A catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation, its preparation method, and its application.
By adjusting the local coordination environment and interfacial electronic state of ZnO, xFZO-y catalysts were prepared, which solved the problems of low selectivity and efficiency of H2O2 generation in the two-electron water oxidation reaction at the anode, and achieved efficient H2O2 generation and good electrocatalytic stability.
Patent Information
- Application Number
- CN202611506030.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-25
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, the selectivity and efficiency of the two-electron water oxidation reaction (2e-WOR) at the anode to generate hydrogen peroxide (H2O2) are low, making it difficult to effectively promote the generation of H2O2 in carbonate-mediated electrolyte systems. Furthermore, the local coordination environment and interfacial electronic state regulation of ZnO materials are insufficient.
By solid-phase mixing of ZnO and ZnF2 and calcination under different atmospheres, the local coordination environment and interfacial electronic state of ZnO were adjusted, and the H2O2 generation performance in the carbonate-mediated anodic two-electron water oxidation process was optimized.
The catalyst significantly improved the selectivity and reaction efficiency of H2O2 formation. It exhibited high H2O2 Faradaic efficiency and formation rate in the carbonate-mediated anodic two-electron water oxidation process and had good electrocatalytic stability.
Smart Images

Figure CN123108604A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of advanced non-ferrous metal materials and electrochemical synthesis of hydrogen peroxide, specifically to a catalytic material for the electrochemical synthesis of hydrogen peroxide from water oxidation, its preparation method, and its application. Background Technology
[0002] Water electrolysis driven by renewable electricity typically produces hydrogen (H2) at the cathode and oxygen (O2) at the anode via the oxygen evolution reaction (OER). Since the value of O2 is relatively low, the use of anodic reactions to prepare chemicals with higher application value is gaining attention. Hydrogen peroxide (H2O2) is an important green oxidant widely used in chemical synthesis, environmental remediation, disinfection, and energy, but current industrial production of H2O2 still mainly relies on the anthraquinone process, which is complex and consumes a large amount of solvent. A green, distributed synthesis of H2O2 using water as a raw material and renewable electricity provides a new technological path for traditional centralized production methods. Among these methods, the two-electron water oxidation reaction at the anode (2e...)... - WOR can directly generate H2O2 from water, which is expected to improve the utilization value of the anode products of water electrolysis, and therefore has attracted widespread attention.
[0003] Despite the anode 2e - WOR provides a direct pathway for the direct electrosynthesis of H₂O₂, but its reaction selectivity still faces significant challenges. Compared to the four-electron OER with a thermodynamic potential of approximately 1.23 V, 2e - The thermodynamic potential for H₂O₂ formation from WOR is approximately 1.76 V, which is thermodynamically unfavorable and susceptible to competition from OER. During the reaction, the catalytic interface needs to promote the effective activation of the reaction precursor, stabilize the O–O bond-containing intermediate, and simultaneously inhibit further four-electron oxidation and secondary oxidation of H₂O₂. Therefore, it is crucial to improve the anolyte 2electron potential by controlling the interfacial structure and electronic state of the catalyst. - The selectivity and reaction efficiency of H2O2 generation during the WOR process remain important technical issues that need to be addressed in this field.
[0004] Previous studies have shown that carbonate / bicarbonate electrolytes can promote anodic 2e -WOR generates H2O2 and provides a new reaction pathway for H2O2 formation by participating in the anodic interface reaction. Zinc oxide (ZnO) has the characteristics of simple composition, stable structure, and easy control of surface defects and electronic structure, making it a suitable catalytic material for related electrocatalytic reactions. Modifying the local coordination environment and interfacial electronic state of ZnO through heteroelement doping and defect modulation is an effective means to improve its catalytic performance. Fluorine, with its strong electronegativity, can regulate the local coordination structure and electronic state of ZnO after introduction, providing the possibility of further improving the adsorption and transformation behavior of reactive species at the catalytic interface.
[0005] Chinese invention patent application CN102013327A discloses a method for preparing a fluoride-doped ZnO porous prismatic array thin film. This method uses an aqueous solution containing zinc and fluoride salts to form a fluoride precursor on a conductive substrate via a low-temperature chemical bath, followed by heat treatment to obtain the fluoride-doped ZnO array thin film, primarily for applications in solar cells and photocatalysis. However, this technology mainly focuses on the construction of ZnO array thin films. Its preparation method, material morphology, and application scenarios differ significantly from the carbonate-mediated anodic two-electron water oxidation electrosynthesis of H2O2. Furthermore, it does not involve the preparation of fluoride-doped ZnO through solid-phase mixing and calcination of ZnO with a fluoride-containing zinc source for use in the aforementioned reaction system. Therefore, although fluoride-doped ZnO materials and their preparation have been disclosed, how to control the local structure and interfacial electronic states of ZnO through appropriate fluoride introduction and heat treatment conditions to improve the carbonate-mediated anodic 2e2-electron oxidation of H2O2 remains a significant challenge. - The selectivity of H2O2 formation and reaction efficiency during the WOR process still have room for further research and improvement. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation, its preparation method, and its application. The catalyst, by introducing fluorine to regulate the local coordination environment and interfacial electronic state of ZnO, significantly improves the selectivity and reaction efficiency of H2O2 generation during the carbonate-mediated two-electron anodic water oxidation process. The catalyst preparation method is simple, the conditions are easy to control, and it exhibits good electrocatalytic activity and stability.
[0007] A method for preparing a catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation includes the following steps: (1) ZnO and ZnF2 are mixed in a solid phase according to a set ratio and then ground thoroughly to obtain a mixed precursor; (2) The mixed precursor obtained in step (1) is calcined under a certain atmosphere, cooled and ground again to obtain the catalyst.
[0008] For ease of description, the obtained catalyst material is denoted as xFZO-y, where x represents the mass percentage of ZnF2 in the total feed mass of ZnO and ZnF2, and y represents the calcination temperature.
[0009] The specific process conditions for each step in the above preparation route are as follows: (a) In step (1): Both ZnO and ZnF2 can be used as powdered solid raw materials, and ZnO and ZnF2 are mixed in a certain mass ratio. The mass percentage of ZnF2 in the total mass of ZnO and ZnF2 is 1% to 60%. Preferably, the mass percentage of ZnF2 is 5% to 40%.
[0010] The mixing method of ZnO and ZnF2 can be one or more of mortar grinding, mechanical grinding or ball milling, so as to ensure that the two solid raw materials are fully contacted and uniformly mixed.
[0011] (ii) In step (2): The mixed precursor can be heat-treated in an alumina crucible, a ceramic crucible, or other high-temperature resistant container. Preferably, a ceramic crucible is used.
[0012] The calcination atmosphere is at least one of air, oxygen, nitrogen, and argon. Preferably, calcination is carried out in an air atmosphere.
[0013] The calcination temperature is 100–800 °C, preferably 200–600 °C. During calcination, the heating rate can be 1–10 °C / min. -1 Preferably 4–6 ℃ min -1 After reaching the set temperature, the heat preservation time can be 1 to 8 hours, preferably 2 hours.
[0014] After calcination, the resulting product is cooled to room temperature. Cooling can be achieved through natural cooling or programmed cooling; preferably, it is cooled to room temperature at a rate of 5 °C min⁻¹. The cooled solid is then ground again to obtain the catalyst material for the electrosynthesis of hydrogen peroxide from water oxidation.
[0015] This invention also provides an application of the prepared catalytic material in the carbonate-mediated anodic two-electron water oxidation to H2O2 electrosynthesis. Specifically, it includes the following steps: The catalytic material was used as the working electrode and placed in a carbonate electrolyte system to carry out an electrochemical oxidation reaction to prepare hydrogen peroxide from water. After the reaction was completed, the hydrogen peroxide in the electrolyte was quantitatively analyzed.
[0016] Preferably, the electrochemical reaction is carried out using a three-electrode system, wherein the working electrode is an FZO catalytic electrode, the counter electrode is a platinum sheet, and the reference electrode is one of an Ag / AgCl electrode or a Hg / HgO electrode.
[0017] Preferably, the electrolysis method is constant potential electrolysis, and the applied potential is preferably 2.5 to 3.2 V vs. RHE; the electrolysis time is 5 to 500 min.
[0018] Preferably, the carbonate includes, but is not limited to, carbonate systems such as Na₂CO₃ and K₂CO₃; the concentration of the carbonate in the electrolyte is 0.1–2.0 mol / L. -1 .
[0019] In this invention, the catalyst prepared by the solid-phase mixing-calcination method exhibits good structural stability, and the doping of F element can effectively regulate the local coordination environment and interfacial electronic state of ZnO. The prepared catalyst has good interfacial electrochemical activity, showing high H2O2 generation selectivity, generation rate, and good electrocatalytic stability in the carbonate-mediated anodic two-electron water oxidation process.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The present invention uses a solid-phase mixing-calcination method of ZnO and ZnF2 to prepare a catalyst for the electrosynthesis of hydrogen peroxide by water oxidation. The preparation process is simple, without the need for complex solution synthesis and precursor deposition processes. The process conditions are easy to control, and the composition and structure of the catalyst can be optimized by adjusting the ZnF2 feeding ratio and calcination temperature.
[0021] (2) The present invention regulates the local coordination environment and electronic structure of ZnO by introducing F element, forming a catalytic interface that is conducive to the adsorption of carbonate reaction species and the conversion of intermediates containing peroxy bonds. This promotes the activation of reaction precursors, while also facilitating the retention of O–O bonds and inhibiting competitive oxygen evolution reaction, thereby improving the selectivity of anodic two-electron water oxidation to H2O2.
[0022] (3) The catalyst prepared in this invention exhibits high H2O2 Faradaic efficiency, formation rate, and good operational stability during carbonate-mediated anodic two-electron water oxidation. Specifically, the optimized catalyst achieves an H2O2 Faradaic efficiency of approximately 84.7% at 2.7 V vs. RHE, and a H2O2 formation rate of up to 59.7 μmol cm⁻¹ at 3.0 V vs. RHE. -2 h -1 It maintains approximately 80.6% Faraday efficiency and can operate stably for extended periods. Attached Figure Description
[0023] Figure 1 This is a transmission electron microscope (TEM) image of the 10FZO-400 catalyst.
[0024] Figure 2 A comparison of the concentration and Faraday efficiency of FZO catalysts prepared with different ZnF2 feed ratios and different calcination temperatures in carbonate electrolytes for the electrosynthesis of H2O2.
[0025] Figure 3 This is a comparison chart showing the concentration and Faraday efficiency of 10FZO-400 catalyst in different types and concentrations of electrolytes for the electrosynthesis of H2O2.
[0026] Figure 4 The graph shows the concentration changes of H2O2 synthesized by 10FZO-400, ZnO-400 and ZnO catalysts under different applied potentials.
[0027] Figure 5 The graph shows the variation of the Faraday efficiency of 10FZO-400, ZnO-400 and ZnO catalysts in the electrosynthesis of H2O2 under different applied potentials.
[0028] Figure 6 Linear sweep voltammetry (LSV) curves of 10FZO-400, ZnO-400 and ZnO catalysts in carbonate electrolyte.
[0029] Figure 7 Electrochemical impedance spectroscopy (EIS) spectra of 10FZO-400, ZnO-400 and ZnO catalysts in carbonate electrolyte.
[0030] Figure 8 The double-layer capacitance (C) of 10FZO-400, ZnO-400 and ZnO catalysts dl Test results diagram.
[0031] Figure 9 The graph shows the changes in current density and H2O2 Faraday efficiency over time during the continuous electrolysis of 10FZO-400 catalyst for 8 h. Detailed Implementation
[0032] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.
[0033] Example 1 The preparation method of a catalytic material for the electrosynthesis of hydrogen peroxide by water oxidation in this embodiment includes the following steps: (1) Weigh ZnO and ZnF2 powders according to the ratio of ZnF2 to 10% of the total mass of ZnO and ZnF2, place them in a mortar and grind them thoroughly to make them evenly mixed to obtain a mixed precursor; (2) The mixed precursor obtained in step (1) is placed in an alumina crucible and heated to 400 ℃ at a heating rate of 5 ℃ min⁻¹ in an air atmosphere and held for 2 h. After the heat treatment, it is cooled to room temperature at a rate of 5 ℃ min⁻¹ and the resulting solid is ground again to obtain the catalyst material for the electrosynthesis of hydrogen peroxide by water oxidation, which is denoted as 10FZO-400 catalyst.
[0034] Example 2 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that in step (1), ZnF2 accounted for 40% of the total feed mass of ZnO and ZnF2. The resulting catalyst was denoted as 40FZO-400.
[0035] Example 3 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that in step (2), the calcination temperature was 200 °C. The resulting catalyst was designated as 10FZO-200.
[0036] Example 4 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that in step (2), the calcination temperature was 600 °C. The resulting catalyst was designated as 10FZO-600.
[0037] Example 5 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that ZnO and ZnF2 were fully ground and mixed at a ratio of ZnF2 accounting for 10% of the total feed mass. After obtaining the mixed precursor, step (2) was not performed, and the resulting sample was recorded as 10FZO.
[0038] Example 6 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that in step (1), ZnF2 was not added, only ZnO was weighed, and ZnO was placed in an alumina crucible and calcined at 400 °C for 2 h according to the same heat treatment procedure as step (2) of Example 1. After cooling to room temperature, it was ground to obtain ZnO-400 catalyst.
[0039] Figure 1 The image shows the transmission electron microscope (TEM) morphology of the 10FZO-400 catalyst obtained in Example 1. As can be seen from the image, 10FZO-400 is composed of nanoscale particles with a certain degree of contact and aggregation between the particles, maintaining a relatively complete particle structure. This indicates that a structurally stable FZO catalyst can be obtained after solid-phase mixing of ZnO / ZnF2 and heat treatment at 400 °C.
[0040] Figure 2The performance of FZO catalysts prepared with different ZnF2 feed ratios and calcination temperatures for the electrosynthesis of H2O2 was compared. The results showed that both the ZnF2 feed ratio and calcination temperature significantly affected the H2O2 formation performance. With changes in the amount of F introduced and the calcination conditions, the H2O2 concentration and Faradaic efficiency of each sample varied significantly. 10FZO-400 exhibited the best overall performance, indicating that appropriate F introduction and heat treatment temperature are beneficial for forming a suitable catalytic interface for carbonate-mediated two-electron water oxidation at the anolyte.
[0041] Figure 3 The H2O2 generation performance of the 10FZO-400 catalyst in electrolytes of different types and concentrations is shown in the figure. As can be seen from the figure, electrolyte composition and carbonate concentration have a significant impact on H2O2 generation. In 1 M NaOH electrolyte, both the H2O2 generation concentration and the Faradaic efficiency are low. When using Na2CO3 as the electrolyte, as the Na2CO3 concentration increases from 0.1 M to 1 M, both the H2O2 generation concentration and the Faradaic efficiency generally improve significantly, with 1 M Na2CO3 exhibiting superior overall H2O2 generation performance. Furthermore, a high H2O2 Faradaic efficiency can also be obtained when using 1 M K2CO3 as the electrolyte, indicating that carbonate species have a significant promoting effect on the oxidation of two-electron water to H2O2 at the anolyte. Simultaneously, the conductivity of different carbonate systems will affect H2O2 accumulation to some extent.
[0042] Figure 4 and Figure 5 The H2O2 formation concentrations and Faradaic efficiencies of 10FZO-400, ZnO-400, and ZnO at different applied potentials are shown. In a 1 M Na2CO3 electrolyte, the overall H2O2 formation of the three materials increased with increasing applied potential, with 10FZO-400 exhibiting higher H2O2 formation capacity at all test potentials. Meanwhile, 10FZO-400 maintained a high H2O2 Faradaic efficiency over a wide potential range, reaching approximately 84.7% at 2.7 V vs. RHE; when the potential increased to 3.0 V vs. RHE, the H2O2 formation rate reached 59.7 μmol / cm³. -2 h -1 While maintaining a Faraday efficiency of approximately 80.6%, ZnO and ZnO-400 exhibit significantly lower H2O2 selectivity. These results indicate that the introduction of F significantly improves the H2O2 generation performance of ZnO in the carbonate-mediated anodic two-electron water oxidation process, and this improvement is not solely due to heat treatment.
[0043] Figure 6Linear sweep voltammetry curves for 10FZO-400, ZnO-400, and ZnO are shown. Compared to ZnO and ZnO-400, 10FZO-400 exhibits a lower reaction onset potential and a higher anodic current response, indicating that the electrochemical reaction kinetics at the catalytic interface are improved after the introduction of F, which is beneficial to the anodic reaction.
[0044] Figure 7 Electrochemical impedance spectroscopy (EIS) spectra of 10FZO-400, ZnO-400, and ZnO are shown. The significantly reduced semicircle diameter of the Nyquist curve for 10FZO-400 indicates a decrease in charge transfer resistance at the electrode / electrolyte interface, suggesting improved interfacial charge transport. This result is consistent with linear sweep voltammetry, further demonstrating that F doping is beneficial for enhancing the interfacial electrochemical reaction kinetics of the catalyst.
[0045] Figure 8 The results show the electric double-layer capacitance of 10FZO-400, ZnO-400, and ZnO. The electric double-layer capacitance (C0) of 10FZO-400 was obtained by fitting the electrochemical response at different scan rates. dl The value is 49.5 μF cm⁻¹ -2 It is higher than the 30.4 μF cm⁻¹ of ZnO. -2 And ZnO-400's 9.6 μF cm -2 This indicates that 10FZO-400 has a larger effective electrochemical active interface. ZnO, after separate heat treatment, C dl The decrease may be related to particle growth and surface sintering caused by heat treatment. Introducing fluorine (F) can regulate the local structure and defect state of ZnO, which is beneficial for retaining more active sites that can participate in interfacial reactions.
[0046] Figure 9 The changes in current density and H2O2 Faradaic efficiency over time during the continuous electrolysis of 10FZO-400 for 8 h are shown. During continuous operation, the current density of 10FZO-400 remained stable overall, and the H2O2 Faradaic efficiency maintained a high level throughout the long electrolysis process without significant rapid decay, indicating that the prepared 10FZO-400 exhibits good electrocatalytic operational stability.
[0047] Example 7 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that in step (2), the air atmosphere was changed to an N2 atmosphere. The resulting catalyst was denoted as 10FZO-400-N2.
[0048] Under the same electrochemical testing conditions as in Example 1, the H2O2 Faradaic efficiency of 10FZO-400-N2 was 64.1%, which was lower than that of 10FZO-400 prepared under an air atmosphere, indicating that the calcination atmosphere has a significant impact on the structure formation and H2O2 selectivity of the FZO catalyst.
[0049] Example 8 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that in step (2), the air atmosphere was changed to an Ar atmosphere. The resulting catalyst was denoted as 10FZO-400-Ar.
[0050] Under the same electrochemical testing conditions as in Example 1, the H2O2 Faraday efficiency of 10FZO-400-Ar was 47.8%, which was also lower than that of 10FZO-400 prepared in an air atmosphere. This further indicates that a suitable oxygen-containing calcination atmosphere is beneficial to obtaining an FZO catalyst with better H2O2 generation performance.
[0051] Example 9 To facilitate performance comparison, the operation steps of Example 1 were repeated, except that in step (2), the heat preservation time was 0.5 h.
[0052] Under the same electrochemical testing conditions as in Example 1, the H2O2 Faradaic efficiency of the obtained FZO catalyst was 43.8%, which was lower than that of 10FZO-400 prepared in Example 1. This indicates that the short heat treatment time is not conducive to the formation of an FZO catalytic interface with better H2O2 generation performance.
[0053] Example 10 To facilitate performance comparison, the operation steps of Example 1 are repeated, except that in step (2), the heat preservation time is 4 h.
[0054] Under the same electrochemical testing conditions as in Example 1, the H2O2 Faradaic efficiency of the obtained FZO catalyst was 73.4%, which was lower than that of 10FZO-400 prepared in Example 1. This indicates that excessively long heat treatment time is also not conducive to obtaining better H2O2 generation performance of FZO catalyst.
[0055] The specific embodiments described above illustrate the technical solution and beneficial effects of the present invention in detail. It should be understood that the above description is only the most preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, additions, and equivalent substitutions made within the scope of the principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation, characterized in that, Includes the following steps: (1) ZnO and ZnF2 are mixed in a solid phase according to a set ratio and then ground thoroughly to obtain a mixed precursor; (2) The mixed precursor obtained in step (1) is calcined under a certain atmosphere, cooled and ground again to obtain the catalyst.
2. The method for preparing a catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation according to claim 1, characterized in that, In step (1), ZnF2 accounts for 1% to 60% of the total mass of ZnO and ZnF2.
3. The method for preparing a catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation according to claim 1, characterized in that, In step (2), the calcination temperature is 100-800 ℃.
4. The method for preparing a catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation according to claim 1, characterized in that, In step (2), the calcination atmosphere is at least one of air, oxygen, nitrogen and argon.
5. A method for preparing a catalytic material for the electrosynthesis of hydrogen peroxide from water oxidation according to claim 1, characterized in that, In step (2), the holding time after reaching the set calcination temperature is 1 to 8 hours.
6. A catalytic material prepared by the method according to any one of claims 1 to 5, characterized in that, The catalytic material has the ability to synthesize hydrogen peroxide by oxidizing water with two electrons at the anode.
7. The application of the catalytic material as described in claim 6 in the electrochemical synthesis of hydrogen peroxide by the oxidation of water with two electrons at the anode.
Citation Information
Patent Citations
Fluorinion-doped zinc oxide porous prism array film, and preparation and application thereof