[0066] The present application is further described in detail below in conjunction with specific examples. For experimental parameters not specified in the following specific examples, reference is made to the instructions given in the present application document, and reference may also be made to the experimental manual of the art or other experimental methods known in the art, or to the experimental conditions recommended by the manufacturer. It is understood that the instruments and raw materials used in the following examples are relatively specific, and may not be limited thereto in other specific examples.

[0067] The following are specific embodiments.

[0068] Example 1

[0069] Add 4% mass concentration of alkylphenol ether surfactant (nonylphenol polyoxyethylene ether), 0.5% mass concentration of sodium phosphate, 1.6% mass concentration of glycerol, 0.5% mass concentration of azole corrosion inhibitor (5-aminotetrazolyl) and the rest of water into the reactor, mix well, stir at room temperature for 1 hour, and then you can get antioxidant solution 1.

[0070] Example 2

[0071] Add 7% mass concentration of alkylphenol ether surfactant (nonylphenol polyoxyethylene ether), 0.5% mass concentration of sodium phosphate, 1.8% mass concentration of glycerol, 0.5% mass concentration of azole corrosion inhibitor, and the rest of water, add to the reactor, mix well, stir at room temperature for 1 hour, and you can get antioxidant solution 2.

[0072] Example 3

[0073] Add 4% mass concentration of alkylphenol ether surfactant (nonylphenol polyoxyethylene ether), 0.5% mass concentration of sodium phosphate, 1.8% mass concentration of glycerol, 1% mass concentration of azole corrosion inhibitor (5-aminotetrazolyl) and the rest of water, add to the reactor, mix well, stir at room temperature for 1 hour, and then you can get antioxidant solution 3.

[0074] Example 4

[0075] Add 7% mass concentration of alkylphenol ether surfactant (nonylphenol polyoxyethylene ether), 0.2% mass concentration of sodium phosphate, 1.5% mass concentration of glycerol, 0.5% mass concentration of azole corrosion inhibitor (5-aminotetrazolyl) and the rest of water, add to the reactor, mix well, stir at room temperature for 1 hour, and you can get antioxidant solution 4.

[0076] Example 5

[0077] Add 6% by mass of alkylphenol ether surfactant (nonylphenol polyoxyethylene ether), 0.4% by mass of sodium phosphate, 1.6% by mass of glycerol, 0.8% by mass of azole corrosion inhibitor (5-aminotetrazolyl) and the rest of water, add to the reactor, mix well, stir at room temperature for 1 hour, and then you can get antioxidant solution 5.

[0078] Comparative Example 1

[0079] In Comparative Example 1, no antioxidant solution was prepared.

[0080] Comparative Example 2

[0081] The preparation method of Comparative Example 2 is substantially the same as that of Example 1, except that glycerol and sodium phosphate are omitted from the antioxidant solution.

[0082] Comparative Example 3

[0083] The preparation method of Comparative Example 3 is substantially the same as that of Example 1, except that the alkylphenol ether surfactant (nonylphenol polyoxyethylene ether) is omitted in the antioxidant liquid.

[0084] Comparative Example 4

[0085] The preparation method of Comparative Example 4 is substantially the same as that of Example 1, except that the azole corrosion inhibitor (5-aminotetrazolyl) is omitted in the antioxidant solution.

[0086] The antioxidant solutions prepared in Examples 1 to 5 and Comparative Examples 2 to 4 and the composite copper foil in Comparative Example 1 were subjected to antioxidant treatment.

[0087] The preparation process of composite copper foil treated with antioxidant solution is as follows: Figure 1 As shown, the specific steps are as follows: take 50-100mL of the above antioxidant solution and add it to 1L of pure water, stir and disperse for 5 minutes, soak the copper foil in the antioxidant solution for 10s, take it out, remove the residual antioxidant solution on the surface and blow it dry with an air knife to obtain a composite copper foil.

[0088] The prepared composite copper foil was then subjected to performance tests, and the test results are shown in Table 1 below.

[0089] Table 1

[0090]

[0091] As can be seen from Table 1 above, the composite copper foil treated with the antioxidant solution of this embodiment does not change color when placed in an air circulation high-temperature oven and continuously heated at 150°C for 30 minutes, showing good performance stability, excellent antioxidant discoloration ability and meeting the use requirements of relevant companies. Without the antioxidant solution treatment or lacking a certain component in the antioxidant solution, oxidation blackening will occur.

[0092] In summary, the present application designs the components of the chromium-free antioxidant liquid composition and reasonably adjusts the proportions of the components so that the components can work synergistically after reasonable compatibility, and finally obtains a chromium-free antioxidant composition whose main raw materials include non-ionic surfactants, inorganic salts, glycerin, corrosion inhibitors and water. At the same time, it was found through experimental verification that after the composite copper foil was treated with the chromium-free antioxidant composition of the present application, it was placed in an air-circulating high-temperature oven and heated continuously for 30 minutes at 150°C without changing color, showing good performance stability, excellent anti-oxidation and discoloration ability, and meeting the use requirements of relevant companies.

[0093] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0094] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.

Claims

1. A chromium-free antioxidant composition, It is characterized in that The raw materials include non-ionic surfactant, inorganic salt, glycerin and corrosion inhibitor in a mass ratio of (1-10): (0.1-1): (1-2): (0.1-2).

2. The chromium-free antioxidant composition according to claim 1, It is characterized in that The nonionic surfactant is an alkylphenol ether surfactant; Optionally, the alkylphenol ether surfactant includes one or more of nonylphenol polyoxyethylene ether and octylphenol polyoxyethylene ether.

3. The chromium-free antioxidant composition according to claim 1, It is characterized in that The corrosion inhibitor is an azole corrosion inhibitor; Optionally, the azole corrosion inhibitor includes 5-aminotetrazodone.

4. The chromium-free antioxidant composition according to claim 1, It is characterized in that The inorganic salt is phosphate; Optionally, the phosphate comprises trisodium phosphate.

5. The chromium-free antioxidant composition according to any one of claims 1 to 4, It is characterized in that The raw materials include non-ionic surfactant, inorganic salt, glycerin and corrosion inhibitor in a mass ratio of (2-7): (0.2-0.5): (1.5-1.8): (0.5-1).

6. A method for preparing the chromium-free antioxidant composition according to any one of claims 1 to 5, It is characterized in that The following steps are involved: The nonionic surfactant, inorganic salt, glycerin, corrosion inhibitor and water are mixed and stirred.

7. The method for preparing the chromium-free antioxidant composition according to claim 6, It is characterized in that The stirring time is 0.5h-2h; and / or The stirring temperature is room temperature.

8. A method for preparing a composite copper foil, It is characterized in that The steps include: The chromium-free antioxidant composition according to any one of claims 1 to 5 is mixed with water, stirred, and a copper foil is immersed in the obtained mixed solution to prepare an antioxidant layer on the surface of the copper foil, which is then taken out and blown dry.

9. A composite copper foil prepared according to the method for preparing a composite copper foil according to claim 8.

10. Use of the composite copper foil according to claim 9 in the preparation of lithium ion batteries or printed circuit boards.