High-purity copper electrolytic refining additives, high-purity copper electrolytes and their applications

By using a silver ion masking agent composed of a complex heterocyclic compound and a nonionic surfactant, the problem of removing silver impurities in copper electrolytic refining in existing technologies has been solved, achieving stable preparation and purity improvement of high-purity copper, which is suitable for large-scale production.

CN123108657APending Publication Date: 2026-11-17GEM CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611336867.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing copper electrolytic refining processes are unable to effectively remove silver impurities, making it difficult for high-purity copper products to meet the 6N grade standard.

Method used

A silver ion masking agent composed of a complex heterocyclic compound and a nonionic surfactant is used to chelate silver ions in the electrolyte and form an ultrathin adsorption film on the cathode surface, thus constructing a dual defense line of liquid-phase complexation and interfacial barrier to remove silver impurities quickly and efficiently.

Benefits of technology

It significantly reduces the silver content in electrolytic copper materials, improves product purity to 6N grade, and has a short process flow, making it suitable for large-scale continuous production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application provides a high-purity copper electrolytic refining additive, a high-purity copper electrolyte, and their applications. The high-purity copper electrolytic refining additive includes a silver ion masking agent, which comprises a complex heterocyclic compound and a nonionic surfactant. The high-purity copper electrolyte provided by this application, using the aforementioned high-purity copper electrolytic refining additive, has the advantage of stably preparing 6N-grade high-purity copper. Compared to conventional processes, the silver content in the resulting copper material is significantly reduced, thus significantly improving the production quality of electrolytic copper materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of electrolytic copper technology, specifically relating to a high-purity copper electrolytic refining additive, a high-purity copper electrolyte, and their applications. Background Technology

[0002] High-purity copper (HPCu) refers to copper materials with a purity of 99.999% (5N) or higher. With the rapid development of modern technology, the demand for high-purity copper in the electronics, semiconductor, aerospace, and nuclear industries is increasing daily. For example, in the electronics industry, high-purity copper is used to manufacture high-performance chips and integrated circuit lead frames; in the semiconductor field, high-purity copper is a key material for manufacturing high-precision semiconductor devices; and in the aerospace and nuclear industries, high-purity copper is used to manufacture critical components, as its high purity and excellent electrical and thermal conductivity meet the requirements of use in extreme environments.

[0003] Copper electrolytic refining is a crucial step in the production of high-purity copper. Its purpose is to remove impurities from crude copper through electrolysis, yielding high-purity electrolytic copper. However, the aforementioned copper electrolytic refining process also has certain limitations. For example, due to the influence of various factors such as electrolyte composition, current density, and temperature, when producing high-purity copper (e.g., HPCu-6N and above), some difficult-to-remove impurities (such as silver) may remain, making it difficult to achieve higher purity standards in the product.

[0004] To address the aforementioned issues, the industry currently widely uses bone glue, thiourea, hydrochloric acid, or gelatin as additives in the copper electrolytic refining process. However, the current copper electrolytic refining additive system still falls short of meeting the quality requirements of 6N grade high-purity copper.

[0005] Therefore, there is an urgent need to develop an additive that can quickly and efficiently remove silver impurities and produce 6N grade high-purity copper, thereby overcoming the limitations of existing processes in terms of purification efficiency and product quality. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the purpose of this application is to provide a high-purity copper electrolytic refining additive and a high-purity copper electrolyte containing the additive, which has the advantage of stably preparing 6N grade high-purity copper. Compared with conventional processes, the silver content in the copper material obtained can be significantly reduced, thus significantly improving the production quality of electrolytic copper materials.

[0007] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a high-purity copper electrolytic refining additive, which includes a silver ion masking agent, wherein the silver ion masking agent comprises a complex heterocyclic compound and a nonionic surfactant.

[0008] This application employs a compounded silver ion masking agent for electrolytic refining of high-purity copper. Based on the synergistic effect between the compound heterocyclic compound and the nonionic surfactant, high-purity copper cathodes with extremely low silver impurity content are stably obtained.

[0009] Specifically, complex heterocyclic compounds can exist stably in a strong acid environment, thus chelating most of the silver ions in the electrolyte; while nonionic surfactants can form an ultrathin adsorption film on the cathode surface, further blocking residual free silver ions from reaching the cathode surface, thereby constructing a dual defense of liquid-phase complexation + interface barrier, while avoiding the introduction of too many organic impurities into the system, resulting in high chemical purity and stability of the high-purity copper prepared by electrolysis.

[0010] In some embodiments, the complex heterocyclic compounds include mercaptotetrazole compounds and triazole compounds.

[0011] By selecting a combination of specific types of heterocyclic compounds, the binding interaction with silver ions is enhanced, facilitating the rapid and efficient removal of silver impurities. Specifically, the nitrogen atoms and thiol groups in the nitrogen-containing groups can form stable coordination bonds with silver ions, thereby better controlling the content of silver impurities in the system.

[0012] In some embodiments, the mercaptotetrazole compound includes 5-mercaptotetrazole, wherein the 5-mercaptotetrazole is selected from at least one of 1-phenyl-5-mercaptotetrazole or 5-methylmercapto-1H-tetrazole.

[0013] In some embodiments, the triazole compounds include benzotriazole.

[0014] In some embodiments, the mass ratio of the mercaptotetrazole compound to the triazole compound is 2.8:1 to 3.2:1, for example, it can be 2.8:1, 2.85:1, 2.9:1, 2.95:1, 3:1, 3.05:1, 3.1:1, 3.15:1 or 3.2:1, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0015] By adjusting the mass ratio of mercaptotetrazole compounds to triazole compounds to a narrower range, a strong acid-stable complex system is formed, which facilitates the chelation of the vast majority of silver ions in the electrolyte.

[0016] In some embodiments, the nonionic surfactant includes C12 to C18 fatty alcohol polyoxyethylene ethers, such as C12, C13, C14, C15, C16, C17, or C18 fatty alcohol polyoxyethylene ethers, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0017] By selecting fatty alcohol polyoxyethylene ethers with short carbon chains, excessive organic impurities can be introduced, thus avoiding exceeding the organic carbon limit.

[0018] In some embodiments, the nonionic surfactant accounts for 1.5% to 4% of the total mass of the complex heterocyclic compound, for example, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0019] By adjusting the mass ratio of nonionic surfactants to a reasonable range, it is beneficial to form an ultrathin adsorption film on the cathode surface, which can block residual free silver ions from reaching the cathode surface and better play the role of an interface barrier.

[0020] Secondly, this application provides a high-purity copper electrolyte, which includes the high-purity copper electrolytic refining additives according to the first aspect.

[0021] In some embodiments, the high-purity copper electrolyte further includes copper ions and sulfuric acid.

[0022] In some embodiments, the copper ion concentration in the high-purity copper electrolyte is 30 g / L to 60 g / L, for example, it can be 30 g / L, 35 g / L, 40 g / L, 45 g / L, 50 g / L, 55 g / L or 60 g / L, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0023] In some embodiments, the sulfuric acid concentration in the high-purity copper electrolyte is 120 g / L to 200 g / L, for example, it can be 120 g / L, 140 g / L, 160 g / L, 180 g / L or 200 g / L, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0024] Thirdly, this application provides a method for preparing high-purity copper using the high-purity copper electrolyte according to the second aspect, the method comprising the following steps: Using copper as the anode and an inert material as the cathode, the anode and cathode are immersed in the high-purity copper electrolyte according to the second aspect for electrolytic refining to obtain high-purity copper.

[0025] In some embodiments, the current density of the electrolytic refining is 150 A / m. 2 ~250A / m 2 For example, it can be 150A / m 2 180A / m 2 200A / m 2 220A / m 2 Or 250A / m 2 The term "etc." is not limited to the listed values; it also applies to other unlisted values ​​within the range.

[0026] In some embodiments, the electrolytic refining temperature is 20°C to 60°C, for example, it can be 20°C, 30°C, 40°C, 50°C or 60°C, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0027] Fourthly, this application provides a high-purity copper, which is prepared by the method for preparing high-purity copper according to the third aspect, wherein the purity of copper in the high-purity copper is not less than 99.9999%.

[0028] This application utilizes an electrolyte containing the high-purity copper electrolytic refining additives described in the first aspect to directly prepare 6N high-purity copper in a sulfuric acid system in one step. The process is simple, and the copper crystals are uniform, making it suitable for large-scale continuous production.

[0029] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0030] Compared with the prior art, this application has the following advantages: This application provides a high-purity copper electrolytic refining additive, which uses a compounded silver ion masking agent for electrolytic refining of high-purity copper. Based on the synergistic effect between the compound heterocyclic compound and the nonionic surfactant, high-purity copper cathode with extremely low silver impurity content is stably obtained.

[0031] Specifically, complex heterocyclic compounds can exist stably in a strong acid environment, thus chelating most of the silver ions in the electrolyte; while nonionic surfactants can form an ultrathin adsorption film on the cathode surface, further blocking residual free silver ions from reaching the cathode surface, thereby constructing a dual defense of liquid-phase complexation + interface barrier, while avoiding the introduction of too many organic impurities into the system, resulting in high chemical purity and stability of the high-purity copper prepared by electrolysis.

[0032] This application utilizes an electrolyte containing the aforementioned high-purity copper electrolytic refining additive to directly prepare 6N high-purity copper in a single step via electrolysis in a sulfuric acid system. The process is simple, and the copper crystals are uniform, making it suitable for large-scale continuous production. Detailed Implementation

[0033] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0034] Example 1 This embodiment provides a high-purity copper electrolytic refining additive, which includes a silver ion masking agent, comprising a complex heterocyclic compound and a nonionic surfactant.

[0035] The complex heterocyclic compounds include 1-phenyl-5-mercaptotetrazole and benzotriazole in a mass ratio of 3:1, and the nonionic surfactant is a C15 fatty alcohol polyoxyethylene ether (CAS No.: 56049-80-0). Based on the total mass of the complex heterocyclic compounds being 100%, the nonionic surfactant accounts for 2.5% of the total mass.

[0036] This embodiment also provides a method for preparing high-purity copper using an electrolyte containing the above-mentioned high-purity copper electrolytic refining additives, which includes the following steps: Using a 4N copper plate as the anode and a titanium plate as the cathode, the anode and cathode are immersed in an electrolyte containing the aforementioned high-purity copper electrolytic refining additives for electrolytic refining. The current density for electrolytic refining is 200 A / m. 2 The electrolytic refining temperature is 40℃ to obtain the high-purity copper. The electrolyte also includes copper sulfate and sulfuric acid, with the concentration of copper sulfate being 45 g / L and the concentration of sulfuric acid being 150 g / L.

[0037] Example 2 This embodiment provides a high-purity copper electrolytic refining additive, which includes a silver ion masking agent, comprising a complex heterocyclic compound and a nonionic surfactant.

[0038] The complex heterocyclic compounds include 1-phenyl-5-mercaptotetrazole and benzotriazole in a mass ratio of 2.8:1, and the nonionic surfactant is a C12 fatty alcohol polyoxyethylene ether (laurate ether-2). Based on the total mass of the complex heterocyclic compounds being 100%, the nonionic surfactant accounts for 1.5% of the total mass.

[0039] This embodiment also provides a method for preparing high-purity copper using an electrolyte containing the above-mentioned high-purity copper electrolytic refining additives, which includes the following steps: Using a 4N copper plate as the anode and a titanium plate as the cathode, the anode and cathode are immersed in an electrolyte containing the aforementioned high-purity copper electrolytic refining additives for electrolytic refining. The current density for electrolytic refining is 150 A / m. 2 The electrolytic refining temperature is 20℃ to obtain the high-purity copper. The electrolyte also includes copper sulfate and sulfuric acid, with the concentration of copper sulfate being 30 g / L and the concentration of sulfuric acid being 120 g / L.

[0040] Example 3 This embodiment provides a high-purity copper electrolytic refining additive, which includes a silver ion masking agent, comprising a complex heterocyclic compound and a nonionic surfactant.

[0041] The complex heterocyclic compounds include 1-phenyl-5-mercaptotetrazole and benzotriazole in a mass ratio of 3.2:1, and the nonionic surfactant is a C18 fatty alcohol polyoxyethylene ether (stearyl alcohol polyether-2). Based on the total mass of the complex heterocyclic compounds being 100%, the nonionic surfactant accounts for 4% of the total mass.

[0042] This embodiment also provides a method for preparing high-purity copper using an electrolyte containing the above-mentioned high-purity copper electrolytic refining additives, which includes the following steps: Using a 4N copper plate as the anode and a titanium plate as the cathode, the anode and cathode are immersed in an electrolyte containing the aforementioned high-purity copper electrolytic refining additives for electrolytic refining. The current density for electrolytic refining is 250 A / m. 2 The electrolytic refining temperature is 60℃ to obtain the high-purity copper. The electrolyte also includes copper sulfate and sulfuric acid, with the concentration of copper sulfate being 60 g / L and the concentration of sulfuric acid being 200 g / L.

[0043] Example 4 The difference between this embodiment and Example 1 is that the mass ratio of 1-phenyl-5-mercaptotetrazole to benzotriazole is 2:1, while all other aspects are the same as in Example 1.

[0044] Example 5 The difference between this embodiment and Example 1 is that the mass ratio of 1-phenyl-5-mercaptotetrazole to benzotriazole is 4:1, while all other aspects are the same as in Example 1.

[0045] Example 6 The difference between this embodiment and Example 1 is that 1-phenyl-5-mercaptotetrazole is replaced with an equal mass of 5-amino-1H-tetrazole, while all other aspects are the same as in Example 1.

[0046] Example 7 The difference between this embodiment and Embodiment 1 is that, with the total mass of the complex heterocyclic compound being 100%, the mass percentage of the nonionic surfactant is 1%, while everything else is the same as in Embodiment 1.

[0047] Example 8 The difference between this embodiment and Embodiment 1 is that, with the total mass of the complex heterocyclic compound being 100%, the mass percentage of the nonionic surfactant is 8%, while all other aspects are the same as in Embodiment 1.

[0048] Example 9 The difference between this embodiment and Example 1 is that the C15 fatty alcohol polyoxyethylene ether (CAS No.: 56049-80-0) is replaced with an equal mass of behenyl alcohol polyether-5 (CAS No.: 136207-49-3), while all other aspects are the same as in Example 1.

[0049] Comparative Example 1 The difference between this comparative example and Example 1 is that the silver ion masking agent only includes complex heterocyclic compounds, which include 1-phenyl-5-mercaptotetrazole and benzotriazole in a mass ratio of 3:1, the same as in Example 1.

[0050] Comparative Example 2 The difference between this comparative example and Example 1 is that the silver ion masking agent only includes complex heterocyclic compounds, the complex heterocyclic compounds only include benzotriazole, and the total mass of benzotriazole is the same as the total mass of 1-phenyl-5-mercaptotetrazole and benzotriazole in Example 1. Everything else is the same as in Example 1.

[0051] Comparative Example 3 The difference between this comparative example and Example 1 is that the silver ion masking agent only includes a nonionic surfactant, which is a C15 fatty alcohol polyoxyethylene ether (CAS No.: 56049-80-0). Everything else is the same as in Example 1.

[0052] Test conditions The purity and impurity content of the electrolytic copper obtained in the above examples and comparative examples were determined, and the test results are shown in Table 1.

[0053] Table 1 As can be seen from Table 1, compared with Comparative Examples 1 to 3, Examples 1 to 3 of this application use a compounded silver ion masking agent for electrolytic refining of high-purity copper. Based on the synergistic effect between the compound heterocyclic compound and the nonionic surfactant, high-purity copper cathodes with extremely low silver impurity content are stably obtained.

[0054] Comparing Examples 1 and 4-5, it can be seen that by adjusting the mass ratio of 1-phenyl-5-mercaptotetrazole and benzotriazole to a narrower range, a strong acid-stable complex complex system can be formed, which facilitates the chelation of most silver ions in the electrolyte.

[0055] Comparing Examples 1 and 6, it can be seen that replacing it with the existing 5-amino-1H-tetrazole cannot achieve all the technical effects of the technical solution of this application.

[0056] Comparing Examples 1 and 7-9, it can be seen that by adjusting the type and mass ratio of nonionic surfactants to a reasonable range, it is beneficial to form an ultrathin adsorption film on the cathode surface, which can block residual free silver ions from reaching the cathode surface and better play the role of an interface barrier.

[0057] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A high-purity copper electrolytic refining additive, characterized in that, The high-purity copper electrolytic refining additive includes a silver ion masking agent, which comprises a complex heterocyclic compound and a nonionic surfactant.

2. The high-purity copper electrolytic refining additive according to claim 1, characterized in that, The complex heterocyclic compounds include mercaptotetrazole compounds and triazole compounds; The mercaptotetrazole compounds include 5-mercaptotetrazole, wherein the 5-mercaptotetrazole is selected from at least one of 1-phenyl-5-mercaptotetrazole or 5-methylmercapto-1H-tetrazole; The triazole compounds include benzotriazole.

3. The high-purity copper electrolytic refining additive according to claim 2, characterized in that, The mass ratio of the mercaptotetrazole compound to the triazole compound is 2.8:1 to 3.2:

1.

4. The high-purity copper electrolytic refining additive according to any one of claims 1 to 3, characterized in that, The nonionic surfactant includes C12-C18 fatty alcohol polyoxyethylene ethers.

5. The high-purity copper electrolytic refining additive according to any one of claims 1 to 4, characterized in that, Based on the total mass of the complex heterocyclic compound being 100%, the mass percentage of the nonionic surfactant is 1.5% to 4%.

6. A high-purity copper electrolyte, characterized in that, The high-purity copper electrolyte includes high-purity copper electrolytic refining additives according to any one of claims 1 to 5.

7. The high-purity copper electrolyte according to claim 6, characterized in that, The high-purity copper electrolyte also includes copper ions and sulfuric acid; And / or, the copper ion concentration in the high-purity copper electrolyte is 30 g / L to 60 g / L; And / or, the sulfuric acid concentration in the high-purity copper electrolyte is 120 g / L to 200 g / L.

8. A method for preparing high-purity copper using the high-purity copper electrolyte according to claim 6 or 7, characterized in that, The method includes the following steps: Using copper as the anode and an inert material as the cathode, the anode and the cathode are immersed in the high-purity copper electrolyte according to claim 6 or 7 for electrolytic refining to obtain high-purity copper.

9. The method according to claim 8, characterized in that, The current density for the electrolytic refining process is 150 A / m. 2 ~250A / m 2 ; And / or, the temperature of the electrolytic refining is 20℃~60℃.

10. A high-purity copper, characterized in that, The high-purity copper is prepared by the method for preparing high-purity copper according to claim 8 or 9, wherein the purity of copper in the high-purity copper is not less than 99.9999%.