A Citric Acid-Controlled Electrolytic Manganese Dioxide Preparation and Post-treatment Modification Process

By using citric acid-controlled electrolytic manganese dioxide preparation and post-treatment modification processes, the problems of insufficient purity and dispersibility of EMD were solved, resulting in high-purity and highly dispersible EMD products. This improved electrochemical performance and process controllability, making it suitable for large-scale industrial production.

CN123108581APending Publication Date: 2026-11-17GUANGXI DAXIN HUIYUAN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611346913.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, the compatibility of citric acid in the post-processing stage is not considered in the preparation of electrolytic manganese dioxide (EMD), resulting in insufficient purity and dispersibility of EMD, crystal distortion, and the formation of impurity phases. This makes it difficult to meet the synthesis requirements of cathode materials such as lithium manganese oxide, and the process controllability is poor, making it difficult to achieve industrial-scale mass production.

Method used

By employing a citric acid-based electrolytic manganese dioxide preparation and post-treatment modification process, low-concentration citric acid is used in the electrolyte for complexation regulation. Combined with interfacial adsorption and pH buffering in post-treatment, electrolysis and post-treatment parameters are controlled to generate a defect distribution map. The concentration of citric acid is dynamically adjusted to carry out dispersion modification treatment, resulting in a high-purity and highly dispersible EMD product.

Benefits of technology

It achieves high purity and high dispersibility of EMD, improves electrochemical performance, solves the problems of crystal distortion and impurity phase formation, ensures process controllability and product consistency, and is suitable for industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108581A_ABST
    Figure CN123108581A_ABST
Patent Text Reader

Abstract

This invention relates to the field of electrolytic manganese dioxide preparation technology, specifically disclosing a citric acid-controlled process for the preparation and post-processing modification of electrolytic manganese dioxide. The process includes: preparing a basic electrolyte solution with citric acid added to regulate its concentration; electrolyzing, washing, and drying to obtain crude manganese dioxide; dispersing and modifying the crude product with an aqueous citric acid solution, ball milling and centrifuging, followed by washing, drying, calcination, and grinding to obtain a refined product. Furthermore, this invention establishes a method for consistent control of the nucleation environment. By acquiring cross-sectional physical parameters to generate a defect distribution map, the level of deposition defects is identified to match the corresponding citric acid compensation concentration range; the optimal penetration characteristic depth is determined by combining the permeable stratum range; and the combination of feedforward parameters is analyzed to achieve dynamic control of layered modification and convergence. This process helps alleviate problems such as easy crystal distortion and process disconnection, improving the high purity and batch performance consistency of manganese dioxide products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrolytic manganese dioxide preparation technology, specifically to a process for preparing and modifying electrolytic manganese dioxide based on citric acid regulation. Background Technology

[0002] In existing technologies, organic acid additives are often used in the electrolytic preparation of electrolytic manganese dioxide (EMD), but they have the following core defects: Existing studies only focus on the effect of citric acid in the electrolyte on EMD, without considering the adaptation role of citric acid in the EMD post-processing stage, resulting in insufficient purity and dispersibility of EMD, which cannot meet the synthesis requirements of subsequent cathode materials such as lithium manganese oxide; There is no clear optimal range for the concentration of citric acid and the pH control of the electrolyte, which easily leads to EMD crystal distortion and impurity phase formation, resulting in discharge performance degradation and poor high-temperature storage stability.

[0003] Furthermore, the EMD electrolysis and post-processing processes are disconnected, there are no clear rules for concentration matching, the process controllability is poor, it is difficult to achieve industrial-scale mass production, and the product performance consistency is low.

[0004] Therefore, the present invention provides a process for preparing and modifying electrolytic manganese dioxide based on citric acid regulation. Summary of the Invention

[0005] The purpose of this invention is to provide a citric acid-controlled process for the preparation and post-processing modification of electrolytic manganese dioxide, which solves the problems of easy distortion of EMD crystal form, unstable performance, process disconnect, and difficulty in mass production in the prior art, and obtains EMD products with high purity, high dispersibility, and high electrochemical activity.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] A process for preparing and modifying electrolytic manganese dioxide based on citric acid includes the following steps:

[0008] Prepare a sulfuric acid-manganese sulfate basic electrolyte by adding citric acid as an additive and controlling the concentration of citric acid;

[0009] Electrolysis was performed using a titanium-manganese alloy plate as the anode and a copper tube as the cathode. After electrolysis, the anode product was stripped off, washed, and dried to obtain crude manganese dioxide.

[0010] The cross-sectional physical parameters of crude manganese dioxide were obtained and morphological degradation analysis was performed to obtain the structural deviation index; a defect distribution map of the crude manganese dioxide cross-section was generated based on the structural deviation index.

[0011] The defect distribution map was analyzed to identify the deposition defect level, and the corresponding modification intervention weight was retrieved from the process compensation library. The corresponding compensation concentration range of citric acid was then analyzed using the modification intervention weight.

[0012] Based on the defect distribution map, the permeable layer range of the compensation concentration section at the solid-liquid interface is evaluated. The permeable layer range is aligned with the defect-dominant layer to determine the permeation characteristic depth. Based on the permeation characteristic depth, the corresponding control feedforward parameter combination is determined.

[0013] The layered modification configuration was determined based on the combination of feedforward parameters. Citric acid aqueous solution corresponding to the concentration range of citric acid was used to ball mill and disperse crude manganese dioxide according to the layered modification configuration. The modification was terminated after the modification effect was determined to be converged. The treated product was centrifuged, washed, dried and calcined to obtain refined manganese dioxide.

[0014] Furthermore, the concentration of citric acid in the electrolyte is 0.5–1.0 g / L;

[0015] The citric acid compensation concentration range corresponds to a citric acid concentration of 0.3–0.8 g / L;

[0016] Electrolysis temperature: 95±1℃, post-treatment calcination temperature: 350±5℃, and the upper limit of calcination temperature is 400℃.

[0017] Furthermore, the defect distribution map is generated in the following way:

[0018] Microscopic morphology images of the cross-section of crude manganese dioxide were extracted. The microscopic porosity and grain morphology features of the cross-section were identified by image segmentation algorithm, and the physical parameters of the cross-section were quantified.

[0019] A gray-level co-occurrence matrix is ​​introduced to analyze the morphological degradation of the cross-sectional physical parameters. Texture feature values ​​are extracted from each physical scan grid, and a multi-dimensional feature vector of each grid is constructed.

[0020] Extract the mean vector and covariance matrix of the standard sample set, and perform deviation measurement processing on the multidimensional feature vector of each physical scan grid to obtain the structural deviation index of each grid.

[0021] By setting a chi-square distribution critical value, the structural deviation index of each physical scan grid is compared with the chi-square distribution critical value to determine the local distortion state, and a discrete mapping defect distribution map is generated.

[0022] Furthermore, the method for analyzing the compensation concentration range is as follows:

[0023] Using the deposition defect level as the retrieval index, the modification intervention weights are retrieved from the process compensation database by table lookup and interpolation.

[0024] Multiply the modified intervention weight by the citric acid baseline concentration to obtain the center value of the compensation concentration;

[0025] Using the center value of the compensation concentration as the benchmark point of the section, retrieve the process tolerance of citric acid concentration from the process compensation library;

[0026] Using the center value of the compensation concentration as the center and the process tolerance as half the bandwidth, the upper limit of the compensation concentration section is obtained by offsetting upwards and the lower limit of the compensation concentration section is obtained by offsetting downwards.

[0027] Based on the upper and lower limits of the compensation concentration range, a compensation concentration range for citric acid is established.

[0028] Furthermore, the process for establishing the aforementioned deposition defect level is as follows:

[0029] The spatial distribution characteristics of deposition defects are obtained by statistically analyzing the area ratio of the warning color mark grid in the defect distribution map and locating the distribution centroid of the warning color mark along the thickness direction.

[0030] Based on the spatial distribution characteristics, the dominant layer of defects is determined, and a continuous scoring mapping is performed on the defect area ratio to determine the depositional defect level.

[0031] Furthermore, the process of determining the feedforward parameter combination is as follows:

[0032] Extract the target depth of the defect and perform alignment analysis with the permeable layer range to determine the optimal permeation characteristic depth that covers the defect layer while protecting the qualified layer;

[0033] Based on the optimal penetration feature depth, the trend of modification gains and excessive damage during the dispersion process is tracked, the inflection point of temporal competition is identified, the dispersion time limit is determined, and integrated into a feedforward parameter combination.

[0034] Furthermore, the method for determining the penetration feature depth is as follows:

[0035] If the depth of the defect target falls within the permeable layer range, the depth of the defect target is used as the lower limit of coverage, and the depth of the defect target plus a pre-defined etching allowance is used as the upper limit.

[0036] The median of the coverage lower and upper bounds is taken as the optimal penetration feature depth;

[0037] If the depth of the defect target exceeds the upper limit of the permeable layer range, the optimal permeability characteristic depth is temporarily taken as the upper limit of the permeable layer range, and a correction flag is generated to adjust the compensation concentration value upwards until the depth of the defect target falls into the permeable layer range, thus obtaining the optimal permeability characteristic depth.

[0038] Furthermore, the method for extracting the permeable stratum interval is as follows:

[0039] Read the centroid thickness position and the dominant layer of the defect distribution in the defect distribution map, retrieve the corresponding pore depth mapping coefficient based on the dominant layer of the defect, and multiply the depth mapping coefficient by the pore depth reference of the powder particles to obtain the target depth of the defect.

[0040] Based on the upper and lower limits of the compensation concentration range, capillary permeability analysis was used to assess the depth to which citric acid can permeate along the pores of particles, thus obtaining the permeable stratum range.

[0041] Furthermore, the process for determining the convergence of the modification effect is as follows:

[0042] Real-time characterization parameters are extracted and batch-to-batch performance consistency deviation is calculated during the application of the modification process. The convergence of the modification process is determined based on the batch-to-batch performance consistency deviation.

[0043] The intensity and duration of the modification are dynamically adjusted based on the batch-to-batch performance consistency deviation. After convergence, the modification is terminated and the product is dried and calcined to output refined manganese dioxide.

[0044] Furthermore, the method for establishing the process of applying the modification effect is as follows:

[0045] The feedforward parameter combination is analyzed, and the post-processing is configured to the corresponding modification mode according to the defect-dominant layer to obtain the layered modification configuration;

[0046] The execution parameters for acid injection and ball milling are set according to the layered modification configuration, and the execution parameters are sent to the post-processing process to obtain the modification effect application process.

[0047] The beneficial effects of this invention are as follows:

[0048] 1. This invention establishes an integrated electrolysis-post-treatment control system, which delays degradation through the complexation control, interfacial adsorption, and pH buffering effect of low-concentration citric acid in the electrolyte. The deposition rate promotes uniform nucleation of EMD, refines grains, increases porosity, and inhibits the formation of impurity phases. Meanwhile, in the post-processing stage, citric acid surface cleaning, light etching, and dispersion modification remove residual impurities such as sulfate and lead ions from the EMD surface, improving purity and dispersibility, thereby achieving significant optimization of the electrochemical performance of refined manganese dioxide.

[0049] 2. For coarse product characterization, a structural deviation index is generated, which converges the multi-dimensional chaotic appearance into a single quantifiable index; the morphological difference value is calculated by combining the characteristics of standard samples and the distortion state is determined based on the chi-square distribution critical value. This method distinguishes between slight fluctuations and real structural deterioration through statistical measurement. The generated defect distribution map transforms physical defects into a visual data matrix, realizing the spatial positioning of nucleation environment differences.

[0050] 3. In the defect analysis and parameter compensation stage, the centroid of defect distribution along the thickness direction is located and the area ratio is statistically analyzed to extract the spatial distribution characteristics of deposition defects. This helps to distinguish between acid-poor nucleation-dominated and homogeneous residual-dominated defects. The spatial characteristics are integrated with the defect-dominated layer to obtain a defect severity score. The corresponding modification intervention weight is retrieved from the process compensation library. The weight modulates the baseline concentration and combines it with the process tolerance to generate a compensation concentration range. This helps to achieve dynamic adaptive adjustment of acid concentration and reduce the risk of over-etching of the inner layer structure.

[0051] 4. To control the spatial and temporal aspects of the modification depth, the defect thickness scale is converted into a pore depth benchmark and combined with capillary permeability analysis to assess the reachable layers of citric acid, thereby predicting the spatial boundary of the chemical reaction zone. By aligning the defect target depth with the reachable layer range, the optimal permeability characteristic depth is determined, which helps to block destructive permeation into the qualified inner layer. The timing competition inflection point is identified to define the dispersion time limit. This feature uses a dynamic game mechanism to find the extreme point of modification efficiency, preventing severe collapse of surface pores caused by prolonged immersion.

[0052] 5. In the modification execution and dynamic convergence stages, the combination of feedforward parameters is analyzed and the bulk etching or surface replacement layered modification mode is allocated according to the defect-dominant layer site. This feature highly decouples and synergistically reuses the crushing and homogenization of mechanical ball milling and the chemical complexation of citric acid, and specifically treats coarse grains or surface impurities. Matching the acid addition rate with the optimal penetration characteristic depth is conducive to promoting a high degree of synchronization between the acid replenishment rhythm and the pore advancement rate, reducing the ineffective accumulation of reagents on the surface. By extracting the real-time particle size of the slurry and the residual sulfate concentration, the batch-to-batch performance consistency deviation is synthesized, and the concentration or ball milling cycle is corrected in different directions. The process execution deviation can be continuously fine-tuned until convergence, reducing the fluctuation range of electrochemical performance between product batches. Attached Figure Description

[0053] The invention will now be further described with reference to the accompanying drawings.

[0054] Figure 1 This is a flowchart of a process for preparing and modifying electrolytic manganese dioxide based on citric acid regulation according to the present invention;

[0055] Figure 2 This is a flowchart of a method for controlling the consistency of the nucleation environment of electrolytic manganese dioxide based on citric acid regulation in this invention;

[0056] Figure 3 This is a flowchart of the electrolytic manganese dioxide layered modification and dynamic convergence control process of the present invention. Detailed Implementation

[0057] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.

[0058] Example 1:

[0059] like Figure 1 As shown, a process for preparing and modifying electrolytic manganese dioxide based on citric acid includes the following steps:

[0060] A1. Electrolyte preparation: Prepare a sulfuric acid-manganese sulfate basic electrolyte, add citric acid as an additive and control the concentration of citric acid;

[0061] The concentration of MnSO4 was 0.49 mol / L, the concentration of H2SO4 was 0.29 mol / L, and citric acid was added as an additive with a concentration controlled at 0.5 g / L.

[0062] It should be noted that the concentration of citric acid in the electrolyte is 0.5–1.0 g / L. Exceeding this range (e.g., ≥5 g / L) will cause the EMD crystal form to transform into ε-MnO2 and defective fluorite phases, resulting in impurity phases.

[0063] A2. Electrolytic preparation of manganese dioxide (EMD): A titanium-manganese alloy plate is used as the anode and a copper tube is used as the cathode. The electrolysis process parameters are controlled. After electrolysis, the anode product is stripped off and washed and dried to obtain crude EMD.

[0064] The electrolysis process parameters include: electrolysis temperature, current density, and electrolysis time;

[0065] It should be noted that the electrolysis temperature is 95±1℃, the post-treatment calcination temperature is 350±5℃, and the calcination temperature should not exceed 400℃ to prevent the EMD crystal form from changing.

[0066] Preferably, the electrolysis temperature is controlled at 95℃ and the current density is maintained at 80A / m. 2 The electrolysis time was 168 h. After electrolysis, the anode product was stripped off, and the product was washed with deionized water until the pH of the washing solution was 6.8 (no white precipitate was found after testing with BaCl2 solution, confirming that no sulfate residue was present). The product was then dried at a constant temperature of 105℃ for 2.0 h to obtain crude EMD.

[0067] A3. EMD post-processing and modification: Crude EMD is extracted and dispersed by adding citric acid aqueous solution. The dispersed and modified solution is then ball-milled and centrifuged. The processed product is then washed, dried, calcined, cooled to room temperature, and ground to obtain refined EMD.

[0068] The concentration of citric acid used for dispersion modification was 0.8 g / L;

[0069] It should be noted that the concentration of citric acid used for dispersion modification in the post-treatment is 0.3–0.8 g / L, which is adapted to the concentration of citric acid in the electrolyte (0.5–1.0 g / L electrolyte corresponds to 0.8 g / L post-treatment, and ≥2.0 g / L electrolyte corresponds to 0.3 g / L post-treatment).

[0070] Preferably, ball milling at 300 r / min for 30 min and centrifugation at 3000 r / min for 10 min are used;

[0071] Wash three times with deionized water (50 mL of water each time), dry at 110℃ for 2.5 h, calcine at 350℃ for 1.0 h, cool to room temperature (25℃), and grind to a particle size of 1-3 μm (particle size distribution RSD≤18%) to obtain refined EMD.

[0072] It should be noted that the refined EMD specifications are as follows: purity ≥ 99.0%, particle size 1–3 μm, porosity 26%–28%, discharge capacity ≥ 230 mAh / g, crystallinity 80%–83%, and lattice defect density ≤ ;

[0073] The crude EMD content is 100.0g / serving.

[0074] Example 2:

[0075] like Figure 1 As shown, a process for preparing and modifying electrolytic manganese dioxide based on citric acid includes the following steps:

[0076] A1. Electrolyte preparation: Prepare a sulfuric acid-manganese sulfate basic electrolyte, add citric acid as an additive and control the concentration of citric acid;

[0077] The concentration of MnSO4 was 0.51 mol / L, the concentration of H2SO4 was 0.29 mol / L, and citric acid was added as an additive with a concentration controlled at 1 g / L.

[0078] It should be noted that the concentration of citric acid in the electrolyte is 0.5–1.0 g / L. Exceeding this range (e.g., ≥5 g / L) will cause the EMD crystal form to transform into ε-MnO2 and defective fluorite phases, resulting in impurity phases.

[0079] A2. Electrolytic preparation of manganese dioxide (EMD): A titanium-manganese alloy plate is used as the anode and a copper tube is used as the cathode. The electrolysis process parameters are controlled. After electrolysis, the anode product is stripped off and washed and dried to obtain crude EMD.

[0080] The electrolysis process parameters include: electrolysis temperature, current density, and electrolysis time;

[0081] It should be noted that the electrolysis temperature is 95±1℃, the post-treatment calcination temperature is 350±5℃, and the calcination temperature should not exceed 400℃ to prevent the EMD crystal form from changing.

[0082] Preferably, the electrolysis temperature is controlled at 95℃ and the current density is maintained at 80A / m. 2 The electrolysis time was 168 h. After electrolysis, the anode product was stripped off, and the product was washed with deionized water until the pH of the washing solution was 6.8 (no white precipitate was found after testing with BaCl2 solution, confirming that no sulfate residue was present). The product was then dried at a constant temperature of 105℃ for 2.0 h to obtain crude EMD.

[0083] A3. EMD post-processing and modification: Crude EMD is extracted and dispersed by adding citric acid aqueous solution. The dispersed and modified solution is then ball-milled and centrifuged. The processed product is then washed, dried, calcined, cooled to room temperature, and ground to obtain refined EMD.

[0084] The concentration of citric acid used for dispersion modification was 0.8 g / L;

[0085] It should be noted that the concentration of citric acid used for dispersion modification in the post-treatment is 0.3–0.8 g / L, which is adapted to the concentration of citric acid in the electrolyte (0.5–1.0 g / L electrolyte corresponds to 0.8 g / L post-treatment, and ≥2.0 g / L electrolyte corresponds to 0.3 g / L post-treatment).

[0086] Preferably, ball milling at 300 r / min for 30 min and centrifugation at 3000 r / min for 10 min are used;

[0087] Wash three times with deionized water (50 mL of water each time), dry at 110℃ for 2.5 h, calcine at 350℃ for 1.0 h, cool to room temperature (25℃), and grind to a particle size of 1-3 μm (particle size distribution RSD≤18%) to obtain refined EMD.

[0088] The crude EMD content is 100.0g / serving.

[0089] Comparative Example 1:

[0090] like Figure 1 As shown, a process for preparing and modifying electrolytic manganese dioxide based on citric acid includes the following steps:

[0091] A1. Electrolyte preparation: Prepare a sulfuric acid-manganese sulfate basic electrolyte, add citric acid as an additive and control the concentration of citric acid;

[0092] The concentration of MnSO4 was 0.51 mol / L, the concentration of H2SO4 was 0.29 mol / L, and citric acid was added as an additive with a concentration controlled at 5 g / L.

[0093] A2. Electrolytic preparation of manganese dioxide (EMD): A titanium-manganese alloy plate is used as the anode and a copper tube is used as the cathode. The electrolysis process parameters are controlled. After electrolysis, the anode product is stripped off and washed and dried to obtain crude EMD.

[0094] The electrolysis process parameters include: electrolysis temperature, current density, and electrolysis time;

[0095] Preferably, the electrolysis temperature is controlled at 95℃ and the current density is maintained at 80A / m. 2 The electrolysis time was 168 h. After electrolysis, the anode product was stripped off and washed with deionized water until the pH of the washing solution was 6.8 (no white precipitate was found after testing with BaCl2 solution, confirming that no sulfate residue was present). The product was then dried at a constant temperature of 105℃ for 2.0 h to obtain crude EMD.

[0096] A3. EMD post-processing and modification: Crude EMD is extracted and dispersed by adding citric acid aqueous solution. The dispersed and modified solution is then ball-milled and centrifuged. The processed product is then washed, dried, calcined, cooled to room temperature, and ground to obtain refined EMD.

[0097] The concentration of citric acid used for dispersion modification was 0.3 g / L;

[0098] Preferably, ball milling at 300 r / min for 30 min and centrifugation at 3000 r / min for 10 min are used;

[0099] Wash three times with deionized water (50 mL each time), dry at 110℃ for 2.5 h, calcine at 350℃ for 1.0 h, cool to room temperature (25℃), and grind to a particle size of 1-3 μm (particle size distribution RSD ≤ 18%) to obtain refined EMD;

[0100] The crude EMD content was 100.0g per serving.

[0101] Based on the different citric acid concentrations in Examples 1-3, the characteristic changes of the corresponding products are shown in Table 1.

[0102] It should be noted that the testing methods for product characteristics include: in-situ monitoring using an electrochemical quartz microbalance (EQCM). Deposition rate was measured using atomic force microscopy (AFM) combined with colloidal probe technology to measure interparticle van der Waals forces, and lead ion and sulfate residues were detected using ICP-OES.

[0103] As can be seen from the test data in Table 1, this invention effectively delays the degradation of electrolytes through complexation regulation, interfacial adsorption, and pH buffering effects of low-concentration citric acid. The deposition rate (measured in Examples 1-2) decreased to 0.05–0.08. This promotes uniform nucleation of EMD and inhibits the formation of impurity phases;

[0104] The dispersion modification in the post-treatment stage removed residual sulfate (≤0.1%) and lead ions (≤0.005%) on the EMD surface, effectively reducing interparticle van der Waals forces (measured reduction of 30% to 40%), improving the initial discharge capacity of the final product and reducing the high-current discharge decay rate.

[0105] Table 1: Summary of Test Data

[0106]

[0107] Example 4:

[0108] Please see Figure 2 Based on a citric acid-regulated process for the preparation and post-treatment modification of electrolytic manganese dioxide, a method for controlling the consistency of the nucleation environment of electrolytic manganese dioxide based on citric acid is established, including the following steps:

[0109] Step 1: Obtain the cross-sectional physical parameters of crude manganese dioxide and perform morphological degradation analysis to obtain the structural deviation index; generate a defect distribution map of the crude manganese dioxide cross-section based on the structural deviation index;

[0110] The process of obtaining the cross-sectional physical parameters of crude manganese dioxide and performing morphological degradation analysis to derive the structural deviation index is as follows:

[0111] S101. Extract the microscopic morphology image of the cross section of crude manganese dioxide, identify the microscopic porosity and grain morphology features of the cross section through image segmentation algorithm, and quantify the physical parameters of the cross section.

[0112] Specifically, the process of quantifying the physical parameters of the cross-section is as follows:

[0113] The cross-section of the crude manganese dioxide deposition layer is scanned at the set magnification using an electron microscope scanning probe to generate a cross-sectional microscopic morphology image containing structural information from the inner to the outer layers.

[0114] For example, the magnification is set to 2000x, which is beneficial for clearly characterizing the grain morphology and has a moderate field of view.

[0115] An adaptive thresholding method was applied to binarize the microscopic morphology image and extract the grain connected regions composed of continuous pixels.

[0116] The connected component algorithm is called to calculate the actual area of ​​each grain's connected component and the area of ​​its circumscribed equivalent circle. The ratio of the two is defined as the grain morphology regularity data.

[0117] At the same time, the proportion of the total area of ​​pixels in the connected regions of pores to the total area of ​​the image is statistically analyzed to obtain porosity data;

[0118] The porosity data and grain morphology regularity data were combined to form the cross-sectional physical parameters of crude manganese dioxide.

[0119] S102. Introduce the gray-level co-occurrence matrix to analyze the morphological degradation of the cross-sectional physical parameters, extract texture feature values ​​for each physical scan grid, and construct a multi-dimensional feature vector for each grid.

[0120] Specifically, the process of constructing multidimensional feature vectors is as follows:

[0121] Extract the grayscale pixel matrix of the microscopic morphology image described in S101, and divide the grayscale pixel matrix into multiple physical scanning grids according to the set physical scanning grid size; for example, the size of a single physical scanning grid is set to 10μm×10μm;

[0122] For each physical scan grid, a gray-level co-occurrence matrix with four different phase length directions is established; for example, the four different phase length directions are set to 0°, 45°, 90° and 135° respectively, and the pixel offset distance is set to 1;

[0123] The texture analysis algorithm is called to extract the texture contrast, texture energy value and texture entropy value from the gray-level co-occurrence matrix of each physical scan grid. The three-dimensional spatial feature vector of the grid is directly constructed using the texture contrast, texture energy value and texture entropy value of the same grid.

[0124] S103. Retrieve the mean vector and covariance matrix of the standard sample set, and perform deviation measurement processing on the multidimensional feature vector of each physical scan grid grid by grid to obtain the structural deviation index of each grid.

[0125] Specifically, the process of obtaining the deviation index of each grid structure is as follows:

[0126] Retrieve N consecutive batches of post-processed standard crude manganese dioxide samples from the local database, and read the texture contrast, texture energy, and texture entropy values ​​calculated for each standard sample using the same physical scanning grid size; for example, N=50.

[0127] Calculate the expected value of the standard sample in the three texture feature dimensions mentioned above, establish the mean vector, and calculate the covariance between the three dimensions to construct the covariance matrix.

[0128] For each physical scan grid, the Mahalanobis distance algorithm is used to measure the degree of deviation between the three-dimensional spatial feature vector of the grid and the mean vector of the standard sample under the constraint of the covariance matrix. The calculated Mahalanobis distance is defined as the structural deviation index of the physical scan grid.

[0129] The process of generating the defect distribution map of the coarse section based on the structural deviation index is as follows:

[0130] S104. Set the chi-square distribution critical value, compare the structural deviation index of each physical scan grid with the chi-square distribution critical value to determine the local distortion state, and generate a discrete mapping defect distribution map.

[0131] Specifically, the process of generating the defect distribution map of the rough section is as follows:

[0132] Set the significance level parameter and consult the chi-square distribution table to determine the critical value of the chi-square distribution; for example, the significance level parameter is set to 0.05.

[0133] The structural deviation index of each physical scan grid described in S103 is read one by one. If the structural deviation index of the current grid is greater than the chi-square distribution critical value, the grid is determined to be in a state of severe distortion and marked as a warning color mark; if the structural deviation index of the current grid is less than or equal to the chi-square distribution critical value, the grid is determined to be in a state of mild distortion and marked as a normal color mark.

[0134] The warning color mark and the normal color mark are mapped in a two-dimensional plane according to the grid node coordinate matrix to generate a defect distribution map for guiding local strengthening of post-processing technology.

[0135] Step 2: Analyze the defect distribution map, identify the deposition defect level left over from the electrolysis process, retrieve the modification intervention weight that matches the deposition defect level from the process compensation library, and use the modification intervention weight to analyze the corresponding citric acid compensation concentration range.

[0136] The process of analyzing the defect distribution map and identifying the level of deposition defects left over from the electrolysis process includes:

[0137] S201. Calculate the area ratio of the warning color mark grid in the statistical defect distribution map, and locate the distribution center of the warning color mark along the thickness direction to obtain the spatial distribution characteristics of the deposition defects.

[0138] Specifically, the process of obtaining spatial distribution characteristics is as follows:

[0139] Read the defect distribution map and extract the coordinate matrix of the corresponding grid node and the set size of a single physical scan grid;

[0140] The area of ​​the grid marked with the warning color code is used as the actual area of ​​the defect area.

[0141] Simultaneously, the total scanned area is statistically analyzed, and the proportion of the actual area of ​​the defective region to the total scanned area is calculated to obtain the defective area percentage.

[0142] Meanwhile, the grid row coordinates of the cross-sectional image are normalized to a thickness position scale of 0 to 1 along the direction from the inner layer to the outer layer of the anode product. The thickness position scale corresponding to the distribution centroid of all warning color marks is calculated by using the thickness position of each warning color mark grid as the coordinate and the number of occurrences of each warning color mark grid at that position as the weight.

[0143] By combining the defect area ratio with the thickness position scale of the distribution centroid, we can obtain spatial distribution characteristics that reflect both the quantity of defects and whether the defects are biased towards the inner or outer layer.

[0144] S202. Determine the dominant defect layer based on spatial distribution characteristics, and perform continuous scoring mapping on the defect area ratio to determine the deposition defect level;

[0145] Specifically, the process for determining the level of depositional defects is as follows:

[0146] The thickness position of the distribution centroid is used to determine the dominant layer of defects. If the thickness position of the distribution centroid is biased towards the outer layer, it is determined to be a poor acid nucleation type, that is, the defects mainly originate from the decrease in effective acid content in the later stage of electrolysis.

[0147] If the thickness position scale of the distribution center is biased towards the inner layer or located in the middle, it is judged to be a homogeneous residual dominant type, that is, the defects mainly originate from the surface sulfate and lead ion residues.

[0148] After determining the dominant defect layer, retrieve the monotonically increasing mapping curve between the defect area ratio and the defect severity score, which was pre-calibrated with qualified batches in the process compensation library.

[0149] By interpolating the current defect area ratio on the mapping curve, a defect severity score of 0 to 1 is obtained. The combination of the defect-dominant layer and the defect severity score is used to determine the depositional defect level.

[0150] The process of retrieving modification intervention weights from the process compensation library and analyzing the citric acid compensation concentration range is as follows:

[0151] S203. Using the deposition defect level as the retrieval index, the modification intervention weight is retrieved from the process compensation library by table lookup and interpolation.

[0152] Specifically, the process of retrieving the weights of the modification intervention is as follows:

[0153] The process compensation library pre-sorts two sets of calibration data according to the defect-dominant layer, with the acid-poor nucleation-dominant type corresponding to the enhanced etching calibration group and the homogeneous residue-dominant type corresponding to the mild dispersion calibration group.

[0154] Each set of calibration data stores a curve showing the correspondence between the defect severity score and the weight of the modification intervention;

[0155] The modified intervention weight is defined as a dimensionless modulation coefficient relative to the post-treatment citric acid baseline concentration;

[0156] If the current defect-dominant layer is acid-poor nucleation-dominant, then select the corresponding relationship curve of the enhanced etching calibration group, so that the weight increases with the increase of defect severity score and the amount of citric acid used.

[0157] If the current defect-dominant layer is of the homogeneous residual type, then select the corresponding relationship curve of the mild dispersion calibration group so that the weight only changes with the defect degree score in a small range, and prevents excessive etching damage to the pore structure.

[0158] The modification intervention weights are obtained by interpolating the defect severity score on the selected correspondence curve.

[0159] S204. Modulate the citric acid baseline concentration using the modified intervention weight, and analyze to obtain the citric acid compensation concentration range;

[0160] Specifically, the process of analyzing and obtaining the compensation concentration range is as follows: retrieve the preset citric acid baseline concentration and its permissible fluctuation range in the post-processing stage, wherein the baseline concentration is 0.6 g / L;

[0161] Multiply the modified intervention weight output by S203 by the citric acid baseline concentration to obtain the center value of the compensation concentration;

[0162] It should be noted that the modification intervention weight is a dimensionless modulation coefficient. The modification intervention weight is based on 1. A value greater than 1 indicates that the amount of citric acid is increased relative to the baseline concentration to enhance etching, while a value less than 1 indicates that the amount of citric acid is decreased relative to the baseline concentration to prevent over-etching.

[0163] For example, with a citric acid baseline concentration of 0.6 g / L, when the modification intervention weight is 1.25, the central value of the compensation concentration is 0.75 g / L; when the modification intervention weight is 0.6, the central value of the compensation concentration is 0.36 g / L.

[0164] The lower and upper limits of the compensation concentration range are determined by constructing the floating range, so as to obtain the compensation concentration range of citric acid that matches the current level of deposition defect;

[0165] Specifically, the method for determining the lower and upper limits of the compensation concentration range is as follows:

[0166] Using the center value of the compensation concentration as the reference point for the section, the process tolerance of citric acid concentration, which is calibrated along with the corresponding relationship curve in the process compensation library, is retrieved. The process tolerance represents the allowable deviation range of the actual amount of citric acid used in each qualified batch relative to the center value of the compensation concentration under the same defect degree score in the calibration stage. It is stored in the form of a relative percentage, which is used as the fluctuation range.

[0167] Using the center value of the compensation concentration as the center and the process tolerance as half the bandwidth, the upper limit of the compensation concentration section is obtained by offsetting upward and the lower limit of the compensation concentration section is obtained by offsetting downward. Based on this, the compensation concentration section of citric acid that matches the current deposition defect level and falls within the allowable range of the post-processing process is determined.

[0168] For example, when the center value of the compensation concentration is 1.0 g / L and the process tolerance is 5%, the corresponding upper deviation limit is 0.05 g / L and the lower deviation limit is 0.05 g / L, and the compensation concentration range is determined to be 0.95 g / L to 1.05 g / L.

[0169] Example 5:

[0170] Please see Figure 2 and Figure 3 As shown, a method for controlling the consistency of the nucleation environment of electrolytic manganese dioxide based on citric acid regulation further includes the following steps:

[0171] Step 3: Based on the defect distribution map, assess the permeable layer range of the compensation concentration zone at the solid-liquid interface. Through alignment analysis between the permeable layer range and the defect-dominant layer, determine the optimal permeation characteristic depth. Based on the optimal permeation characteristic depth, determine the corresponding control feedforward parameter combination.

[0172] The method for determining the optimal penetration depth is as follows: Based on the defect distribution map, the permeability range of the compensation concentration zone at the solid-liquid interface is assessed. This permeability range is then aligned with the defect-dominant layer.

[0173] S301. Read the centroid thickness position and the dominant layer of the defect distribution in the defect distribution map. Based on the dominant layer of the defect, retrieve the corresponding pore depth mapping coefficient. Multiply the depth mapping coefficient by the pore depth reference of the powder particles to obtain the target depth of the defect.

[0174] Specifically, the process of obtaining the depth of the defect target is as follows: read the thickness position scale of the centroid of the defect distribution in the defect distribution map and the dominant layer of the defect;

[0175] The average pore penetration depth of crude manganese dioxide single particles, which has been pre-calibrated and stored in the local database with qualified batches, is used as a depth reference for mapping the thickness position scale to the inside of the particles.

[0176] Based on the identified defect-dominant layer type, the corresponding preset pore depth mapping coefficient is retrieved from the process compensation library; the depth mapping coefficient is multiplied by the depth reference to obtain the defect target depth, that is, the depth of the citric acid-etched layer in the particle pore direction.

[0177] If the defect-dominant layer is acid-poor nucleation-dominant, then the target defect depth is taken as the shallower depth obtained by mapping to correspond to the coarse-grained defects in the outer layer.

[0178] If the defect-dominant layer is homogeneous and residual, the defect target depth is taken as the shallow depth close to the particle surface to correspond to the surface residual impurities. In both cases, the defect target depth changes in the same direction as the thickness position of the defect distribution centroid and is stored in the local cache.

[0179] S302. Based on the upper and lower limits of the compensation concentration range, capillary permeability analysis is used to evaluate the depth that citric acid can penetrate along the pores of particles, and the permeable stratum range is obtained.

[0180] Specifically, the process of obtaining the permeable stratum range is as follows:

[0181] Read the lower and upper limits of the compensation concentration range described in step two, as well as the pre-calibrated average equivalent pore size, pore tortuosity, viscosity and surface tension of the citric acid aqueous solution at the set dispersion temperature in the local database.

[0182] Using existing capillary permeation analysis methods, a shallow permeation progression curve with increasing permeation depth as dispersion progress is obtained by compensating for the solution properties corresponding to the lower limit of the concentration range, and a deep permeation progression curve is obtained by compensating for the solution properties corresponding to the upper limit of the concentration range. The two curves correspond to the shallowest and deepest permeation depths respectively on the same dispersion time axis.

[0183] The stable permeation depths that the shallow and deep permeation advancement curves can reach at a given dispersion temperature are taken as the lower and upper boundaries of the permeable stratum range, respectively, to obtain the permeable stratum range of the particle pore depth range that citric acid can reach in the current compensation concentration section.

[0184] The method for determining the corresponding feedforward parameter combination based on the optimal penetration feature depth is as follows:

[0185] S303. Perform alignment analysis between the target depth of the defect and the range of layers that can be penetrated to determine the optimal penetration characteristic depth that covers the defect layer and protects the qualified layer.

[0186] Specifically, the process of determining the optimal penetration feature depth is as follows:

[0187] Compare the target depth of defects obtained from S301 with the permeable stratum range obtained from S302 on the same particle pore depth coordinate;

[0188] If the target depth of the defect falls within the permeable layer range, it indicates that the citric acid in the compensation concentration section can reach the defect layer. At this time, the target depth of the defect is used as the lower limit of coverage, and the target depth of the defect plus a pre-calibrated etching allowance is used as the upper limit. The midpoint between the lower and upper limits of coverage is taken as the optimal penetration characteristic depth, so that the citric acid penetration just covers the defect layer without penetrating too deeply into the qualified inner layer.

[0189] It should be noted that the pre-calibrated etching allowance is 0.05–0.15 μm;

[0190] If the depth of the defect target exceeds the upper limit of the permeable layer range, it indicates that the current compensation concentration section is insufficient to reach the defect layer. At this time, the optimal permeability characteristic depth is temporarily taken as the upper limit of the permeable layer range, and a correction flag is generated to feed back to step two to adjust the compensation concentration value. After the compensation concentration section is updated, S302 and S303 are re-executed until the depth of the defect target falls into the permeable layer range, and the optimal permeability characteristic depth is obtained.

[0191] S304. Based on the optimal penetration feature depth, track the trend of modification gains and excessive damage during the dispersion process, identify the inflection point of temporal competition, determine the dispersion time limit, and integrate them into a feedforward parameter combination.

[0192] Specifically, the process of determining the dispersed time limits and integrating the feedforward parameter combinations is as follows:

[0193] On the deep penetration advancement curve obtained by S302, the dispersion process node corresponding to the optimal penetration characteristic depth is read. The process before the dispersion process node, where citric acid continues to advance into the defect layer and the etching modification area increases with dispersion time, is defined as the modification benefit rising segment.

[0194] At the same time, the cumulative change relationship of surface pore collapse degree with dispersion time, which was pre-calibrated with qualified batches in the local database, was retrieved. The process of pore collapse and specific surface area decline of the etched surface due to continuous immersion was defined as the excessive damage rising stage.

[0195] The unit time increment of the modification benefit is compared with the unit time increment of the excessive damage point by point along the dispersed time axis. When the unit time increment of the modification benefit changes from being greater than the unit time increment of the excessive damage to being less than the increment, it is determined that the time competition in the stalemate between the modification benefit and the excessive damage has been reached. The dispersed time corresponding to the time competition inflection point is determined as the dispersed time limit.

[0196] If the incremental benefit of modification is always greater than the incremental damage before the penetration depth reaches the optimal penetration feature depth, then the dispersion time corresponding to the penetration depth reaching the optimal penetration feature depth is determined as the dispersion time limit to ensure that the defect layer is completely covered.

[0197] Finally, the compensation concentration range, the optimal permeation characteristic depth, and the dispersion time limit are linked together to integrate the feedforward parameter combination.

[0198] Step 4: Analyze the feedforward parameter combination and determine the layered modification configuration based on the defect-dominant layer; perform modification treatment according to the layered modification configuration and determine whether the modification effect has converged; after convergence, terminate the modification and dry and calcine to output refined manganese dioxide.

[0199] The process of analyzing the feedforward parameter combination and determining the layered modification configuration based on the defect-dominant layer is as follows:

[0200] S401. Analyze the combination of feedforward parameters and configure the post-processing to the corresponding modification mode according to the defect-dominant layer to obtain the layered modification configuration.

[0201] Specifically, the process of obtaining the hierarchical modification configuration is as follows:

[0202] Retrieve the feedforward parameter combination described in step three, and read the interlinked compensation concentration range, optimal permeation characteristic depth, dispersion time limit, and associated defect-dominant layer.

[0203] If the defect-dominant layer is acid-poor nucleation-dominant, then the post-processing is configured as a bulk etching mode, so that citric acid penetrates to the optimal penetration depth during the dispersion process to perform interface etching modification on the coarse-grained defects on the outer layer.

[0204] If the defect-dominant layer is homogeneous and residual, then the post-treatment will be configured as surface replacement mode, so that citric acid will act on the particle surface to complex and replace residual sulfate and lead ions without penetrating into the qualified inner layer.

[0205] The selected modification mode is bound to the compensation concentration range, the optimal permeation characteristic depth, and the dispersion time limit in the feedforward parameter combination to obtain the stratified modification configuration and store it in the local cache.

[0206] The process of performing modification treatment according to the layered modification configuration, determining whether the modification has converged, terminating the modification after convergence, drying and calcining, and outputting refined manganese dioxide is as follows:

[0207] S402. Set the execution parameters for acid injection and ball milling according to the layered modification configuration, and send the execution parameters to the post-processing process to obtain the modification effect application process;

[0208] Specifically, the process of obtaining the modification effect is as follows:

[0209] Read the compensation concentration range and the optimal permeation characteristic depth in the stratified modification configuration obtained from S401;

[0210] The concentration of citric acid solution to be added is determined by the median of the compensation concentration range, and the acid addition rate is determined by the permeation advance rhythm corresponding to the optimal permeation characteristic depth, so that the replenishment rate of citric acid is connected with its permeation advance along the pores and does not accumulate on the surface.

[0211] Meanwhile, the ball milling cycle is set according to the modification mode. The bulk etching mode uses a higher ball milling speed and a longer ball milling period to promote the citric acid to penetrate into the defect layer along with the cross-section of the new particles. The surface replacement mode uses a lower ball milling speed and a shorter ball milling period to avoid excessive crushing of the qualified inner layer.

[0212] The concentration of acid added, the acid addition rate, and the cycle time of the ball mill are sent to the post-processing process as execution parameters to initiate the mechanochemical synergistic modification of crude manganese dioxide by citric acid. This process achieves the modification effect of selectively etching the defect layer along the thickness direction, homogenizing the layered structure, and complexing to remove residual impurities on the surface.

[0213] The process of dynamically correcting the modification effect and outputting refined manganese dioxide with batch-to-batch performance consistency as the convergence objective is as follows:

[0214] S403. Extract real-time characterization quantities and calculate batch-to-batch performance consistency deviation during the application of modification; determine whether the modification has converged based on the batch-to-batch performance consistency deviation.

[0215] Specifically, the process for determining whether the modification has converged is as follows:

[0216] During the modification process, a small amount of dispersed slurry was taken out at the set sampling interval. The real-time particle size distribution was determined by online particle size analysis, and the real-time concentration of residual sulfate in the filtrate was determined by online turbidimetric method (with the addition of barium chloride reagent for color development). The real-time characterization quantities that characterize the modification process were obtained.

[0217] Retrieve the target particle size distribution range and the qualified residual sulfate concentration pre-calibrated with qualified batches from the local database, and combine the deviation of the real-time particle size distribution relative to the median of the target particle size distribution range and the deviation of the real-time residual sulfate concentration relative to the qualified concentration according to the pre-calibrated weights to form the inter-batch performance consistency deviation.

[0218] It should be noted that in the pre-calibrated weights, the particle size deviation weight is 0.35 to 0.45, the sulfate deviation weight is 0.55 to 0.65, and the sum of the two weights is 1. This weight allocation emphasizes the dominant role of chemical purity (residual sulfate) on electrochemical performance.

[0219] If the batch-to-batch performance consistency deviation has entered the pre-calibrated convergence range, for example, the convergence range is set to a comprehensive deviation value ≤ 5%, then the modification effect is determined to have converged and proceeds to S404;

[0220] If the batch-to-batch performance consistency deviation is still outside the convergence range, it is determined that the modification effect has not yet converged and will proceed to the following dynamic correction.

[0221] S404. Based on the batch-to-batch performance consistency deviation, dynamically correct the intensity and duration of the modification effect, terminate the modification after convergence, and dry and calcine to output refined manganese dioxide.

[0222] Specifically, the process of outputting refined manganese dioxide is as follows: when S403 determines that the modification effect has not yet converged, it is corrected according to the source of the batch-to-batch performance consistency deviation. If the deviation is mainly due to the high residual sulfate, the concentration of citric acid is increased within the allowable range of the compensation concentration range and the dispersion duration is extended to enhance complexation and replacement.

[0223] If the deviation is mainly due to the real-time particle size being too coarse, then increase the rotation speed of the ball mill and extend the ball milling period to enhance crushing and homogenization. After correction, return to S403 to re-extract the real-time characterization and make a judgment.

[0224] When S403 determines that the modification effect has reached convergence, or the dispersion duration reaches the dispersion time limit described in step three, the addition of citric acid and ball milling are terminated. The dispersion slurry is then centrifuged, washed with deionized water, and dried at 110°C and calcined at 350°C according to predetermined conditions to obtain refined manganese dioxide with consistent batch-to-batch performance.

[0225] The foregoing has provided a detailed description of one embodiment of the present invention, but this description is merely a preferred embodiment and should not be construed as limiting the scope of the invention. All equivalent variations and modifications made within the scope of the present invention should still fall within the scope of the present invention.

Claims

1. A process for preparing and modifying electrolytic manganese dioxide based on citric acid regulation, characterized in that, Includes the following steps: Prepare a sulfuric acid-manganese sulfate basic electrolyte by adding citric acid as an additive and controlling the concentration of citric acid; Electrolysis was performed using a titanium-manganese alloy plate as the anode and a copper tube as the cathode. After electrolysis, the anode product was stripped off, washed, and dried to obtain crude manganese dioxide. The cross-sectional physical parameters of crude manganese dioxide were obtained and morphological degradation analysis was performed to obtain the structural deviation index. Defect distribution maps of coarse sections are generated based on structural deviation index; The defect distribution map was analyzed to identify the deposition defect level, and the corresponding modification intervention weight was retrieved from the process compensation library. The corresponding compensation concentration range of citric acid was then analyzed using the modification intervention weight. Based on the defect distribution map, the permeable layer range of the compensation concentration section at the solid-liquid interface is evaluated. The permeable layer range is aligned with the defect-dominant layer to determine the permeation characteristic depth. Based on the permeation characteristic depth, the corresponding control feedforward parameter combination is determined. The hierarchical modification configuration is determined based on the combination of feedforward parameters; Crude manganese dioxide was ball-milled and dispersed using a citric acid aqueous solution corresponding to the concentration range of citric acid compensation, according to the layered modification configuration. The modification was terminated after the modification effect was determined to be convergent. The treated product was centrifuged, washed, dried and calcined to obtain refined manganese dioxide.

2. The process for preparing and modifying electrolytic manganese dioxide based on citric acid regulation according to claim 1, characterized in that: The concentration of citric acid in the electrolyte is 0.5–1.0 g / L; The citric acid compensation concentration range corresponds to a citric acid concentration of 0.3–0.8 g / L; Electrolysis temperature: 95±1℃, post-treatment calcination temperature: 350±5℃, and the upper limit of calcination temperature is 400℃.

3. The process for preparing and modifying electrolytic manganese dioxide based on citric acid regulation according to claim 1, characterized in that: The defect distribution map is generated as follows: Microscopic morphology images of the cross-section of crude manganese dioxide were extracted. The microscopic porosity and grain morphology features of the cross-section were identified by image segmentation algorithm, and the physical parameters of the cross-section were quantified. A gray-level co-occurrence matrix is ​​introduced to analyze the morphological degradation of the cross-sectional physical parameters. Texture feature values ​​are extracted from each physical scan grid, and a multi-dimensional feature vector of each grid is constructed. Extract the mean vector and covariance matrix of the standard sample set, and perform deviation measurement processing on the multidimensional feature vector of each physical scan grid to obtain the structural deviation index of each grid. By setting a chi-square distribution critical value, the structural deviation index of each physical scan grid is compared with the chi-square distribution critical value to determine the local distortion state, and a discrete mapping defect distribution map is generated.

4. The preparation and post-treatment modification process of electrolytic manganese dioxide based on citric acid regulation according to claim 1, characterized in that: The method for analyzing the compensation concentration range is as follows: Using the deposition defect level as the retrieval index, the modification intervention weights are retrieved from the process compensation database by table lookup and interpolation. Multiply the modified intervention weight by the citric acid baseline concentration to obtain the center value of the compensation concentration; Using the center value of the compensation concentration as the benchmark point of the section, retrieve the process tolerance of citric acid concentration from the process compensation library; Using the center value of the compensation concentration as the center and the process tolerance as half the bandwidth, the upper limit of the compensation concentration section is obtained by offsetting upwards and the lower limit of the compensation concentration section is obtained by offsetting downwards. Based on the upper and lower limits of the compensation concentration range, a compensation concentration range for citric acid is established.

5. The electrolytic manganese dioxide preparation and post-treatment modification process based on citric acid regulation according to claim 4, characterized in that: The process for establishing the aforementioned deposition defect level is as follows: The spatial distribution characteristics of deposition defects are obtained by statistically analyzing the area ratio of the warning color mark grid in the defect distribution map and locating the distribution centroid of the warning color mark along the thickness direction. Based on the spatial distribution characteristics, the dominant layer of defects is determined, and a continuous scoring mapping is performed on the defect area ratio to determine the depositional defect level.

6. The preparation and post-treatment modification process of electrolytic manganese dioxide based on citric acid regulation according to claim 1, characterized in that: The process of determining the feedforward parameter combination is as follows: Extract the target depth of the defect and perform alignment analysis with the permeable layer range to determine the optimal permeation characteristic depth that covers the defect layer while protecting the qualified layer; Based on the optimal penetration feature depth, the trend of modification gains and excessive damage during the dispersion process is tracked, the temporal competition inflection point is identified to determine the dispersion time limit, and integrated into a feedforward parameter combination.

7. The preparation and post-treatment modification process of electrolytic manganese dioxide based on citric acid regulation according to claim 6, characterized in that: The method for determining the penetration feature depth is as follows: If the depth of the defect target falls within the permeable layer range, the depth of the defect target is used as the lower limit of coverage, and the depth of the defect target plus a pre-defined etching allowance is used as the upper limit. The median of the coverage lower and upper bounds is taken as the optimal penetration feature depth; If the depth of the defect target exceeds the upper limit of the permeable layer range, the optimal permeability characteristic depth is temporarily taken as the upper limit of the permeable layer range, and a correction flag is generated to adjust the compensation concentration value upwards until the depth of the defect target falls into the permeable layer range, thus obtaining the optimal permeability characteristic depth.

8. The preparation and post-treatment modification process of electrolytic manganese dioxide based on citric acid regulation according to claim 6, characterized in that: The method for extracting the permeable stratum range is as follows: Read the centroid thickness position and the dominant layer of the defect distribution in the defect distribution map, retrieve the corresponding pore depth mapping coefficient based on the dominant layer of the defect, and multiply the depth mapping coefficient by the pore depth reference of the powder particles to obtain the target depth of the defect. Based on the upper and lower limits of the compensation concentration range, capillary permeability analysis was used to assess the depth to which citric acid can permeate along the pores of particles, thus obtaining the permeable stratum range.

9. The preparation and post-treatment modification process of electrolytic manganese dioxide based on citric acid regulation according to claim 1, characterized in that: The process for determining the convergence of the modification effect is as follows: Real-time characterization parameters are extracted and batch-to-batch performance consistency deviation is calculated during the application of the modification process. The convergence of the modification process is determined based on the batch-to-batch performance consistency deviation. The intensity and duration of the modification are dynamically adjusted based on the batch-to-batch performance consistency deviation. After convergence, the modification is terminated and the product is dried and calcined to output refined manganese dioxide.

10. The preparation and post-treatment modification process of electrolytic manganese dioxide based on citric acid regulation according to claim 9, characterized in that: The method for establishing the process of applying the modification effect is as follows: The feedforward parameter combination is analyzed, and the post-processing is configured to the corresponding modification mode according to the defect-dominant layer to obtain the layered modification configuration; The execution parameters for acid injection and ball milling are set according to the layered modification configuration, and the execution parameters are sent to the post-processing process to obtain the modification effect application process.