A NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material, its preparation method and application
By growing a NiFe-LDH active layer in situ on the surface of carbon nanofibers, the problem of insufficient conductivity of NiFe-LDH electrocatalysts was solved, and efficient water electrolysis and oxygen evolution reaction of flexible self-supporting electrodes were realized. This simplified the electrode preparation process and improved the stability and mechanical durability of the catalyst.
Patent Information
- Application Number
- CN202611367963.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing NiFe-LDH electrocatalysts have poor conductivity and insufficient electron transport capacity. Furthermore, the use of polymer binders in the preparation of traditional composite catalysts leads to problems such as increased contact resistance, coverage of active sites, and blockage of mass transfer channels, which affect the stability and durability of the catalyst.
By growing a NiFe-LDH active layer in situ on the surface of carbon nanofibers, avoiding the use of polymer binders, flexible self-supporting carbon nanofiber composite materials were prepared by electrospinning and electrodeposition, maintaining good flexibility and catalytic activity.
This invention enables a self-supporting electrode that requires no external binder or conductive substrate, thereby improving electron transport capability and catalytic activity, simplifying the electrode preparation process, enhancing mechanical flexibility and structural stability, and lowering the energy barrier of the oxygen evolution reaction.
Smart Images

Figure CN123108609A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrocatalytic materials technology, and in particular to a NiFe-LDH supported flexible self-supporting carbon nanofiber composite material, its preparation method, and its application. Background Technology
[0002] With the deepening of energy structure transformation, the development and utilization of clean and renewable alternative energy sources has become a key focus in this field. Hydrogen energy, with its high energy density and clean, pollution-free combustion products, is considered one of the ideal energy carriers with development potential. Electrolysis of water to produce hydrogen has attracted widespread attention due to its wide availability of raw materials, low carbon emissions, and compatibility with renewable energy sources such as wind and solar power. The core of this technology lies in the electrocatalytic splitting of water, and its efficiency directly determines the economic viability and feasibility of the hydrogen production process.
[0003] Electrocatalytic water splitting involves two half-reactions: the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. The OER, involving a four-electron transfer process, exhibits relatively slow reaction kinetics and is a key factor limiting the improvement of water electrolysis efficiency. Therefore, developing efficient and stable OER electrocatalysts has always been a research focus in this field. Nickel-iron layered bimetallic hydroxides (NiFe-LDH), with their two-dimensional layered structure, abundant interlayer active sites, and synergistic electronic effects between Ni and Fe, are among the most studied OER catalysts, demonstrating good intrinsic catalytic activity. However, NiFe-LDH itself has poor electrical conductivity and insufficient electron transport capacity, restricting further improvements in its catalytic efficiency.
[0004] To address these issues, researchers attempted to composite NiFe-LDH with conductive carbon-based materials, leveraging the conductive carbon framework to improve the charge transport capacity of NiFe-LDH. However, existing composite catalysts are typically in powder form. In actual electrode fabrication, polymer binders such as perfluorosulfonic acid resin and polytetrafluoroethylene are required to coat them onto the surface of glassy carbon electrodes or conductive substrates such as nickel foam. These binders are insulating materials, and their introduction increases the contact resistance between the catalyst and the conductive substrate, affecting the rapid transfer of electrons. Simultaneously, the binders cover some active sites on the catalyst surface, blocking the pore structure within the catalyst layer, affecting electrolyte penetration and the release of gases generated during oxygen evolution, leading to a decrease in mass transfer efficiency. Furthermore, the binders may swell, age, or even detach during long-term electrolysis, causing deterioration of the electrical contact between the catalyst and the conductive substrate, affecting the stability and durability of the catalyst.
[0005] Self-supported electrodes, which eliminate the need for external binders and conductive substrates, represent one possible solution to the aforementioned problems. Carbon nanofibers have been studied as substrate materials for self-supported electrodes. However, carbon nanofiber materials obtained through conventional preparation methods are brittle and lack flexibility, making it difficult to meet the mechanical durability requirements of applications involving repeated bending. Some studies have attempted to improve this by introducing second-phase polymers or controlling the carbonization process; however, subsequent loading of active materials still often employs methods such as impregnation, coating, or hydrothermal growth, which suffer from weak adhesion between the active layer and the substrate, poor control of loading amount, and a tendency to agglomerate. Summary of the Invention
[0006] The purpose of this invention is to address the problems existing in the prior art by providing a NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material, its preparation method, and its applications. By growing a NiFe-LDH active layer in situ on the surface of carbon nanofibers, the use of polymer binders is avoided, while maintaining good flexibility and catalytic activity.
[0007] To achieve the above objectives, this invention provides a method for preparing a NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material, comprising the following steps: S1. Mix polyacrylonitrile, polyvinylpyrrolidone, nickel salt and solvent to obtain spinning solution; S2. Electrospin the spinning solution to obtain a carbon fiber precursor; S3. The carbon fiber precursor is subjected to pre-oxidation and carbonization treatments in sequence to obtain flexible self-supporting carbon nanofibers. S4. Using flexible self-supporting carbon nanofibers as working electrodes, electrodeposition is performed in an electrolyte containing nickel and iron sources to allow NiFe-LDH to grow in situ on the surface of flexible self-supporting carbon nanofibers, thus obtaining a NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material.
[0008] In some optional embodiments, in S1, the nickel salt is selected from nickel acetate; the nickel acetate is nickel acetate tetrahydrate; and the solvent is selected from N,N-dimethylformamide.
[0009] In some optional embodiments, in S1, the mixing temperature is 20-30°C. The mixing includes: mixing a nickel salt and a solvent to obtain a nickel salt solution; mixing polyacrylonitrile and the nickel salt solution to obtain a spinning solution; and mixing the spinning solution and polyvinylpyrrolidone to obtain a spinning solution.
[0010] In some optional embodiments, in S1, the mass of the polyacrylonitrile accounts for 8-15% of the total mass of the polyacrylonitrile, nickel salt and solvent (i.e., the mass fraction of polyacrylonitrile in the spinning solution is 8-15%); the mass of the polyvinylpyrrolidone accounts for 20-75% of the mass of the polyacrylonitrile.
[0011] In some optional embodiments, in S2, the applied voltage for electrospinning is 17-20kV, the distance from the needle to the receiver is 13-22cm, and the liquid supply rate is 0.5-1.5mL / h. The ambient humidity for electrospinning is 40-70%, and the temperature is 20-30℃.
[0012] In some optional embodiments, in S3, the pre-oxidation treatment is carried out at a temperature of 220-250°C for 1-3 hours. The pre-oxidation treatment causes the polyacrylonitrile molecular chains to undergo a cyclization reaction, forming a ladder-like structure and improving the thermal stability of the fiber. However, excessively high pre-oxidation temperatures can lead to uneven heating of the fiber, causing it to become brittle.
[0013] In some optional embodiments, in step S3, the carbonization treatment is carried out under an inert atmosphere; the heating rate of the carbonization treatment is 2-6°C / min, the target temperature is 700-900°C, and the holding time is 1-3 hours. Under the pre-oxidation and carbonization treatment conditions defined in this invention, the obtained carbon nanofibers maintain flexibility while exhibiting good electrical conductivity.
[0014] In some optional embodiments, in S4, the nickel source is selected from nickel nitrate; the nickel nitrate is nickel nitrate hexahydrate; the iron source is selected from ferric nitrate; the ferric nitrate is ferric nitrate nonahydrate; the molar ratio of nickel to iron in the electrolyte is (3-5):1; and the total concentration of nickel and iron in the electrolyte is 0.1-0.5 mol / L.
[0015] In some optional embodiments, in S4, the electrodeposition counter electrode is a platinum sheet electrode, and the reference electrode is an Ag / AgCl electrode.
[0016] In some optional embodiments, in S4, the electrodeposition voltage is -0.8 to -1.2 V (relative to the Ag / AgCl electrode), and the time is 600-1500 s. Under the electrodeposition conditions defined in this invention, the formation of NiFe-LDH and the improvement of OER performance are beneficial. However, excessively long deposition times lead to increased NiFe-LDH nanosheet thickness, increased mass transfer resistance, and decreased intrinsic activity.
[0017] In some alternative embodiments, in S4, after electrodeposition, the material is dried to obtain a NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material.
[0018] The present invention also provides a NiFe-LDH supported flexible self-supporting carbon nanofiber composite material, which is prepared by the preparation method described above.
[0019] In some optional embodiments, the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material has a pore size of 3-5 nm and a specific surface area of 30-100 m². 2 / g.
[0020] The present invention also provides the application of the aforementioned NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material in the oxygen evolution reaction of water electrolysis.
[0021] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention uses polyacrylonitrile, polyvinylpyrrolidone and nickel salt as raw materials to prepare spinning solution. After electrospinning, pre-oxidation treatment and carbonization treatment, flexible self-supporting carbon nanofibers are obtained. Then, NiFe-LDH active layer is grown in situ on the surface of carbon nanofibers by electrodeposition method, which avoids the problems of increased contact resistance, coverage of active sites and blockage of mass transfer channels caused by the use of polymer adhesives in the traditional electrode preparation process.
[0022] (2) By adding an appropriate amount of polyvinylpyrrolidone to the spinning solution, the present invention utilizes its optimization effect on the polymer interwoven network inside the fiber during the spinning and forming stage, as well as the stress buffer structure formed by pyrolysis during the pre-oxidation and carbonization process, so that the obtained carbon nanofibers can still maintain the conductive network after bending, and have good mechanical flexibility and structural integrity.
[0023] (3) This invention improves the conductivity of carbon nanofibers by introducing nickel acetate into the spinning solution. The resulting composite material has a three-dimensional interwoven porous fiber network structure, which can construct conductive and mass transfer channels, and is beneficial for electron transport and diffusion of electrolyte and bubbles.
[0024] (4) By controlling the concentration ratio of Ni to Fe in the electrolyte during the electrodeposition process, the present invention enables NiFe-LDH nanosheets to be uniformly loaded on the surface of carbon nanofibers, and the loading amount is controllable, thus avoiding the problems of weak bonding between the active layer and the substrate, uneven loading, and easy agglomeration in traditional impregnation, coating or hydrothermal growth methods.
[0025] (5) In this invention, there is a catalytic synergistic effect between the carbon nanofiber conductive framework and the NiFe-LDH active layer, which can reduce the energy barrier and overpotential of the oxygen evolution reaction and improve the catalytic activity and structural stability of the electrode.
[0026] (6) The flexible self-supporting carbon nanofiber composite material supported by NiFe-LDH prepared by the present invention can be directly used as a self-supporting electrode for the oxygen evolution reaction of water electrolysis without the need for external adhesives and conductive substrates, which simplifies the electrode preparation process. Attached Figure Description
[0027] Figure 1 This is a SEM characterization image of the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material in Example 1 of this invention. Figure 2 This is a SEM characterization image of the flexible self-supporting carbon nanofibers in Comparative Example 1 of this invention. Figure 3 This is a schematic diagram of the bending of the flexible self-supporting carbon nanofiber in Comparative Example 1 of the present invention; Figure 3 In the diagram, 'a' represents the unbent state, while 'b', 'c', and 'd' represent diagrams under different bending conditions. Figure 4 These are X-ray diffraction characterization diagrams of the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material in Example 1 of the present invention and the flexible self-supporting carbon nanofiber in Comparative Example 1. Figure 5 These are the nitrogen adsorption-desorption curves and pore size distribution diagrams of the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material in Example 1 of this invention and the flexible self-supporting carbon nanofiber in Comparative Example 1. Figure 5 In the diagram, 'a' represents the nitrogen adsorption-desorption curve, and 'b' represents the pore size distribution. Figure 6 These are comparison graphs of linear scanning voltammetric curves of the flexible self-supporting carbon nanofiber composite materials supported by NiFe-LDH in Examples 1-3 of this invention. Figure 7 This is a comparison diagram of the Tafel slope of the flexible self-supporting carbon nanofiber composite materials supported by NiFe-LDH in Examples 1-3 of this invention; Figure 8 These are comparative electrochemical impedance spectroscopy diagrams of the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite materials in Examples 1-3 of this invention. Figure 9 This is a comparison chart of linear scanning voltammetric curves of different materials in Embodiment 1, Comparative Example 1, and Comparative Example 2 of the present invention. Detailed Implementation
[0028] The following embodiments are provided to better understand the present invention and are not limited to the described embodiments. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0029] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0030] Example 1 This embodiment provides a method for preparing NiFe-LDH-supported flexible self-supporting carbon nanofiber composite materials, including the following steps: 0.5 g of nickel acetate tetrahydrate and 10 mL of N,N-dimethylformamide were mixed at 25 °C to obtain a nickel salt solution. Polyacrylonitrile and the nickel salt solution were mixed at 25 °C to obtain a spinning solution with a polyacrylonitrile mass fraction of 9.3%. The spinning solution and polyvinylpyrrolidone were mixed at 25 °C to obtain a spinning bath, with polyvinylpyrrolidone comprising 25% of the mass of polyacrylonitrile.
[0031] Electrospinning was performed on the spinning solution. The applied voltage for electrospinning was set to 20kV, the distance from the needle to the receiver was 17cm, the liquid supply rate was 1mL / h, the ambient humidity was 55%, and the temperature was 25℃, thus obtaining the carbon fiber precursor.
[0032] The carbon fiber precursor was placed in a forced-air drying oven and pre-oxidized at 230℃ for 2 hours. After pre-oxidation, carbonization was carried out under a nitrogen atmosphere, with the temperature increased to 800℃ at a rate of 5℃ / min and held for 2 hours to obtain flexible self-supporting carbon nanofibers.
[0033] Flexible self-supporting carbon nanofibers were cut into 1cm × 2cm pieces and used as the working electrode, with a platinum sheet electrode as the counter electrode and an Ag / AgCl electrode as the reference electrode. The electrolyte was prepared by dissolving nickel nitrate hexahydrate and ferric nitrate nonahydrate in 30mL of water to obtain a mixed solution with a Ni to Fe molar ratio of 4:1 and a total Ni and Fe concentration of 0.5mol / L. The working voltage was set to -1.0V (relative to the Ag / AgCl reference electrode), and the deposition time was 1200s. Electrodeposition was performed on the surface of the flexible self-supporting carbon nanofibers to allow NiFe-LDH to grow in situ on the surface. After electrodeposition, the resulting product was placed in a vacuum oven and dried at 60℃ for 12h to obtain the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material.
[0034] Example 2 The only difference between this embodiment and Embodiment 1 is that the molar ratio of Ni to Fe in the mixed solution is adjusted to 3:1.
[0035] Example 3 The only difference between this embodiment and Embodiment 1 is that the molar ratio of Ni to Fe in the mixed solution is adjusted to 5:1.
[0036] Comparative Example 1 The only difference between this comparative example and Example 1 is that the electrodeposition step is omitted; that is, the process is terminated after the flexible self-supporting carbon nanofibers are prepared.
[0037] Comparative Example 2 The only difference between this comparative example and Example 1 is that the addition of polyvinylpyrrolidone is omitted.
[0038] Experimental Example 1 Scanning electron microscopy (SEM) analysis was performed on the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material prepared in Example 1 and the flexible self-supporting carbon nanofiber prepared in Comparative Example 1. The SEM characterization images of the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material in Example 1 are shown below. Figure 1 As shown; SEM characterization image of the flexible self-supporting carbon nanofibers in Comparative Example 1, as shown. Figure 2 As shown.
[0039] Depend on Figure 1 As can be seen, NiFe-LDH exhibits a two-dimensional nanosheet structure and is uniformly distributed on the surface of flexible, self-supporting carbon nanofibers. Figure 2 It can be seen that the fibers are of uniform thickness and have a rich porous structure on the fiber surface, which may be one of the reasons for their good flexibility.
[0040] Experiment Example 2 The flexibility of the flexible self-supporting carbon nanofibers prepared in Comparative Example 1 was tested, and a bending diagram of the flexible self-supporting carbon nanofibers in Comparative Example 1 was obtained, as shown in the figure. Figure 3 As shown; Figure 3 In the diagram, 'a' represents the unbent state, while 'b', 'c', and 'd' represent diagrams showing different bending conditions. Figure 3 It can be seen that the prepared flexible self-supporting carbon nanofibers can be bent and folded without breaking, indicating that they have good flexibility.
[0041] Experimental Example 3 X-ray diffraction analysis was performed on the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material prepared in Example 1 and the flexible self-supporting carbon nanofiber prepared in Comparative Example 1. The X-ray diffraction characterization patterns of the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material in Example 1 and the flexible self-supporting carbon nanofiber in Comparative Example 1 are shown below. Figure 4 As shown. By Figure 4As can be seen, the XRD pattern of Example 1 shows characteristic diffraction peaks corresponding to the NiFe-LDH standard card, indicating that NiFe-LDH has been successfully loaded onto the surface of flexible self-supporting carbon nanofibers.
[0042] Experiment Example 4 Nitrogen adsorption-desorption tests were performed on the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material prepared in Example 1 and the flexible self-supporting carbon nanofiber prepared in Comparative Example 1 to analyze the specific surface area and pore size distribution. The nitrogen adsorption-desorption curves and pore size distribution diagrams of the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material in Example 1 and the flexible self-supporting carbon nanofiber in Comparative Example 1 were obtained, as shown below. Figure 5 As shown; Figure 5 In the diagram, 'a' represents the nitrogen adsorption-desorption curve, and 'b' represents the pore size distribution. Figure 5 It can be seen that both isotherms exhibit the characteristics of type IV isotherms, indicating that both materials are predominantly mesoporous. Calculations show that the specific surface area of the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material prepared in Example 1 is 61 m². 2 / g, with a pore size of 4.68nm; the specific surface area of the flexible self-supporting carbon nanofibers prepared in Comparative Example 1 was 118m². 2 / g, with a pore size of 5.01nm. The above results indicate that the flexible self-supporting carbon nanofibers themselves have abundant porous structures, while the loading of NiFe-LDH will cover some of the pores on the surface of the carbon nanofibers, resulting in a decrease in both the specific surface area and pore size of the composite material.
[0043] Experimental Example 5 The oxygen evolution reaction electrocatalytic performance of the NiFe-LDH supported flexible self-supporting carbon nanofiber composite materials prepared in Examples 1-3 and the comparative samples prepared in Comparative Examples 1-2 were tested. Figure 6 This is a comparison of the linear sweep voltammetry curves of the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composites in Examples 1-3. Figure 7 This is a comparison of the Tafel slopes of the NiFe-LDH-loaded flexible self-supporting carbon nanofiber composites in Examples 1-3. Figure 8 This is a comparison of the electrochemical impedance spectroscopy (EIS) of the NiFe-LDH-supported flexible self-supporting carbon nanofiber composites in Examples 1-3. Figure 9 The graph shows a comparison of linear scanning voltammetric curves of different materials in Example 1, Comparative Example 1, and Comparative Example 2.
[0044] Depend on Figure 6-8 It can be seen that the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material prepared in Example 1 has a performance of 10 mA / cm². 2The overpotential at the current density was 207 mV, the Tafel slope was 208 mV / dec, and the electrochemical impedance was 1.2 Ω. The overpotential of the composite material prepared in Example 2 was 209 mV, the Tafel slope was 259 mV / dec, and the electrochemical impedance was 3.6 Ω. The overpotential of the composite material prepared in Example 3 was 243 mV, the Tafel slope was 261 mV / dec, and the electrochemical impedance was 6.6 Ω. These results indicate that when the molar ratio of Ni to Fe in the electrolyte is 4:1, the prepared composite material exhibits the lowest overpotential, the smallest Tafel slope, and the lowest electrochemical impedance, demonstrating optimal electrocatalytic performance for the oxygen evolution reaction, the fastest reaction kinetic rate, and the highest charge transfer efficiency.
[0045] Depend on Figure 9 It can be seen that the overpotential of the flexible self-supporting carbon nanofibers prepared in Comparative Example 1 is 513 mV, the overpotential of the NiFe-LDH-supported carbon nanofiber material prepared in Comparative Example 2 (coated to the glassy carbon electrode with an adhesive) is 289 mV, and the overpotential of Example 1 is 207 mV. The overpotential of Comparative Example 1 is the highest because it lacks the NiFe-LDH active component and has a single active site. Comparative Example 2 uses an adhesive to coat the catalyst to the glassy carbon electrode, which increases the contact resistance and limits the mass transfer efficiency during the reaction process. Therefore, its catalytic performance is lower than that of Example 1.
[0046] In summary, this invention prepares a spinning solution using polyacrylonitrile, polyvinylpyrrolidone, and nickel salt. This solution is then electrospun, pre-oxidized, and carbonized to obtain flexible, self-supporting carbon nanofibers. These carbon nanofibers are then used as working electrodes, and NiFe-LDH is grown in situ on the surface of the carbon nanofibers via electrodeposition in an electrolyte containing nickel and iron sources. This results in a NiFe-LDH-loaded flexible, self-supporting carbon nanofiber composite material. This material avoids the use of polymer binders in traditional electrode fabrication processes, simplifying the electrode preparation process, while exhibiting good mechanical flexibility and structural integrity. The catalytic synergistic effect between the conductive carbon nanofiber framework and the NiFe-LDH active layer helps lower the oxygen evolution reaction energy barrier, enhancing the catalytic activity and stability of the electrode, and demonstrating good application potential in the oxygen evolution reaction of water electrolysis.
[0047] Finally, it should be noted that the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A method for preparing a NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material, characterized in that, Includes the following steps: S1. Mix polyacrylonitrile, polyvinylpyrrolidone, nickel salt and solvent to obtain spinning solution; S2. Electrospin the spinning solution to obtain a carbon fiber precursor; S3. The carbon fiber precursor is subjected to pre-oxidation and carbonization treatments in sequence to obtain flexible self-supporting carbon nanofibers. S4. Using flexible self-supporting carbon nanofibers as working electrodes, electrodeposition is performed in an electrolyte containing nickel and iron sources to allow NiFe-LDH to grow in situ on the surface of flexible self-supporting carbon nanofibers, thus obtaining a NiFe-LDH-loaded flexible self-supporting carbon nanofiber composite material.
2. The preparation method according to claim 1, characterized in that, In S1, the nickel salt is selected from nickel acetate; the solvent is selected from N,N-dimethylformamide.
3. The preparation method according to claim 1, characterized in that, In S1, the mass of the polyacrylonitrile accounts for 8-15% of the total mass of the polyacrylonitrile, nickel salt, and solvent; the mass of the polyvinylpyrrolidone accounts for 20-75% of the mass of the polyacrylonitrile.
4. The preparation method according to claim 1, characterized in that, In S2, the applied voltage for electrospinning is 17-20kV, the distance from the needle to the receiver is 13-22cm, and the liquid supply rate is 0.5-1.5mL / h.
5. The preparation method according to claim 1, characterized in that, In S3, the pre-oxidation treatment is carried out at a temperature of 220-250℃ for 1-3 hours.
6. The preparation method according to claim 1, characterized in that, In S3, the heating rate of the carbonization treatment is 2-6℃ / min, the target temperature is 700-900℃, and the holding time is 1-3h.
7. The preparation method according to claim 1, characterized in that, In S4, the nickel source is selected from nickel nitrate; the iron source is selected from ferric nitrate; and the molar ratio of nickel to iron in the electrolyte is (3-5):
1.
8. The preparation method according to claim 1, characterized in that, In S4, the electrodeposition operation voltage is -0.8 to -1.2V, and the time is 600-1500s.
9. A flexible self-supporting carbon nanofiber composite material supported by NiFe-LDH, characterized in that, It is prepared by the preparation method according to any one of claims 1-8.
10. The application of the NiFe-LDH-supported flexible self-supporting carbon nanofiber composite material according to claim 9 in the oxygen evolution reaction of water electrolysis.