A honeycomb Ni3ZnC suitable for high current density alkaline hydrogen evolution 0.7 / CrN / CC electrocatalytic materials and their preparation methods

The Ni3ZnC0.7/CrN/CC composite electrocatalyst was prepared by hydrothermal-electrodeposition method, which solved the problem of unstable catalytic activity of existing electrocatalysts under high current density. It achieved high efficiency of hydrogen evolution electrocatalysis performance and structural stability in alkaline solution, reduced cost, and is suitable for industrial application.

CN123108629APending Publication Date: 2026-11-17SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611411082.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing electrocatalysts exhibit unstable catalytic activity and insufficient conductivity at high current densities, while noble metal-based catalysts are costly and difficult to meet the needs of large-scale applications.

Method used

A Ni3ZnC0.7/CrN/CC composite electrocatalyst was prepared by hydrothermal-electrodeposition. By growing Ni3ZnC0.7 and CrN in situ on a carbon substrate to form a honeycomb heterostructure, charge transport was promoted and more active sites were exposed. Combined with the regulation of band structure and interfacial interaction, surface agglomeration was suppressed.

Benefits of technology

It exhibits excellent electrocatalytic hydrogen evolution performance under high current density, has high structural stability, is suitable for acid and alkaline solutions, has low cost, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108629A_ABST
    Figure CN123108629A_ABST
Patent Text Reader

Abstract

A honeycomb Ni3ZnC suitable for high current density alkaline hydrogen evolution 0.7 This paper describes a Ni3ZnC / CrN / CC electrocatalytic material and its preparation method, belonging to the field of water electrolysis for hydrogen production. The material is mainly synthesized in situ on a carbon substrate (CC) using a hydrothermal-electrodeposition method. 0.7 / CrN / CC. The specific preparation process is as follows: First, the pretreated CC substrate is vertically immersed in a precursor solution containing nickel, zinc, chromium sources, and urea, and a hydrothermal reaction is carried out in a high-pressure reactor lined with polytetrafluoroethylene. Then, using dicyandiamide as the electrolyte, electrodeposition is performed on the formed backbone structure. Finally, it is calcined under an argon atmosphere to obtain Ni3ZnC. 0.7 / CrN / CC composite material. The electrocatalytic material prepared by this method has a unique honeycomb-like heterostructure and exhibits excellent electrocatalytic hydrogen evolution activity and stability at high current densities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalytic material preparation technology, specifically relating to a honeycomb Ni3ZnC substrate grown on a carbon (CC) surface suitable for high current density. 0.7 / CrN / CC materials, prepared via a hydrothermal-electrodeposition method, are applied in the field of alkaline water electrolysis for hydrogen production. The materials prepared using this method possess a unique honeycomb heterostructure and exhibit excellent electrocatalytic hydrogen evolution activity and stability at high current densities. Background Technology

[0002] Energy is a crucial material foundation for human societal development and a core driving force for the progress of human civilization and high-quality economic development. With rapid global economic development and a continuously expanding population, energy demand is soaring, and practical issues such as energy security, environmental protection, and sustainable development are becoming increasingly prominent. Coupled with the continued consumption and depletion of fossil fuels, global energy development is currently facing the dual challenges of surging demand and the demands of sustainable development. Hydrogen energy, as a clean energy source, is considered a key medium for achieving energy transition due to its safety, high energy density, zero carbon emissions, and multi-source production characteristics. Water splitting for hydrogen production, with its environmentally friendly and economically feasible advantages, has become a research focus in green hydrogen production technology. Research on electrocatalysts for the hydrogen evolution reaction is currently one of the hot topics in the fields of energy conversion and environmental remediation.

[0003] Electrocatalysts, as the core materials for the hydrogen evolution reaction, directly affect the efficiency and cost of hydrogen production. While noble metal-based catalysts such as platinum, iridium, and ruthenium exhibit excellent catalytic activity and stability, their scarcity and high price make them unsuitable for large-scale applications. Therefore, further development of low-cost and efficient non-noble metal-based electrocatalysts (NPMs) for water electrolysis to produce hydrogen is a central research topic. Significant progress has been made in this area, resulting in the development of the following electrode material systems: transition metal compound systems, such as carbides, nitrides, oxides, sulfides, and phosphides; single-atom and alloy systems, such as bi / multi-metal alloys and intermetallic compounds; non-metallic and composite support systems; and other special systems such as MOF / COF-derived catalysts. However, two major challenges remain: first, the conductivity of catalytic materials is generally poor, leading to unstable catalytic activity; second, although developed catalytic material systems such as phosphides, carbides, and transition metal sulfides have made breakthroughs in constructing active sites, they still face two major technical bottlenecks: insufficient conductivity and limited electrochemical stability.

[0004] Transition metal carbide systems, due to the small radius of carbon atoms, can embed themselves in the interstitial spaces of metal lattices to form unique interstitial structures. This allows them to simultaneously possess the high strength of covalent bonds, the conductivity of metallic bonds, and the polar adsorption properties of ionic bonds, exhibiting superior performance in multiple fields. Among these, bimetallic carbides, by introducing two metal elements and utilizing the electronic regulation and synergistic effects between different metal atoms, further optimize the mechanical properties, electronic structure, and catalytic activity of the materials, overcoming the limitations of single-metal carbides in terms of structural and performance regulation. Compared to single-metal carbides, bimetallic carbides offer superior mechanical properties, more constructable active sites, and greater tunability of electronic structure, even mimicking the electronic configuration of noble metals. They combine the conductivity of metallic materials with the stability of non-metallic materials, exhibiting superior catalytic activity at a lower cost, providing a new solution to overcome the aforementioned challenges.

[0005] The two-dimensional ternary hydroxide material involved in this invention has a huge specific surface area and more diverse surface defects. The two work together to provide a large number of active centers for electrocatalytic reactions. Under the stable structural support of CC, the three metal ions, combined with the supporting effect of interlayer anions, endow the material with good thermal and chemical stability. In high-temperature calcination or catalytic reactions, it can effectively inhibit the migration and aggregation of metal atoms, thereby ensuring the existence of active sites.

[0006] Ni3ZnC 0.7 As a typical bimetallic carbide, it provides a highly conductive metallic framework, with carbon as the framework center. Its strong covalent nature significantly improves the stability of the catalyst. However, its ion / charge transport rate is relatively slow, and its surface is easily oxidized, potentially dissolving during long-term reactions, leading to a decrease in catalytic performance. Chromium nitride, with the chemical formula CrN, is a black or light gray powder with a cubic crystal system and a crystal structure similar to platinum. Due to its advantages such as good adhesion, chemical stability, low price, high conductivity, tunable electronic structure, and low cost, it has become a popular candidate to replace noble metal-based electrocatalysts, showing broad application prospects in energy conversion and environmental remediation. Combining these two elements and growing them in situ on a carbon substrate, by introducing CrN and Ni3ZnC... 0.7 This forms a unique honeycomb-like heterogeneous structure. Furthermore, the interaction between the two inhibits surface aggregation and promotes rapid charge transport, exposing more active sites while maintaining structural integrity. In addition, CrN exhibits high oxidation temperature and good resistance to acid and alkali corrosion, ensuring long-term stability in acid and alkaline solutions. Summary of the Invention

[0007] This invention uses hydrothermal-electrodeposition as the main preparation method, combined with auxiliary methods such as grinding, stirring, and ultrasonication, to prepare a Ni3ZnC with high catalytic performance. 0.7The / CrN / CC electrocatalyst has the advantages of unique morphology, controllable structure, multiple active sites, tight phase interface contact, and high charge transport efficiency, exhibiting excellent electrocatalytic hydrogen evolution performance under high current density and alkaline solution. Furthermore, the synthesis process of this invention is extremely simple, low-cost, and suitable for industrial production.

[0008] To achieve the above objectives, the present invention employs the following technical solution: A Ni3ZnC 0.7 The preparation method of / CrN / CC composite electrocatalytic material includes the following steps: Step 1: Cut the carbon fiber cloth to 1×2 cm. 2 The carbon cloth was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 20 minutes in sequence. Then, it was immersed in concentrated nitric acid and treated at 60 ℃ for 1-2 hours. It was then rinsed repeatedly with ethanol and deionized water until neutral and vacuum dried at 60 ℃ for later use. Step 2: Dissolve nickel chloride hexahydrate (NiCl2·6H2O), zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and chromium nitrate nonahydrate (Cr(NO3)3·9H2O) in deionized water in a molar ratio of 1:1:(0.5~1). Then add ammonia (NH3·H2O) and polyvinyl alcohol and mix thoroughly to obtain the precursor solution. Step 3: Transfer the precursor solution obtained in Step 2 to a high-pressure reactor lined with polytetrafluoroethylene, vertically immerse the CC substrate obtained in Step 1 into the solution, and carry out a hydrothermal reaction at 160 °C for 10 h. Step 4: Weigh 0.75 g of dicyandiamide to prepare an electrodeposition solution, and deposit the ternary hydroxide obtained in Step 2 onto the CC substrate; Step 5: Place the sample obtained in Step 4 into a porcelain boat, and then place the porcelain boat into a high-temperature tube furnace for sintering under an argon atmosphere. Set the reaction temperature to around 800 °C and the reaction time to 2 hours to obtain the desired Ni3ZnC. 0.7 / CrN / CC composite electrocatalyst.

[0009] The present invention also has the following technical features: Preferably, the pretreatment method described in step one, which involves alternating ultrasonic cleaning with deionized water and ethanol for 20 minutes, can remove as many impurities as possible from the surface of the CC substrate.

[0010] Preferably, the precursor solution described in step two is stirred uniformly on a constant temperature magnetic stirrer for 6 to 12 hours to ensure as uniform mixing of the precursor solution as possible.

[0011] Preferably, the hydrothermal reaction described in step three can ensure that the nanosheets grow uniformly on the CC substrate surface as much as possible, expose as many active sites as possible, and ensure their hydrogen evolution activity under high current density.

[0012] Preferably, in the preparation of the electrolyte in step four, dicyandiamide should be ground for 40-60 minutes first, and then deionized water should be used as the solvent and boric acid should be used as the pH buffer to prepare the electrolyte.

[0013] The carbon substrate described in this invention includes, but is not limited to, materials such as carbon cloth, carbon-carbon composites, and carbon foam. This invention also protects a Ni3ZnC substrate prepared using the method described above. 0.7 Application of / CrN / CC composite electrocatalyst as an alkaline hydrogen evolution material in electrocatalytic water electrolysis.

[0014] Compared with the prior art, the present invention has the following technical effects: This invention synthesizes Ni3ZnC via a hydrothermal-electrodeposition method. 0.7 The / CrN / CC composite electrocatalyst has a simple synthesis process, low error, and convenient operation.

[0015] The precursor preparation process of this invention is rigorous, ensuring uniform dispersion of the phase.

[0016] This invention synthesizes Ni3ZnC by in-situ growth of ternary hydroxides on CC. 0.7 The / CrN / CC composite electrocatalyst ensures the uniformity of the interfacial structure, reduces the interfacial transfer resistance, and accelerates the reaction rate.

[0017] This invention regulates Ni3ZnC by introducing CrN. 0.7 The band structure optimizes the adsorption energy of intermediates, reducing the energy barrier of hydrogen evolution reaction in water electrolysis while forming a heterojunction surface. This interaction inhibits surface aggregation and promotes rapid charge transport. While ensuring structural integrity, it exposes more active sites, thus ensuring long-term stability.

[0018] This invention regulates the active sites, interface structure, and electronic structure of the product by adjusting the precursor ratio, pressure, atmosphere, reaction temperature, and reaction time, thereby reducing the overpotential of the water splitting reaction, improving the reaction kinetics, and ultimately optimizing the electrocatalytic hydrogen evolution performance of the product.

[0019] The Ni3ZnC prepared by this invention 0.7 The / CrN / CC composite electrocatalyst has a wide pH range and maintains good stability in both acidic and alkaline solutions.

[0020] The Ni3ZnC prepared by this invention 0.7 / CrN / CC composite electrocatalysts have abundant and inexpensive raw material reserves, making them suitable for industrial-scale mass production. Attached Figure Description

[0021] Figure 1 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 XRD pattern of / CrN / CC electrocatalyst; Figure 2 This is a SEM image of the ternary hydroxide prepared by hydrothermal treatment under the conditions of Example 1 of this invention; Figure 3 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 SEM image of the / CrN / CC electrocatalyst; Figure 4 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 Linear polarization curve of / CrN / CC electrocatalyst in 1 M KOH solution; Figure 5 The Ni3ZnC prepared under the conditions of Example 1 of this invention 0.7 Chronoamperometry curve of / CrN / CC electrocatalyst in 1 M KOH solution; Figure 6 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 TEM image of / CrN / CC electrocatalyst; Figure 7 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 TEM image of / CrN / CC electrocatalyst after HER. Detailed Implementation

[0022] The specific content of the present invention will be further explained in detail below with reference to the embodiments.

[0023] The reagents, methods, and equipment used in this invention are conventional reagents, methods, and equipment in this technical field. Test methods in the following examples that do not specify specific experimental conditions are generally performed under conventional experimental conditions. Unless otherwise stated, the reagents and raw materials used in this invention are commercially available.

[0024] In the following embodiments, the CC substrate was cleaned by placing the substrate in a beaker and then ultrasonically cleaning it alternately with deionized water and ethanol for 20 minutes each. Example

[0025] Step 1: Cut the carbon fiber cloth to 1×2 cm. 2The carbon cloth was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 20 minutes in sequence. Then, it was immersed in concentrated nitric acid and treated at 60°C for 2 hours. It was then rinsed repeatedly with ethanol and deionized water until neutral and vacuum dried at 60°C for later use. Step 2: Dissolve 0.46 g of nickel chloride hexahydrate (NiCl2·6H2O), 0.35 g of zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and 0.18 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O) in deionized water in a molar ratio of 1:1:(0.5~1), then add polyvinyl alcohol and mix thoroughly to obtain the precursor solution; Step 3: Transfer the precursor solution obtained in Step 2 to a high-pressure reactor lined with polytetrafluoroethylene, vertically immerse the CC substrate obtained in Step 1 into the solution, and carry out a hydrothermal reaction at 120 °C for 10 h. Step 4: Weigh 0.75 g of melamine to prepare an electrodeposition solution, and deposit the ternary hydroxide obtained in Step 2 onto the CC substrate; Step 5: Place the sample obtained in Step 4 into a porcelain boat, and then place the porcelain boat into a high-temperature tube furnace for sintering under an argon atmosphere. Set the reaction temperature to 800 ℃ and the reaction time to 2 hours to obtain the desired Ni3ZnC. 0.7 / CrN / CC composite electrocatalyst.

[0026] Figure 1 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 The XRD pattern of the Ni3ZnC / CrN / CC electrocatalyst shows that the Ni3ZnC prepared in this invention... 0.7 The diffraction peaks of / CrN correspond well to the standard PDF cards of the two pure phases, and their peak positions are consistent. The strongest peak is also sharp, indicating that the sample has good crystallinity.

[0027] Figure 2 This is a SEM image of the ternary hydroxide obtained by hydrothermal treatment under the conditions of Example 1 of this invention. In the SEM image at 50 μm, we can see Ni3ZnC. 0.7 / CrN grows uniformly on the CC surface, and there is a phenomenon of local connection on the surface, which may indicate the existence of heterogeneous structure, but the surface is relatively rough and pores have not yet formed.

[0028] Figure 3 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 The SEM image of the / CrN / CC electrocatalyst shows a honeycomb morphology on the sample surface at 5 μm. The honeycomb structure has a large number of regular and interconnected pores, which can provide more adsorption sites and reaction sites. The honeycomb structure also has good stability and ensures good performance under high current density.

[0029] Figure 4 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 The linear polarization curve of the / CrN / CC electrocatalyst in 1 M KOH solution shows that the hydrogen evolution performance of the sample can reach 235 mV (η) at a current density of 100. 100 =235 mV).

[0030] Figure 5 The Ni3ZnC prepared under the conditions of Example 1 of this invention 0.7 The chronoamperometry curve of the / CrN / CC electrocatalyst in 1 M KOH solution shows the current-time (it) test curve of the catalyst under alkaline conditions for 2 h, and the current density of the sample hardly changes.

[0031] Figure 6 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 TEM images of the / CrN / CC electrocatalyst reveal a heterogeneous surface structure, indicating that the composite sample, through structural modulation, forms a heterogeneous interface, providing more interactions and improving the kinetics of the electrode reaction. The 0.24 nm lattice spacing corresponds to the CrN(200) crystal plane, and the 0.221 nm lattice spacing corresponds to the Ni3ZnC plane. 0.7 The (111) crystal plane.

[0032] Figure 7 The Ni3ZnC prepared under the conditions of Example 1 according to the present invention 0.7 TEM images of the / CrN / CC electrocatalyst after HER. From the images, we can see that a lattice spacing of 0.24 nm corresponds to the CrN(200) crystal plane, and a lattice spacing of 0.235 nm corresponds to Ni3ZnC. 0.7 The (111) crystal plane. After a series of tests, Ni3ZnC 0.7 The phase structure and heterostructure of the / CrN / CC electrocatalyst remained unchanged, and the sample basically retained its initial morphology and valence state, highlighting the Ni3ZnC 0.7 Structural stability and durability of / CrN / CC catalysts. Example

[0033] Step 1: Cut the carbon fiber cloth to 1×2 cm. 2 The carbon cloth was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 20 minutes in sequence. Then, it was immersed in concentrated nitric acid and treated at 60°C for 2 hours. It was then rinsed repeatedly with ethanol and deionized water until neutral and vacuum dried at 60°C for later use. Step 2: Dissolve 0.41 g of nickel chloride hexahydrate (NiCl2·6H2O), 0.38 g of zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and 0.17 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O) in deionized water in a molar ratio of 1:1:(0.5~1). Then add ammonia (NH3·H2O) and polyvinyl alcohol and mix thoroughly to obtain the precursor solution. Step 3: Transfer the precursor solution obtained in Step 2 to a high-pressure reactor lined with polytetrafluoroethylene, vertically immerse the CC substrate obtained in Step 1 into the solution, and carry out a hydrothermal reaction at 120 °C for 8 h. Step 4: Weigh 0.96 g of dicyandiamide to prepare an electrodeposition solution, and deposit the ternary hydroxide obtained in Step 2 onto the CC substrate; Step 5: Place the sample obtained in Step 4 into a porcelain boat, and then place the porcelain boat into a high-temperature tube furnace for sintering under an argon atmosphere. Set the reaction temperature to around 900 °C and the reaction time to 2 hours to obtain the desired Ni3ZnC. 0.7 / CrN / CC composite electrocatalyst. Example

[0034] Step 1: Cut the carbon fiber cloth to 1×2 cm. 2 The carbon cloth was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 20 minutes in sequence. Then, it was immersed in concentrated nitric acid and treated at 70°C for 2 hours. It was then rinsed repeatedly with ethanol and deionized water until neutral and vacuum dried at 60°C for later use. Step 2: Dissolve 0.56 g of nickel chloride hexahydrate (NiCl2·6H2O), 0.51 g of zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and 0.22 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O) in deionized water in a molar ratio of 1:1:(0.5~1). Then add ammonia (NH3·H2O) and polyvinyl alcohol and mix thoroughly to obtain the precursor solution. Step 3: Transfer the precursor solution obtained in Step 2 to a high-pressure reactor lined with polytetrafluoroethylene, vertically immerse the CC substrate obtained in Step 1 into the solution, and carry out a hydrothermal reaction at 160 °C for 10 h. Step 4: Weigh 1.126 g of dicyandiamide to prepare an electrodeposition solution, and deposit the ternary hydroxide obtained in Step 2 onto the CC substrate; Step 5: Place the sample obtained in Step 4 into a porcelain boat, and then place the porcelain boat into a high-temperature tube furnace for sintering under an argon atmosphere. Set the reaction temperature to 700 °C and the reaction time to 3 hours to obtain the desired Ni3ZnC. 0.7 / CrN / CC composite electrocatalyst. Example

[0035] Step 1: Cut the carbon fiber cloth to 1×2 cm. 2 The carbon cloth was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 30 minutes in sequence. Then, it was immersed in concentrated nitric acid and treated at 80°C for 2 hours. It was then rinsed repeatedly with ethanol and deionized water until neutral and vacuum dried at 60°C for later use. Step 2: Dissolve 0.66 g of nickel chloride hexahydrate (NiCl2·6H2O), 0.63 g of zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and 0.42 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O) in deionized water in a molar ratio of 1:1:(0.5~1). Then add ammonia (NH3·H2O) and polyvinyl alcohol and mix thoroughly to obtain the precursor solution. Step 3: Transfer the precursor solution obtained in Step 2 to a high-pressure reactor lined with polytetrafluoroethylene, vertically immerse the CC substrate obtained in Step 1 into the solution, and carry out a hydrothermal reaction at 180 °C for 8 h. Step 4: Weigh 1.25 g of dicyandiamide to prepare an electrodeposition solution, and deposit the ternary hydroxide obtained in Step 2 onto the CC substrate; Step 5: Place the sample obtained in Step 4 into a porcelain boat, and then place the porcelain boat into a high-temperature tube furnace for sintering under an argon atmosphere. Set the reaction temperature to 1000 °C and the reaction time to 2 hours to obtain the desired Ni3ZnC. 0.7 / CrN / CC composite electrocatalyst. Example

[0036] Step 1: Cut the carbon fiber cloth to 1×2 cm. 2 The carbon cloth was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 40 minutes in sequence. Then, it was immersed in concentrated nitric acid and treated at 60°C for 2 hours. It was then rinsed repeatedly with ethanol and deionized water until neutral and vacuum dried at 60°C for later use. Step 2: Dissolve 0.31 g of nickel chloride hexahydrate (NiCl2·6H2O), 0.28 g of zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and 0.07 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O) in deionized water in a molar ratio of 1:1:(0.5~1). Then add ammonia (NH3·H2O) and polyvinyl alcohol and mix thoroughly to obtain the precursor solution. Step 3: Transfer the precursor solution obtained in Step 2 to a high-pressure reactor lined with polytetrafluoroethylene, vertically immerse the CC substrate obtained in Step 1 into the solution, and carry out a hydrothermal reaction at 100 °C for 12 h. Step 4: Weigh 1.5 g of dicyandiamide to prepare an electrodeposition solution, and deposit the ternary hydroxide obtained in Step 2 onto the CC substrate; Step 5: Place the sample obtained in Step 4 into a porcelain boat, and then place the porcelain boat into a high-temperature tube furnace for sintering under an argon atmosphere. Set the reaction temperature to 850 °C and the reaction time to 2 hours to obtain the desired Ni3ZnC. 0.7 / CrN / CC composite electrocatalyst.

Claims

1. A Ni3ZnC 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... Includes the following steps: Step 1: Cut the carbon substrate to 1×2 cm. 2 The carbon substrate is ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 15-30 minutes in sequence. Then, the carbon substrate is immersed in concentrated nitric acid and treated at 60-80°C for 1-2 hours. It is then rinsed repeatedly with ethanol and deionized water until neutral and vacuum dried at 60°C for later use. Step 2: Dissolve nickel chloride hexahydrate (NiCl2·6H2O), zinc acetate dihydrate (Zn(CH3COO)2·2H2O), and chromium nitrate nonahydrate (Cr(NO3)3·9H2O) in deionized water in a molar ratio of 1:1:(0.5~1). Then add ammonia (NH3·H2O) and polyvinyl alcohol and mix thoroughly to obtain the precursor solution. Step 3: Transfer the precursor solution obtained in Step 2 to a high-pressure reactor lined with polytetrafluoroethylene, vertically immerse the CC substrate obtained in Step 1 into the solution, and carry out a hydrothermal reaction at 90~180 ℃ for 6~12 h. Step 4: Weigh 0.75~1.5 g of dicyandiamide to prepare an electrodeposition solution, and deposit the ternary hydroxide obtained in Step 2 onto the CC substrate; Step 5: Place the sample obtained in Step 4 into a porcelain boat, put the porcelain boat into a high-temperature tube furnace, and sinter it under an argon atmosphere. Set the reaction temperature between 700 and 1000 ℃ and the reaction time between 1 and 4 hours.

2. The Ni3ZnC according to claim 1 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... The carbon substrate mentioned in step one includes, but is not limited to, materials such as carbon cloth, carbon-carbon composites, and carbon foam.

3. The Ni3ZnC according to claim 1 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... The precursor solution described in step two is stirred uniformly on a constant-temperature magnetic stirrer for 6-12 hours to ensure as uniform mixing of the precursor solution as possible.

4. The Ni3ZnC according to claim 1 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... The hydrothermal reaction described in step three can ensure that the nanosheets grow uniformly on the CC substrate surface as much as possible, expose as many active sites as possible, and ensure their hydrogen evolution activity under high current density.

5. The Ni3ZnC according to claim 1 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... In step four, the electrolyte should be prepared by first grinding dicyandiamide for 40-60 minutes, then using deionized water as the solvent and boric acid as the pH buffer.

6. The Ni3ZnC according to claim 1 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... The electrodeposition reaction described in step four can ensure that the ternary hydroxide is deposited uniformly on the CC substrate surface, resulting in a uniform interface, reduced interfacial transfer resistance, and increased reaction rate.

7. The Ni3ZnC according to claim 1 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... The composite material surface forms a unique honeycomb morphology, which reduces the transfer resistance between interfaces, accelerates the reaction rate, and ensures long-term stability due to its structural integrity.

8. The Ni3ZnC according to claim 1 0.7 The method for preparing / CrN / CC composite electrocatalytic materials is characterized by... The prepared composite material forms a heterojunction surface, which can interact to inhibit surface aggregation, promote rapid charge transport, and expose more active sites, making it suitable for hydrogen production by water electrolysis under high current density.