Hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction and its preparation method
The in-situ reconstruction method induced by pulsed current solves the problem of low reconstruction efficiency of hydrogen evolution electrodes under high current density, achieves high activity and stability of electrode surface, is applicable to a variety of catalytic materials and substrates, and improves the efficiency of hydrogen production by water electrolysis.
Patent Information
- Application Number
- CN202611475781.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing hydrogen evolution electrodes suffer from low reconstruction efficiency at high current densities, difficulty in precisely controlling the degree of reconstruction, insufficient generation of active sites, and poor long-term stability, resulting in low efficiency of hydrogen production through water electrolysis.
An in-situ reconstruction method based on pulsed current is adopted. By adjusting the peak current density, frequency, duty cycle, waveform and reconstruction time, an initial hydrogen evolution catalyst layer is constructed and a programmable pulsed current is applied in an alkaline electrolyte to achieve controllable in-situ reconstruction of the electrode surface.
It achieves synergistic optimization of the electrode surface microstructure and electronic structure, forming a defect-rich and highly active reconstructed interface, which improves catalytic activity and stability, and is applicable to a variety of catalytic materials and substrates.
Smart Images

Figure CN123108619A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of water electrolysis for hydrogen production and catalysis technology, specifically relating to a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction and its preparation method. Background Technology
[0002] Currently, nickel-based, nickel-iron-based, and their derivative electrodes are commonly used as cathode hydrogen evolution electrodes in industrial electrolyzers. However, under high current density operating conditions, alkaline water electrolysis and anion exchange membrane (AEM) water electrolysis have become important renewable energy hydrogen production technologies due to their advantages of being green, efficient, and easy to scale up. As a key component of the water electrolysis system, the catalytic activity and long-term stability of the hydrogen evolution electrode directly affect the energy consumption and operational life of the electrolyzer. In recent years, researchers have continuously improved the performance of the hydrogen evolution reaction (HER) by developing catalytic materials such as nickel-based alloys, transition metal phosphides, sulfides, nitrides, and high-entropy alloys. However, in actual operation, the surface composition, crystal structure, and electronic state of most HER catalysts undergo continuous dynamic changes with the electrochemical reaction, ultimately forming the active interface that truly participates in the catalytic reaction—the so-called in-situ reconstruction process. Therefore, how to effectively control the in-situ reconstruction process of the electrode has become an important research direction for improving HER performance.
[0003] Currently, the activation of hydrogen evolution electrodes mainly employs traditional electrochemical methods such as constant current, constant potential, or cyclic voltammetry. These activation methods have relatively singular energy inputs, making it difficult to precisely control the reconstruction rate, reconstruction depth, and defect formation process on the electrode surface. This results in significant differences in the degree of reconstruction between different electrodes, and poor consistency and repeatability of the reconstruction interface. Furthermore, traditional activation methods typically suffer from low reconstruction efficiency, insufficient active site generation, and limited long-term stability. Therefore, developing a novel preparation method that enables precise control of the in-situ reconstruction process of the electrode through controllable current input is of great significance for constructing highly active and stable hydrogen evolution electrodes, improving the efficiency of hydrogen production through water electrolysis, and promoting its industrial application. Summary of the Invention
[0004] To address the problems of low reconstruction efficiency, difficulty in precisely controlling the degree of reconstruction, insufficient generation of active sites, and poor long-term operational stability in the activation process of existing hydrogen evolution electrodes, this invention proposes a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction and its preparation method.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: The preparation method of hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction includes: Select a conductive substrate and pretreat it; An initial hydrogen evolution catalytic layer was constructed on the surface of the treated conductive substrate to obtain an initial hydrogen evolution electrode. The obtained initial hydrogen evolution electrode was placed in an alkaline electrolyte as the working electrode to build a three-electrode or two-electrode electrochemical system. Based on the constructed three-electrode or two-electrode electrochemical system, a programmable pulsed current is applied to the initial hydrogen evolution electrode for in-situ reconstruction. By controlling the peak current density, pulse frequency, duty cycle, pulse width, pulse waveform and reconstruction time, the catalyst layer undergoes controllable in-situ reconstruction, forming a defect-rich and highly active reconstruction interface on the electrode surface. After in-situ reconstruction is completed, the pulsed current treatment is stopped, the electrode is removed, the residual electrolyte is removed, and it is dried to obtain a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction.
[0006] A further improvement of the present invention is that the conductive substrate is one or more of the following: nickel foam, nickel mesh, titanium mesh, stainless steel mesh, copper mesh, carbon cloth, carbon paper, or conductive foam.
[0007] A further improvement of the present invention is that the selected conductive substrate is pretreated, including degreasing, deoxidizing, and surface cleaning. The pretreatment includes: first, ultrasonically cleaning the conductive substrate sequentially with acetone, anhydrous ethanol, and deionized water to remove surface oil and impurities, with ultrasonic cleaning times ranging from 5 to 30 minutes; then, acid washing with one of hydrochloric acid, sulfuric acid, or nitric acid to remove the oxide layer on the surface of the conductive substrate, with an acid washing time ranging from 10 seconds to 10 minutes; after acid washing, thoroughly rinsing with deionized water until neutral, and then drying.
[0008] A further improvement of the present invention is that the initial hydrogen evolution catalyst layer is one or more of the following: nickel-based alloy, nickel-molybdenum alloy, nickel-iron alloy, nickel-cobalt alloy, metal phosphide, sulfide, nitride, carbide, high-entropy alloy or composite material thereof; the thickness of the catalyst layer is 0.1 to 100 μm.
[0009] A further improvement of the present invention is that the alkaline electrolyte is a 0.1-10 mol / L potassium hydroxide solution or sodium hydroxide solution; and the electrolyte temperature is 20-90 °C.
[0010] A further improvement of this invention is that the peak current density of the pulse current is 50–5000 mA / cm². 2 The pulse frequency is 0.01–1000 Hz, the duty cycle is 5%–95%, the single pulse width is 0.1 ms–10 s, and the reconstruction time is 1 min–24 h.
[0011] A further improvement of the present invention is that the pulse waveform is one or a combination of square wave, stepped wave, triangular wave, sine wave or exponential wave.
[0012] A further improvement of the present invention is that the pulse current parameters adopt a constant mode or a program control mode. In the program control mode, one or more parameters among the peak current density, frequency and duty cycle can be continuously or in stages adjusted with the reconstruction time to achieve in-situ reconstruction at different stages.
[0013] A further improvement of the present invention is that the drying method is natural drying, forced air drying or vacuum drying, the drying temperature is 25-80 ℃, and the time is 0.5-12 h.
[0014] The hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction was prepared using the aforementioned preparation method.
[0015] Compared with the prior art, the present invention has at least the following beneficial technical effects: The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction provided by this invention achieves synergistic optimization of the electrode surface microstructure, defect structure and electronic structure by constructing a dynamic evolution process of "initial hydrogen evolution catalytic layer - pulsed current-induced reconstruction layer - in-situ active interface", thereby obtaining a hydrogen evolution electrode with high catalytic activity and excellent stability.
[0016] Specifically, this invention first constructs an initial hydrogen evolution catalyst layer on the surface of a conductive substrate. Subsequently, the resulting electrode is placed in an alkaline electrolyte, and a programmable pulsed current is applied for electrochemical treatment. Unlike traditional constant current activation methods, this invention induces a controllable in-situ reconstruction of the catalyst layer by controlling the peak current density, frequency, duty cycle, waveform, and duration of the pulsed current, causing the electrode surface to undergo periodic oxidation-reduction and hydrogen evolution processes.
[0017] During the pulsed current process, the instantaneous high current density causes periodic changes in the local electric field, charge distribution, and ion concentration on the electrode surface, promoting the continuous generation and recombination of the active phase on the catalyst layer surface. Simultaneously, the intermittent phases of the pulsed current facilitate the redispersion of ions in the electrolyte and the recovery of the reaction interface, mitigating concentration polarization and localized overheating caused by continuous high current, thereby achieving a more uniform and efficient interface reconstruction process.
[0018] Furthermore, pulsed current-induced dynamic reconstruction can promote the formation of abundant lattice defects, low-coordination atoms, grain boundary structures, and active phase interfaces on the electrode surface, while optimizing the electronic structure of the catalyst surface and improving the adsorption and desorption capabilities of reaction intermediates. Compared with the traditional constant current activation method, the in-situ reconstructed interface obtained by this invention has a higher active site density, a faster electron transport rate, and a more stable interface structure.
[0019] The pulse current parameters in this invention can be adjusted according to different catalytic materials, including peak current density, pulse frequency, duty cycle, pulse width, and waveform. The pulse waveform can be a square wave, step wave, triangular wave, sine wave, or a combination thereof to achieve different degrees of in-situ reconstruction. By optimizing the pulse parameters, the reconstruction depth of the catalytic layer and the formation process of the active interface can be precisely controlled, improving the applicability to different catalytic systems.
[0020] The pulsed current-induced in-situ reconstruction method proposed in this invention does not depend on a specific catalytic material system and can be widely applied to nickel-based alloys, nickel-molybdenum alloys, nickel-iron alloys, nickel-cobalt alloys, metal phosphides, sulfides, nitrides, high-entropy alloys, and other hydrogen evolution catalysts. It is also applicable to various conductive substrates such as nickel foam, nickel mesh, titanium mesh, carbon cloth, and carbon paper. This invention features a simple process, controllable parameters, good repeatability, and is easily integrated with existing water electrolysis electrode preparation processes, demonstrating promising industrial application prospects. Attached Figure Description
[0021] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0022] Figure 1 This is a flowchart of catalyst preparation.
[0023] Figure 2 The XRD pattern of the NiMo precursor was obtained.
[0024] Figure 3 The image shows the electrode XRD pattern of the NiMo precursor after reduction treatment in a hydrogen-argon atmosphere.
[0025] Figure 4 SEM images of the catalyst at different treatment stages.
[0026] Figure 5 This is a comparison chart of catalyst performance. Detailed Implementation
[0027] In the following description, only certain exemplary embodiments are briefly described. As those skilled in the art will recognize, the described embodiments can be modified in various ways without departing from the spirit or scope of the invention. Therefore, the drawings and description are considered to be exemplary in nature and not restrictive.
[0028] In the description of this invention, it should be understood that, when used in this specification and the appended claims, the terms "comprising" and "including" indicate the presence of the described features, integrals, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components and / or collections thereof.
[0029] It should also be understood that the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” are intended to include the plural forms unless the context clearly indicates otherwise.
[0030] It should also be further understood that the term "and / or" as used in this specification and the appended claims refers to any combination of one or more of the associated listed items and all possible combinations, and includes such combinations.
[0031] The accompanying drawings illustrate various structural schematic diagrams according to embodiments disclosed in this invention. These drawings are not to scale, and some details have been enlarged for clarity, and some details may have been omitted. The shapes of the various regions and layers shown in the drawings, as well as their relative sizes and positional relationships, are merely exemplary and may deviate from reality due to manufacturing tolerances or technical limitations. Furthermore, those skilled in the art can design regions / layers with different shapes, sizes, and relative positions as needed.
[0032] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0033] like Figure 1 As shown, the method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction provided by the present invention includes: (1) Select a conductive substrate and perform degreasing, deoxidation and surface cleaning treatments on it to obtain a clean conductive substrate; The conductive substrate is one or more of the following: nickel foam, nickel mesh, titanium mesh, stainless steel mesh, copper mesh, carbon cloth, carbon paper, or conductive foam. Cleaning methods include ultrasonic cleaning with acetone, anhydrous ethanol, and deionized water, with ultrasonic times ranging from 5 to 30 minutes; the pickling solution is one of hydrochloric acid, sulfuric acid, or nitric acid, with a pickling time ranging from 10 seconds to 10 minutes.
[0034] (2) An initial hydrogen evolution catalyst layer is constructed on the surface of the conductive substrate. The catalyst layer can be prepared by one or more methods such as electrodeposition, chemical plating, hydrothermal growth, spraying, magnetron sputtering, electrophoretic deposition, in-situ growth or laser cladding to obtain the initial hydrogen evolution electrode. The initial hydrogen evolution catalyst layer is one or more of the following: nickel-based alloy, nickel-molybdenum alloy, nickel-iron alloy, nickel-cobalt alloy, metal phosphide, sulfide, nitride, carbide, high-entropy alloy or composite material; the thickness of the catalyst layer is 0.1 to 100 μm.
[0035] (3) Place the initial hydrogen evolution electrode obtained in step (2) as the working electrode in an alkaline electrolyte to build a three-electrode or two-electrode electrochemical system; The electrolyte is a 0.1–10 mol / L potassium hydroxide solution, sodium hydroxide solution, or other alkaline electrolyte; the electrolyte temperature is 20–90 ℃.
[0036] (4) Apply a programmable pulsed current to the initial hydrogen evolution electrode for in-situ reconstruction. By adjusting the peak current density, pulse frequency, duty cycle, pulse width, pulse waveform and reconstruction time, the catalyst layer undergoes controllable in-situ reconstruction, forming a defect-rich and highly active reconstruction interface on the electrode surface. The peak current density of the pulse current is 50–5000 mA / cm². 2 The pulse frequency ranges from 0.01 to 1000 Hz, the duty cycle from 5% to 95%, the pulse width from 0.1 ms to 10 s, and the reconstruction time from 1 min to 24 h. The pulse current parameters can be in constant mode or program control mode. In program control mode, one or more parameters among peak current density, frequency, and duty cycle can be continuously or in stages adjusted with the reconstruction time to achieve in-situ reconstruction at different stages.
[0037] (5) After the in-situ reconstruction is completed, stop the pulse current treatment, take out the electrode, wash it with deionized water to remove the residual electrolyte, and dry it to obtain the hydrogen evolution electrode based on pulse current induced in-situ reconstruction.
[0038] The drying methods include natural drying, forced air drying, or vacuum drying, with a drying temperature of 25–80 ℃ and a drying time of 0.5–12 h.
[0039] Natural drying is a static drying method under normal temperature and pressure. It relies on ambient air convection to remove residual deionized water from the electrode surface. The process temperature is fixed at around room temperature (around 25°C), and the drying time is controlled between 0.5 and 12 hours. This drying method requires no external equipment, is simple to operate, and involves no external force intervention. It does not cause mechanical or thermal damage to the electrode microstructure and active site structure formed by in-situ reconstruction with pulsed current, and can preserve the original catalytic structure of the electrode to the greatest extent. However, its drying efficiency is low, it is greatly affected by ambient temperature and humidity, and the drying uniformity is generally poor. It is only suitable for preparation scenarios where the residual electrolyte on the electrode surface is small, drying efficiency is not required, and structural integrity is the priority.
[0040] Forced air drying is a process that achieves drying by using forced air convection within a constant-temperature oven. The drying temperature can be precisely controlled within the range of 25–80℃. A fan drives constant-temperature air to continuously sweep across the electrode surface, accelerating moisture evaporation. Compared to natural drying, forced convection significantly increases the drying rate and shortens the drying time. Simultaneously, the uniform temperature field inside the oven ensures uniform drying of the entire electrode, effectively avoiding surface water residue and uneven drying in certain areas. This process is characterized by low equipment cost, convenient operation, and strong controllability. It is suitable for most post-processing scenarios of hydrogen evolution electrodes, and the temperature gradient can be adapted to electrode materials with different structural stability. It is a conventional drying method for in-situ reconstructed electrodes.
[0041] Vacuum drying relies on vacuum drying equipment to remove moisture under negative pressure and low atmospheric pressure, with an operating temperature range of 25–80℃. The negative pressure environment significantly reduces the saturated vapor pressure of water, allowing moisture to rapidly vaporize and evaporate at low temperatures. This achieves efficient drying while avoiding thermal damage to the active components and microporous structure of the electrode surface caused by high temperatures. Simultaneously, the vacuum-sealed environment, free from oxygen and dust interference, effectively prevents oxidation of the active sites and surface contamination of the reconstructed electrode, maximizing the preservation of the electrode's hydrogen evolution catalytic performance. This method offers thorough drying, high purity, and excellent protection, making it particularly suitable for the post-processing of highly active, easily oxidized, and porous precision hydrogen evolution electrodes.
[0042] Example 1: Taking the fabrication of a biomimetic leaf vein structure NiMo self-breathing hydrogen evolution electrode as an example, the steps are as follows: 1) Prepare 100 mL of a mixed solution consisting of 0.08 mol / L nickel sulfate, 0.04 mol / L ammonium molybdate, 0.15 mol / L urea and 0.05 mol / L sodium citrate.
[0043] 2) The above mixed solution was transferred to a 150 mL polytetrafluoroethylene-lined reactor, with a solution filling rate of 66.7%. A prepared nickel foam electrode was placed in the reactor, and the reaction was carried out hydrothermally at 160 °C for 8 h. After the reaction was completed, the reactor was allowed to cool naturally to room temperature. The nickel foam substrate was then removed and ultrasonically cleaned three times with deionized water and anhydrous ethanol, respectively. Finally, it was vacuum dried at 60 °C for 6 h to obtain a nickel foam electrode supported on the Ni-Mo precursor.
[0044] 3) The sample obtained in step 2) was placed in a hydrogen-argon mixed atmosphere (5% H2 / 95% Ar) for heat treatment. The heating rate was 5 °C / min, the holding temperature was 450 °C, and the holding time was 2 h. After natural cooling, the NiMo catalytic active layer was obtained.
[0045] 4) Polystyrene microspheres with particle sizes of 20 μm, 100 μm, and 300 μm were mixed at a mass ratio of 1:2:3 and uniformly sprayed onto the surface of the NiMo catalyst layer, and dried at 80 °C for 4 h. Subsequently, the mixture was treated at 350 °C for 2 h under a nitrogen atmosphere to remove the template, forming a gradient pore size gas-conducting layer with a gradual transition from small pores to large pores.
[0046] 5) A femtosecond laser was used to fabricate a biomimetic leaf vein structure on the surface of the air-conducting layer. The main vein channel has a width of 800 μm and a depth of 300 μm; the lateral vein channel has a width of 150 μm and a depth of 80 μm; the angle between the lateral vein and the main vein is 45°. The laser power is 15 W, the scanning speed is 1200 mm / s, and the scanning interval is 50 μm.
[0047] 6) The central region of the electrode was treated with oxygen plasma for 5 min to form a superhydrophilic surface; then, the leaf vein gas-conducting region was sprayed with a 1% (w / w) fluorosilane ethanol solution for 30 min. After drying, a wettability gradient structure was formed, in which the water contact angle of the catalytic region was about 8° and the contact angle of the leaf vein gas-conducting region was about 135°.
[0048] 7) Finally, a self-breathing hydrogen evolution electrode with a multi-level structure of "catalytic active layer - gradient pore size gas guiding layer - biomimetic leaf vein gas guiding network" was obtained.
[0049] The resulting electrode was used in a 1 mol / L KOH electrolyte for the hydrogen evolution reaction at the cathode of alkaline water electrolysis.
[0050] Example 2: In Example 1, step 1), the catalyst precursor system was changed from 0.08 mol / L nickel sulfate and 0.04 mol / L ammonium molybdate to 0.06 mol / L nickel nitrate, 0.02 mol / L ferric nitrate and 0.02 mol / L cobalt nitrate, while the other steps remained unchanged.
[0051] After hydrothermal reaction and heat treatment, a NiFeCo composite catalyst layer was obtained, and a gradient pore size air guiding layer, a biomimetic leaf vein air guiding network, and a wettability gradient structure were constructed according to steps 4) to 6) of Example 1.
[0052] The biomimetic self-breathing NiFeCo hydrogen evolution electrode prepared according to the above steps is used for the hydrogen evolution reaction at the cathode of alkaline water electrolysis.
[0053] Example 3: The catalyst precursor system in step 1) of Example 1 was changed to 0.02 mol / L ferric sulfate, 0.02 mol / L cobalt sulfate, 0.02 mol / L nickel sulfate, 0.02 mol / L copper sulfate and 0.02 mol / L manganese sulfate, while the other steps remained unchanged.
[0054] A FeCoNiCuMn multi-element alloy catalyst layer is formed after electrodeposition and heat treatment.
[0055] Subsequently, the gradient pore size air-conducting layer, the biomimetic leaf vein air-conducting network, and the wettability gradient structure are constructed according to steps 4) to 6) of Example 1.
[0056] The biomimetic self-breathing FeCoNiCuMn hydrogen evolution electrode prepared according to the above steps can be used as an alkaline water electrolysis cathode.
[0057] Example 4: In Example 1, step 2), the 95% porosity nickel foam substrate was replaced with a 60-mesh nickel mesh, while all other steps remained unchanged. The resulting electrode still possesses a complete biomimetic leaf vein air-guiding network and gradient pore size structure.
[0058] The biomimetic self-breathing hydrogen evolution electrode prepared according to the above steps is used for the hydrogen evolution reaction at the cathode of alkaline water electrolysis.
[0059] Example 5: Adjust the leaf vein air conduction structure parameters in step 5) of Example 1. The width of the main vein air conduction channel is adjusted from 800 μm to 1200 μm; the width of the lateral vein air conduction channel is adjusted from 150 μm to 250 μm; and the angle between the lateral vein and the main vein is adjusted from 45° to 30°. The remaining steps remain unchanged.
[0060] The biomimetic self-breathing hydrogen evolution electrode prepared by the above steps is used for the hydrogen evolution reaction at the cathode of alkaline water electrolysis.
[0061] Example 6: The biomimetic self-breathing hydrogen evolution electrode prepared in Example 1 was cut into rectangular samples with a length of 1.5 cm and a width of 1 cm. After being fixed with electrode clamps, it was used as the working electrode for hydrogen evolution performance testing. A three-electrode system was used for the test: the working electrode was the biomimetic self-breathing hydrogen evolution electrode; the counter electrode was a platinum mesh; the reference electrode was a mercuric oxide electrode; the electrolyte was a 1 mol / L KOH solution; and the effective testing area of the working electrode was 1 cm². 2 Hydrogen evolution performance was tested using linear sweep voltammetry (LSV) at a scan rate of 5 mV / s. A galvanostatic method was used at 1000 mA·cm⁻¹. -2 Stability tests were conducted under the specified conditions.
[0062] Electrochemical data were measured using linear voltammetry and electrochemical impedance spectroscopy. The linear voltammetry scan rate was 5 mV / s, the electrochemical impedance spectroscopy test potential was 1.53 V (vs. RHE), the electrochemical amplitude was 10 mV, and the frequency range was 10 Hz. 6 ~10 -1 Hz. For example... Figure 5As shown, the hydrogen evolution performance of the electrode gradually improves with the introduction of Ni-Mo / MoO2 heterostructure, gradient pore size gas-conducting structure, and surface regulation during the preparation process. The overpotential of NiMoO4@NF at 1000 mA / cm² is 565 mV, which decreases to 323 mV after reduction to form the Ni-Mo / MoO2 heterostructure, and further decreases to 256 mV after constructing the gradient pore size structure. The final catalyst has an overpotential of only 192 mV, significantly better than the 253 mV of commercial Pt / C. Simultaneously, EIS results show that the final catalyst has a lower charge transfer impedance, indicating more favorable interfacial electron transport; the hydrogen evolution performance of the electrode gradually improves with the introduction of Ni-Mo / MoO2 heterostructure, gradient pore size gas-conducting structure, and surface regulation during the preparation process. dl The values were 87, 40, 28, and 15 mF / cm, respectively. 2 This indicates that the electrochemical response changes significantly at each structural stage. Overall, the synergistic effect of the Ni–Mo / MoO2 heterostructure, the gradient pore size gas-conducting structure, and subsequent surface modulation is beneficial for improving the hydrogen evolution performance of the electrode at high current densities.
[0063] like Figure 4 As shown in the SEM images, NiMoO4@NF is uniformly loaded on the surface of the nickel foam skeleton, forming a relatively continuous catalytic layer; (b) after H2 / Ar reduction, a granular and rough Ni–Mo / MoO2 structure is formed on the surface, further enriching the surface active structure; (c) after introducing and removing polystyrene microsphere templates of different particle sizes, a porous structure with channels of different sizes is formed on the electrode surface, showing obvious gradient pore size characteristics; (d) after further surface treatment, the catalytic layer forms a more loose and interconnected network structure, presenting a multi-level structure combining a catalytic active layer, a gradient pore size gas guiding layer, and a biomimetic gas guiding network, providing a structural basis for reactant transport and rapid bubble desorption.
[0064] like Figure 2 and Figure 3 As shown, XRD results indicate that the precursor obtained after the hydrothermal reaction mainly exhibits the characteristic diffraction peaks of NiMoO4, indicating that the nickel and molybdenum components formed a NiMoO4 precursor structure on the surface of the nickel foam substrate. After reduction treatment at 450 °C under a 5% H2 / 95% Ar atmosphere, the characteristic diffraction peaks of NiMoO4 significantly weakened or disappeared, while diffraction peaks belonging to the Ni-Mo alloy and MoO2 appeared, indicating that the precursor underwent a significant phase transformation during the reduction process. Some Mo species were reduced and formed a Ni-Mo alloy with Ni, while some Mo species were retained as low-valence MoO2, thus forming a Ni-Mo alloy / MoO2 heterostructure. This phase structure evolution provides a material basis for the subsequent construction of a hierarchical catalytic electrode.
[0065] Therefore, the method for preparing hydrogen evolution electrode based on pulse current-induced in-situ reconstruction provided by the present invention is simple in process, has controllable parameters, good repeatability, and is easy to combine with existing water electrolysis electrode preparation processes, and has good prospects for industrial application.
[0066] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered illustrative and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the scope of the invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0067] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can be appropriately combined to form other embodiments that can be understood by those skilled in the art. The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.
Claims
1. A method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction, characterized in that, include: Select a conductive substrate and pretreat it; An initial hydrogen evolution catalytic layer was constructed on the surface of the treated conductive substrate to obtain an initial hydrogen evolution electrode. The obtained initial hydrogen evolution electrode was placed in an alkaline electrolyte as the working electrode to build a three-electrode or two-electrode electrochemical system. Based on the constructed three-electrode or two-electrode electrochemical system, a programmable pulsed current is applied to the initial hydrogen evolution electrode for in-situ reconstruction. By controlling the peak current density, pulse frequency, duty cycle, pulse width, pulse waveform and reconstruction time, the catalyst layer undergoes controllable in-situ reconstruction, forming a defect-rich and highly active reconstruction interface on the electrode surface. After in-situ reconstruction is completed, the pulsed current treatment is stopped, the electrode is removed, the residual electrolyte is removed, and it is dried to obtain a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction.
2. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The conductive substrate is one or more of the following: nickel foam, nickel mesh, titanium mesh, stainless steel mesh, copper mesh, carbon cloth, carbon paper, or conductive foam.
3. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The selected conductive substrate is pretreated, including degreasing, oxide removal and surface cleaning. The pretreatment includes: first, ultrasonically cleaning the conductive substrate sequentially with acetone, anhydrous ethanol, and deionized water to remove surface oil and impurities, with ultrasonic cleaning times ranging from 5 to 30 minutes; then, acid washing with one of hydrochloric acid, sulfuric acid, or nitric acid to remove the oxide layer on the surface of the conductive substrate, with an acid washing time ranging from 10 seconds to 10 minutes; after acid washing, thoroughly rinsing with deionized water until neutral, and then drying.
4. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The initial hydrogen evolution catalyst layer is one or more of the following: nickel-based alloy, nickel-molybdenum alloy, nickel-iron alloy, nickel-cobalt alloy, metal phosphide, sulfide, nitride, carbide, high-entropy alloy or composite material; the thickness of the catalyst layer is 0.1 to 100 μm.
5. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The alkaline electrolyte is a 0.1–10 mol / L potassium hydroxide solution or sodium hydroxide solution; the electrolyte temperature is 20–90℃.
6. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The peak current density of the pulse current is 50–5000 mA / cm². 2 The pulse frequency is 0.01–1000 Hz, the duty cycle is 5%–95%, the single pulse width is 0.1 ms–10 s, and the reconstruction time is 1 min–24 h.
7. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The pulse waveform is one or a combination of square waves, stepped waves, triangular waves, sine waves, or exponential waves.
8. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The pulse current parameters adopt a constant mode or a program control mode. In the program control mode, one or more parameters among the peak current density, frequency and duty cycle can be continuously or in stages adjusted with the reconstruction time to achieve in-situ reconstruction at different stages.
9. The method for preparing a hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction according to claim 1, characterized in that, The drying method is natural drying, forced air drying or vacuum drying, with a drying temperature of 25-80 ℃ and a drying time of 0.5-12 h.
10. A hydrogen evolution electrode based on pulsed current-induced in-situ reconstruction, characterized in that, It is prepared by any one of the preparation methods according to claims 1 to 9.