A controllable preparation method for electrodeposition of micro / nano aluminum particles
By using composite interface control additives in ionic liquid electrodeposition systems, precise control of aluminum particle size has been achieved, solving the problems of uncontrollable particle size and agglomeration in existing technologies. This method is applicable to fields such as energy storage electrodes, catalytic materials, and thermally conductive fillers.
Patent Information
- Application Number
- CN202611335550.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing AlCl3/EMImCl ionic liquid electrodeposition system, the aluminum particle size is uncontrollable and prone to agglomeration, making it difficult to achieve precise preparation with a narrow particle size distribution of 10 nm-600 nm.
Aluminum metal particles with uniform particle size of 10 nm to 600 nm and no obvious agglomeration were prepared by using composite interface-controlled additives, including highly active polar molecules such as N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, and N-bromosuccinimide as core additives, supplemented by polyethylene glycol 200, succinimide and other auxiliary additives, and by precisely controlling the additive ratio and electrodeposition process parameters.
It achieves precise control of aluminum particle size, resulting in high product purity and uniform particle size distribution. It solves the problems of uncontrollable particle size and severe agglomeration in traditional processes, and is suitable for various applications such as energy storage electrodes, catalytic materials, and thermally conductive fillers.
Smart Images

Figure CN123108667A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of controllable preparation of metal micro / nano particles and ionic liquid electrodeposition technology. It relates to a controllable preparation method for electrodeposition of micro / nano aluminum particles, specifically a method for preparing controllable-size aluminum particles by ionic liquid electrodeposition based on composite interface-modifying additives. In particular, it relates to an anhydrous aluminum chloride / 1-ethyl-3-methylimidazolium (AlCl3 / EMImCl) ionic liquid system containing interface-modifying additives and a method for electrodeposition preparation of aluminum metal particles with controllable particle sizes of 10 nm-600 nm. Background Technology
[0002] Aluminum metal micro- and nano-particles possess excellent properties such as high specific surface area, high conductivity, high reactivity, and low density, making them highly valuable for applications in energy storage electrodes, catalytic materials, thermally conductive fillers, metal powder metallurgy, and anti-corrosion coatings. Compared to traditional preparation processes such as mechanical ball milling, vapor deposition, and liquid-phase reduction, electrodeposition technology offers significant advantages, including simpler processes, lower costs, higher product purity, greater controllability of particle size, and scalability, making it the preferred technical route for the preparation of micro- and nano-aluminum particles.
[0003] Ionic liquids, as green non-aqueous solvents, possess advantages such as a wide electrochemical window, low volatility, good thermal stability, and excellent conductivity. They can effectively avoid the problems of hydrogen evolution, severe oxidation, and uneven deposition in aluminum deposition systems, making them ideal electrolyte systems for aluminum electrodeposition. In existing AlCl3 / EMImCl ionic liquid electrodeposition systems, the pure ionic liquid interface has poor stability, the aluminum deposition nucleation rate is uncontrollable, and problems such as particle agglomeration, large particle size range, and irregular morphology are prone to occur, making it impossible to accurately prepare aluminum particles with a narrow particle size distribution of 10 nm-600 nm.
[0004] Currently, the industry mostly uses conventional surfactants and corrosion inhibitors as electrolyte additives, which can only improve deposition uniformity in a simple way and cannot achieve precise control of aluminum particle size. To address the shortcomings of existing technologies, such as low particle size control precision and poor product consistency, there is an urgent need to develop a specific interface control additive system that can achieve stable preparation of narrow-distribution, controllable-size aluminum particles through precise ratio control. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for preparing controllable-size aluminum particles by ionic liquid electrodeposition based on composite interface-regulating additives. The core solution addresses the technical problems of uncontrollable particle size and severe agglomeration in existing aluminum particle preparation methods. This invention uses one or a combination of two of the highly active polar molecules N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide, and N-chlorophthalimide as core interface-regulating additives. A composite interface-regulating additive system is constructed by compounding various auxiliary modifying additives. By precisely controlling the additive ratio and electrodeposition process parameters, aluminum metal particles with a uniform particle size distribution and no obvious agglomeration, ranging from 10 nm to 600 nm, are stably prepared.
[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: <First Aspect> This invention relates to a method for preparing controllable-size aluminum particles by ionic liquid electrodeposition based on composite interface-controlled additives, the method comprising the following steps: S1. Under an anhydrous and oxygen-free inert environment, anhydrous AlCl3 and EMImCl are mixed at a molar ratio of 1.2~1.8:1 and stirred at a constant temperature until the system is clear and transparent to prepare a (homogeneous and stable) ionic liquid-based electrolyte. S2. Add an amount of composite interface control additive to the ionic liquid substrate electrolyte; the composite interface control additive consists of a core additive and an auxiliary modifying additive, wherein the core additive is at least one of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide and N-chlorophthalimide, accounting for more than 60% of the total mass of the composite interface control additive; S3. Stir the electrolyte obtained in step S2 at room temperature to obtain a modified ionic liquid electrolyte. S4. Use a three-electrode system for constant potential electrodeposition or constant current electrodeposition; after deposition, remove the working electrode, rinse, vacuum dry, and peel off the deposits on the electrode surface to obtain the controllable particle size aluminum metal particles.
[0007] The core additive in the composite interface regulation additive of this invention is a highly active polar interface-participating molecule that can be specifically adsorbed on the electrode deposition interface to regulate the nucleation rate of aluminum atoms, inhibit particle agglomeration, and achieve precise control of aluminum particle size. The auxiliary additives are mainly used to optimize electrolyte wettability, stabilize the interfacial electric field, and weaken impurity interference.
[0008] In one embodiment of the present invention, in step S1, the isothermal stirring temperature is 25~35 ℃, and the time is 2~4 h. In some embodiments, the molar ratio of anhydrous AlCl3 to EMImCl is 1.5:1, the stirring temperature is 30 ℃, and the stirring time is 3 h, resulting in optimal electrolyte stability.
[0009] In one embodiment of the present invention, the core additive is one or a combination of two of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide, and N-chlorophthalimide, accounting for more than 70% of the total mass of the composite additive; preferably 70%-80%. The core additive accounting for 70%~80% of the total mass of the composite interface regulating additive represents the optimal ratio range, which can precisely control the aluminum particle size to remain stable at 80 nm-100 nm, with a particle size distribution deviation ≤15%.
[0010] In one embodiment of the present invention, the auxiliary modifying additive is selected from two or more of polyethylene glycol 200, succinimide, methyl carbamate, phthalic anhydride, and dodecyl betaine, accounting for less than 40% of the total mass of the composite interface regulating additive; preferably, the proportion is 10%-40%, more preferably 20%-30%. In some embodiments, the auxiliary modifying additive is a compound of polyethylene glycol 200 and phthalic anhydride, with a mass ratio of 2:1. This compound system can maximize the improvement of electrolyte stability.
[0011] In one embodiment of the present invention, the total mass of the composite interface-regulating additive is 0.1% to 5% of the mass of the ionic liquid-based electrolyte; preferably 1.0% to 2.5%. Within this ratio range, the interface regulation effect of the core additive is optimal, without the problems of excessive additive precipitation or insufficient activity.
[0012] In one embodiment of the present invention, in step S3, the composite interface regulating additive is added (in batches) to the ionic liquid substrate electrolyte, and stirred at room temperature for 1-3 hours under inert gas protection to obtain the modified ionic liquid electrodeposition electrolyte. Ultrasonic dispersion can be continued for 10-30 minutes to ensure complete dissolution of the additive and homogeneity of the system.
[0013] As one embodiment of the present invention, in step S4, the working electrode in the three-electrode system is an aluminum sheet or a glassy carbon electrode, the counter electrode is a high-purity aluminum sheet, and the reference electrode is a high-purity aluminum wire.
[0014] In one embodiment of the present invention, in step S4, the constant potential electrodeposition process parameters are: deposition temperature 25~60℃, deposition voltage... 1.0 V~ 3 V, deposition time 5~30 min. In some implementation examples, the deposition temperature is controlled at 40 ℃ and the deposition voltage is... At 1.8 V and a deposition time of 15 min, the prepared aluminum particles had regular morphology, no agglomeration, and uniform particle size.
[0015] As one embodiment of the present invention, in step S4, the constant current electrodeposition process parameters are: deposition temperature 25~60℃, deposition current 10-100 mA cm⁻¹. 2 Deposition time: 5-30 min.
[0016] As one embodiment of the present invention, the particle size of the controllable particle size aluminum metal particles is 10 nm-600 nm.
[0017] <Second aspect> The present invention also relates to controllable particle size aluminum metal particles prepared by the aforementioned method.
[0018] As one embodiment of the present invention, the aluminum metal particles have a particle size of 10 nm-600 nm, a particle size distribution deviation of ≤15%, and no obvious agglomeration.
[0019] <Third aspect> This invention also relates to an ionic liquid composite electrolyte for electrodeposition to prepare aluminum particles with controllable particle size, comprising an AlCl3 / EMImCl ionic liquid base electrolyte and a composite interface-regulating additive; wherein the molar ratio of anhydrous AlCl3 to EMImCl in the base electrolyte is 1.2~1.8:1; the composite interface-regulating additive is composed of a core additive and an auxiliary modifying additive, wherein the core additive is at least one of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide and N-chlorophthalimide, accounting for more than 60% of the total mass of the composite interface-regulating additive.
[0020] As one embodiment of the present invention, the total mass of the composite interface regulating additive is 0.1% to 5% of the mass of the ionic liquid-based electrolyte; preferably 1.0% to 2.5%.
[0021] As one embodiment of the present invention, the core additive is one or a combination of two of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide and N-chlorophthalimide, accounting for more than 70% of the total mass of the composite additive; preferably 70%-80%.
[0022] As one embodiment of the present invention, the auxiliary modifying additive is selected from two or more of polyethylene glycol 200, succinimide, methyl carbamate, phthalic anhydride, and dodecyl betaine, accounting for less than 40% of the total mass of the composite interface regulating additive; preferably, the proportion is 10%-40%, more preferably 20%-30%.
[0023] This invention innovatively selects one or a combination of two of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide, and N-chlorophthalimide as core interface regulating additives. These molecules have strong polarity and high interfacial adsorption activity. Theoretical simulations show that the adsorption energy of the core interface additive on the aluminum (200) crystal plane is significantly higher than that on Al2Cl7. With AlCl4 ion( Figure 2 Therefore, it can preferentially accumulate at the electrode-ionic liquid deposition interface, precisely controlling the reduction nucleation rate of aluminum ions: on the one hand, it can reduce the critical nucleation radius of aluminum atoms, promoting the generation of a large number of fine crystal nuclei; on the other hand, it can adsorb onto the surface of newly formed aluminum particles, inhibiting particle agglomeration and growth. By controlling its addition ratio, the growth size of aluminum particles can be precisely controlled, achieving high-precision particle size control within a wide range of 10 nm to 600 nm. The various auxiliary additives compounded in this invention play an auxiliary role in optimizing the physical properties of the electrolyte and stabilizing the deposition environment. Under the synergistic effect of the overall system, the industry pain points of uncontrollable particle size and severe agglomeration of aluminum particles in traditional ionic liquid electrodeposition are completely solved.
[0024] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention is the first to use one or a combination of two of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide and N-chlorophthalimide as core interface-participating additives in ionic liquid aluminum electrodeposition systems. By precisely controlling the addition ratio, precise particle size control of aluminum particles from 10 nm to 600 nm is achieved. The product has uniform particle size, no agglomeration and high purity, which solves the core problem of uncontrollable particle size in traditional processes.
[0025] (2) The process of this invention is simple, the conditions are mild and the repeatability is good. The electrolyte has strong stability and can accurately control micro and nano aluminum particles in different particle size ranges. It is suitable for multiple applications such as energy storage, catalysis and heat conduction, and has extremely high industrialization value. Attached Figure Description
[0026] Other features, objects, and advantages of the present invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings: Figure 1 The electrochemical windows of Examples 1-3 and Comparative Example 1; Figure 2 N-chlorosuccinimide and Al2Cl7 AlCl4 Adsorption energy diagram of ions; Figure 3 This is a SEM image of the aluminum particles in Example 1 of the present invention; Figure 4 This is a SEM image of the aluminum particles in Example 2 of the present invention; Figure 5 This is a SEM image of the aluminum particles in Example 3 of the present invention; Figure 6 This is a SEM image of the aluminum particles in Comparative Example 1 of the present invention. Figure 7 This is a SEM image of the aluminum particles in Comparative Example 2 of the present invention. Figure 8 This is a SEM image of the aluminum particles in Comparative Example 3 of the present invention. Figure 9 This is a SEM image of the aluminum particles in Comparative Example 4 of the present invention. Figure 10 The XRD patterns are of Embodiments 1-3 and Comparative Example 1 of the present invention; Figure 11 The graph shows a comparison of the cycle performance of symmetrical batteries assembled using Examples 1-3 of the present invention and Comparative Example 1. Detailed Implementation
[0027] The present invention will be described in detail below with reference to embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make several adjustments and improvements without departing from the concept of the present invention. These all fall within the protection scope of the present invention.
[0028] Example 1 Step 1: Preparation of ionic liquid-based electrolyte: Under inert gas protection and an anhydrous and oxygen-free environment, anhydrous aluminum trichloride (AlCl3) and 1-ethyl-3-methylimidazolium chloride (EMImCl) were mixed at a molar ratio of 1.5:1 and stirred at 30 °C for 3 h to obtain a clear and transparent base electrolyte, which was then cooled to room temperature. Step 2: Prepare composite additives: The total mass of composite interface regulating additives is 2% of the mass of the base electrolyte, of which the core additive N-chlorosuccinimide accounts for 75%, and the auxiliary additives of polyethylene glycol 200 and phthalic anhydride account for 25% (mass ratio 2:1). Step 3: Add the composite interface regulating additive to the base electrolyte and stir at room temperature for 2 hours to obtain a homogeneous modified electrolyte. Step 4, Electrodeposition: A three-electrode system is used, with an aluminum sheet as the working electrode, a high-purity aluminum sheet as the counter electrode, and a high-purity aluminum wire as the reference electrode. The working electrode area is 10 cm². 2 The electrode spacing is 5 cm, the temperature is 40 ℃, and the open-circuit voltage is used as a reference. A constant potential deposition of 1.8V was performed for 15 min. After deposition, the working electrode was removed and rinsed sequentially with anhydrous ethanol and ultrapure water. After vacuum drying, the deposit on the electrode surface was ultrasonically removed (power 400 W, frequency 40 kHz, time 10 s) to obtain aluminum metal particles with controllable particle size. Figure 3 It can be seen that the obtained aluminum particles have a particle size concentrated in the range of 50 nm to 100 nm, with no agglomeration, uniform morphology, and a particle size distribution deviation of ≤10%. Figure 10 The XRD pattern of Example 1 shows that the aluminum deposited particles are of high purity and have no impurity diffraction peaks.
[0029] Example 2 The total mass of the composite interface control additive was 1.2% of the mass of the base electrolyte. The core additive, N-chloropropionamide, accounted for 70%, and the auxiliary additives were succinimide and dodecyl betaine (mass ratio 2:1). The remaining parameters were the same as in Example 1. The resulting aluminum particles had a particle size concentrated in the range of 100 nm to 200 nm. Figure 4 ). Figure 10 The XRD pattern of Example 2 shows that the aluminum deposited particles are of high purity and have no impurity diffraction peaks.
[0030] Example 3 The total mass of the composite interface control additive was 2.5% of the mass of the base electrolyte. The core additive, N-bromosuccinimide, accounted for 80%, and the auxiliary additives were anhydrous ethanol and phthalic anhydride (mass ratio 1:1). The remaining parameters were the same as in Example 1. The resulting aluminum particles had a particle size concentrated in the range of 200 nm to 300 nm. Figure 5 ). Figure 10 The XRD pattern of Example 1 shows that the aluminum deposited particles are of high purity and have no impurity diffraction peaks.
[0031] Example 4 The total mass of the composite interface control additive is 1% of the mass of the base electrolyte. The core additive, N-chlorophthalimide, accounts for 80%, and the auxiliary additive is anhydrous ethanol + phthalic anhydride (mass ratio 1:1). The remaining parameters are the same as in Example 1. The resulting aluminum particles have a particle size concentrated in the range of 400 nm to 500 nm.
[0032] Comparative Example 1 Without adding the core additives, and with the remaining process parameters the same as in Example 1, the deposited product exhibited severe agglomeration, with particle sizes ranging from 500 nm to 2 μm. Figure 6The inability to achieve controllable regulation proves that auxiliary additives lack core regulatory functions. Figure 10 The XRD pattern of Comparative Example 1 shows that the aluminum deposited particles are of high purity and have no impurity diffraction peaks. Figure 1 The electrochemical windows of Examples 1-3 and Comparative Example 1 are shown in the figure. It can be seen that the composite additive can significantly broaden the electrochemical window of ionic liquids and maximize the stability of electrolytes. Figure 11 The graph shows a comparison of the cycle performance of symmetrical batteries assembled using Examples 1-3 and Comparative Example 1 of the present invention. The test conditions were: high-purity aluminum sheets as electrodes, and a current density of 10 mA cm⁻¹. 2 The temperature was 25 °C. The results showed that the composite additive could significantly improve the cycle stability of the symmetric battery, with Example 1 being the optimal ratio.
[0033] Comparative Example 2 Replacing the core additive with N-methylacetamide, and keeping the other process parameters the same as in Example 2, resulted in severe agglomeration of the deposited product, with particle sizes ranging from 100 nm to 2 μm. Figure 7 The inability to achieve controllable regulation proves that N-methylacetamide additives have no regulatory function.
[0034] Comparative Example 3 Replacing the core additive with N,N-dimethylacetamide, and keeping the other process parameters the same as in Example 2, resulted in severe agglomeration of the deposited product, with particle sizes ranging from 50 nm to 3 μm. Figure 8 The inability to achieve controllable regulation proves that the N,N-dimethylacetamide additive has no regulatory function.
[0035] Comparative Example 4 The core additive was replaced with a fluorinated additive (fluoroethylene carbonate), and the remaining process parameters were the same as in Example 1. The deposited product had uneven particle size, with particle sizes ranging from 100 nm to 1 μm. Figure 9 The inability to achieve controllable regulation proves that fluorine-containing additives have no regulatory function.
[0036] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing controllable-size aluminum particles by ionic liquid electrodeposition based on composite interface-controlled additives, characterized in that, The method includes the following steps: S1. Under an anhydrous and oxygen-free inert environment, anhydrous AlCl3 and EMImCl are mixed at a molar ratio of 1.2~1.8:1 and stirred at a constant temperature until the system is clear and transparent to prepare an ionic liquid-based electrolyte. S2. Add a composite interface control additive to the ionic liquid substrate electrolyte; The composite interface regulating additive consists of a core additive and an auxiliary modifying additive. The core additive is at least one of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide and N-chlorophthalimide, accounting for more than 60% of the total mass of the composite interface regulating additive. S3. Stir the electrolyte obtained in step S2 at room temperature to obtain a modified ionic liquid electrolyte. S4. Use a three-electrode system for constant potential electrodeposition or constant current electrodeposition. After deposition is complete, the working electrode is removed, rinsed, vacuum dried, and the deposits on the electrode surface are peeled off to obtain the controllable particle size aluminum metal particles.
2. The preparation method according to claim 1, characterized in that, In step S1, the temperature of the constant-temperature stirring is 25~35 ℃, and the time is 2~4h.
3. The preparation method according to claim 1, characterized in that, The core additive is one or a combination of two of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide and N-chlorophthalimide, accounting for more than 70% of the total mass of the composite additive; preferably 70%-80%.
4. The preparation method according to claim 1, characterized in that, The auxiliary modifying additive is selected from two or more of polyethylene glycol 200, succinimide, methyl carbamate, phthalic anhydride, and dodecyl betaine, accounting for less than 40% of the total mass of the composite interface regulating additive; preferably, the proportion is 10%-40%, more preferably 20%-30%.
5. The preparation method according to claim 1, characterized in that, The total mass of the composite interface regulating additive is 0.1% to 5% of the mass of the ionic liquid-based electrolyte; preferably 1.0% to 2.5%.
6. The preparation method according to claim 1, characterized in that, In step S3, the composite interface control additive is added to the ionic liquid substrate electrolyte and stirred at room temperature for 1-3 h under inert gas protection. And / or, in step S4, the working electrode in the three-electrode system is an aluminum sheet or a glassy carbon electrode, the counter electrode is a high-purity aluminum sheet, and the reference electrode is a high-purity aluminum wire. And / or, in step S4, the constant potential electrodeposition process parameters are: deposition temperature 25~60 ℃, deposition voltage... 1.0 V~ 3V, deposition time 5~30min; constant current electrodeposition process parameters: deposition temperature 25~60 ℃, deposition current 10~100 mA cm⁻¹ 2 Deposition time: 5-30 min.
7. The preparation method according to claim 1, characterized in that, The controllable particle size aluminum metal particles have a particle size of 10 nm-600 nm.
8. A type of aluminum metal particles with controllable particle size prepared by the method described in any one of claims 1-7.
9. The controllable particle size aluminum metal particles according to claim 8, characterized in that, The aluminum metal particles have a particle size of 10nm-600nm, a particle size distribution deviation of ≤15%, and no obvious agglomeration.
10. An ionic liquid composite electrolyte for electrodeposition preparation of aluminum particles with controllable particle size, characterized in that, The mixture includes an AlCl3 / EMImCl ionic liquid substrate electrolyte and a composite interface control additive. The molar ratio of anhydrous AlCl3 to EMImCl in the substrate electrolyte is 1.2~1.8:
1. The composite interface control additive consists of a core additive and auxiliary modifying additives. The core additive is at least one of N-chloroacetamide, N-chloropropionamide, N-chlorosuccinimide, N-bromosuccinimide, and N-chlorophthalimide, accounting for more than 60% of the total mass of the composite interface control additive.