Bending-resistant lithium-ion battery copper foil, electrolyte additives used therein, and preparation method
By adding specific additives to the copper foil electrolyte, the nucleation and growth of copper grains are regulated to form a uniform microstructure, solving the problem that existing evaluation methods for the bending resistance of copper foil are not applicable. This achieves high tensile strength and excellent fatigue resistance, making it suitable for high-energy-density lithium-ion batteries.
Patent Information
- Application Number
- CN202611261689.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for evaluating the bending resistance of copper foil are not applicable to copper foil of 6μm and below, and cannot predict its fatigue fracture resistance potential during long-term cycling, affecting the cycle capacity retention and safety of the battery.
An electrolyte additive using a compound of collagen, hydroxyethyl cellulose, polyethylene glycol, and disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate as a wetting agent, sodium polydisulfide dipropane sulfonate as a promoter, and tetrahydrothiazolyl thione and its derivatives as grain refiners, controls the nucleation and growth of copper grains to form a uniform microstructure, thereby enhancing the fatigue fracture resistance potential of copper foil.
It significantly improves the fatigue fracture resistance potential of copper foil, extends battery life, and enhances safety performance, while maintaining high tensile strength and good ductility, making it suitable for the development of high energy density lithium-ion batteries.
Smart Images

Figure CN123108671A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrolytic copper foil technology, and more particularly to bend-resistant lithium-ion battery copper foil, electrolyte additives used therein, and preparation methods. Background Technology
[0002] In lithium-ion battery systems, copper foil, as the current collector for negative electrode active materials (such as graphite and silicon-carbon composites), plays a crucial role in collecting and conducting current and supporting the coating structure of the negative electrode active material. Its performance directly determines the battery's energy density, cycle life, and safety reliability. With the rapid development of new energy vehicles and large-scale energy storage industries, the requirements for energy density and cycle performance of lithium-ion batteries continue to increase. Silicon-carbon negative electrode materials, with their extremely high theoretical specific capacity, have become the core research and development direction for next-generation high-energy-density lithium-ion batteries; however, their volume expansion rate during charging and discharging can reach over 300%, which applies continuous and alternating cyclic stress to the current collector copper foil, easily causing fatigue damage, cracks, or even breakage of the copper foil. This ultimately leads to a sharp increase in battery internal resistance, rapid capacity decay, and even safety risks such as thermal runaway.
[0003] Previously, the copper foil industry focused on improving the tensile strength of copper foil, paying insufficient attention to its ability to resist crack initiation and propagation under cyclic stress—that is, its bending fatigue resistance. Copper foil with high tensile strength but insufficient toughness is more prone to brittle cracking under the volumetric alternating stress of silicon-carbon anodes. Therefore, developing electrolyte additive formulations that can specifically optimize the microstructure of copper foil and significantly improve its bending fatigue resistance while maintaining high conductivity is a key technological bottleneck to adapt to the development of high-energy-density batteries and support the large-scale application of silicon-carbon anodes. Currently, bending fatigue resistance is measured by the MIT test with standard rounded corners to determine the number of bends before fracture. However, this method is not suitable for testing the bending resistance of copper foils of 6μm and below because the copper foils of 6μm and below are too thin and brittle, resulting in high deviations in the MIT test data. Furthermore, the MIT test measures fatigue life and cannot predict fatigue resistance potential. The copper foil in the inner arc region of the battery is folded, making it more susceptible to fatigue fracture under repeated mechanical stress during long cycles, directly affecting the battery's cycle capacity retention and safety. To avoid this, internal testing needs to predict the copper foil's performance over tens of thousands of cycles. This is more valuable in engineering than simply measuring the initial UTS (tensile strength) or E1 (elongation).
[0004] For example, Chinese invention patent authorization announcement number CN115478305B discloses a method for preparing electrolytic copper foil for lithium-ion batteries with high bending resistance and its additives. The raw material components of the additives include bisbenzenesulfonylimide, fish glue, polypropylene glycol, dextrin, and sodium dimethylformamide propane sulfonate. By adding unique additives, the bending resistance of Cu can be inhibited. 2+Rapid deposition on the cathode roller results in more uniform electrolytic copper foil crystal nuclei and enables the formation of a dense and bright electrolytic copper foil on the cathode roller surface through a complexation reaction. Furthermore, the combined effect of composite additives improves the bending resistance of the copper foil. This patent uses the MIT standard rounded corner reciprocating bending resistance test to measure the number of bends before fracture; however, this method is not applicable to the fatigue fracture resistance potential of copper foils with a diameter of 6μm or less.
[0005] For example, Chinese invention patent publication number CN119332313A discloses a method and application for improving the high-temperature elongation of copper foil by controlling the molecular weight of additives. In the production process of electrolytic copper foil, the molecular weight control technology of additives is an important technical means. It can improve the microstructure and physical properties of copper foil, including elongation and bending resistance, by affecting the reduction process of copper ions in the electrolyte. This patent, like the one published by MIT, measures the number of bends before fracture using a standard rounded corner reciprocating bending test, and is not applicable to evaluating the fatigue fracture resistance potential of copper foil with a diameter of 6μm or less. Summary of the Invention
[0006] The problem this invention aims to solve is that existing copper foil bending resistance indicators rely on the MIT test, which focuses on evaluating fatigue life. This invention takes a different approach and proposes an indicator applicable to the degree of retention of load-bearing capacity after copper foil undergoes bending deformation at extremely small radii, indirectly indicating the material's fatigue fracture resistance potential. To this end, it provides bending-resistant lithium battery copper foil, electrolyte additives used in it, and preparation methods.
[0007] The technical solution of the present invention is: an electrolyte additive for bend-resistant lithium battery copper foil, comprising the following components: a wetting agent composed of collagen, hydroxyethyl cellulose, polyethylene glycol, and disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester; sodium polydisulfide dipropane sulfonate as an accelerator; and a grain refiner composed of one or more mixtures of tetrahydrothiazolyl thione and its derivatives. The total concentration range of the wetting agent, accelerator, and grain refiner is 2 mg / L to 80 mg / L, and the mass ratio of the wetting agent, accelerator, and grain refiner is (10~20): (20~40): (2~5).
[0008] A method for preparing bend-resistant lithium-ion battery copper foil includes the following steps: adding the electrolyte additive for bend-resistant lithium-ion battery copper foil as described above to a copper sulfate electrolyte, stirring evenly to obtain an electrolyte working solution; under constant current electrolysis conditions, electrolytic deposition is performed using a titanium cathode roller as the cathode to generate a copper deposition layer on the surface of the cathode roller, and after peeling, bend-resistant lithium-ion battery copper foil is obtained.
[0009] The copper sulfate electrolyte in the above scheme contains Cu 2+The concentration was 90 g / L~95 g / L, the H2SO4 concentration was 100 g / L~110 g / L, the copper sulfate electrolyte temperature was 50±2 ℃, and the basic chloride ion concentration was 30±2 ppm.
[0010] The constant current electrolysis current density described in the above scheme is 3000 A / m 2 ~4500 A / m 2 .
[0011] The bend-resistant lithium-ion battery copper foil is made by the above-mentioned method for preparing bend-resistant lithium-ion battery copper foil.
[0012] The bending-resistant lithium-ion battery copper foil described in the above scheme has a thickness of 6μm and an original tensile strength of 500 MPa~650 MPa.
[0013] The bending-resistant lithium-ion battery copper foil described in the above scheme exhibits a tensile strength attenuation rate of <20% after a 0°R angle bending test.
[0014] The beneficial effects of this invention are that the formulation, through the synergistic compounding of multiple functional additives, precisely controls the nucleation and growth behavior of copper grains during electrolytic deposition, resulting in a uniform microstructure of copper foil. This significantly enhances the fatigue fracture resistance potential of the copper foil, making it suitable for the cyclic stress conditions of high-volume expansion anode materials (such as silicon-carbon anodes), extending battery life and improving safety performance. The tensile strength decay rate is used as an auxiliary evaluation reference index for bending resistance, mainly for failure analysis and performance comparison verification of parallel samples. During continuous production, this additive system does not exhibit significant foam accumulation problems caused by polymeric wetting agents, and trace amounts of hydrolysis products can be adsorbed through the existing activated carbon adsorption process on the production line without interfering with the balance of the main additives. While improving bending and fatigue resistance, the copper foil prepared using this formula can still maintain high tensile strength and good ductility, and its comprehensive performance meets the application requirements of high-end lithium battery copper foil. The copper foil prepared by this formula is particularly suitable for matching high-capacity anode materials such as silicon-carbon, which can effectively buffer the volume change stress during the anode cycle, improve the cycle stability and safety of the battery, and has important application value for promoting the development of high-energy-density lithium-ion batteries. Attached Figure Description
[0015] Figure 1 EBSD grain distribution diagram of the smooth and matte surface of the copper foil prepared in Example 1; Figure 2 EBSD grain distribution diagram of the smooth and matte surface of the copper foil prepared in Example 2; Figure 3 EBSD grain distribution diagram of the smooth and matte surface of the copper foil prepared in Example 5; Figure 4 EBSD grain distribution diagram of the smoothed and textured surface of the copper foil prepared for Comparative Example 1; Figure 5 EBSD grain distribution diagram of the smoothed and textured surface of copper foil prepared for Comparative Example 2; Figure 6 The EBSD grain distribution diagram of the smoothed and textured surface of the copper foil prepared in Comparative Example 3; Figure 7 Statistical diagram of grain size of copper foil prepared in Example 1; Figure 8 This is a statistical diagram of the grain size of the copper foil prepared in Example 2; Figure 9 This is a statistical diagram of the grain size of the copper foil prepared in Example 5; Figure 10 Grain size statistics of copper foil prepared in Comparative Example 1; Figure 11 A statistical chart of grain size of copper foil prepared for Comparative Example 2; Figure 12 A statistical chart of the grain size of the copper foil prepared in Comparative Example 3; Figure 13 Example 3: SEM image of the rough surface of the prepared copper foil; Figure 14 SEM image of the rough surface of the copper foil prepared in Example 5; Figure 15 SEM image of the rough surface of the copper foil prepared for Comparative Example 3. Detailed Implementation
[0016] To facilitate understanding of the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings. The described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art are within the scope of protection of the present invention.
[0017] For simplicity, this paper only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, just as any upper limit can be combined with any other upper limit to form an undefined range. Furthermore, although not explicitly stated, every point or individual value between the endpoints of a range is included within that range. Therefore, each point or individual value can serve as its own lower or upper limit and be combined with any other point or individual value, or with other lower or upper limits, to form an undefined range.
[0018] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments.
[0019] This invention does not impose any special limitations on the source of the raw materials used; all raw materials are commercially available products conventional in this technical field. Unless otherwise specified, the solvent for all solutions in this application is pure water.
[0020] The concentration data of various additives in this invention were all measured using an electroplating analyzer (CVS Metrohm, Switzerland); the microstructure of the copper foil was characterized and photographed using a field emission scanning electron microscope (TESCAN MIRA).
[0021] Basic experimental conditions: The basic composition of the electrolyte used in all experiments of this invention is as follows: Cu 2+ The concentration is 90-95 g / L, the H2SO4 concentration is 100-110 g / L, the electrolyte temperature range is 50±2 °C, the chloride ion concentration is 30±2 ppm, and the current density is 3000-4500 A / m².
[0022] Experimental preparation process: The additives of this invention were added to the above electrolyte: a wetting agent (a compound of collagen, hydroxyethyl cellulose, polyethylene glycol, and disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate); an accelerator (sodium polydithiopropane sulfonate and chloride ions); and a grain refiner (one or more mixtures of tetrahydrothiazolyl thione and its derivatives). Under constant current power supply conditions, 6μm high tensile strength (500-650MPa) copper foil was electrolytically deposited on a titanium cathode roller.
[0023] Performance testing and characterization methods: This invention employs the 0°R angle bending test method commonly used in the lithium battery copper foil industry to evaluate the fatigue fracture resistance potential of copper foil. The specific test procedure is as follows: a copper foil sample measuring 15mm × 100mm is folded in half, rolled with a 2kg rubber roller, and then tested for tensile strength and elongation before and after bending using a universal testing machine. The tensile strength attenuation rate is used as an auxiliary evaluation reference index for fatigue fracture resistance potential, primarily for failure analysis and performance comparison verification of parallel samples.
[0024] In this test, all examples and comparative examples used the same basic electrolyte system and electrolysis process to prepare 6μm thick electrolytic copper foil.
[0025] The verification experimental schemes for different additive ratios are shown in Table 1 below.
[0026]
[0027] Note: To facilitate the viewing and analysis of the table data, the following additives are represented by codes, and the corresponding relationships are as follows: Collagen (A1), Hydroxyethyl cellulose (A2), Polyethylene glycol (A3), Disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester (A4), Sodium polydisulfide dipropane sulfonate (B1), Tetrahydrothiazolylthione (C1).
[0028] The electrolyte additive for the bend-resistant lithium-ion battery copper foil in Example 1 includes a compound of 10 ppm collagen, hydroxyethyl cellulose, polyethylene glycol, disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester, 30 ppm sodium polydisulfide dipropane sulfonate, 2 ppm tetrahydrothiazolyl thione, and a wetting agent, accelerator and grain refiner in a mass ratio of 5:15:1.
[0029] A method for preparing bend-resistant lithium-ion battery copper foil includes the following steps: adding the above-mentioned electrolyte additive for bend-resistant lithium-ion battery copper foil to a copper sulfate electrolyte, stirring evenly to obtain an electrolyte working solution; under constant current electrolysis conditions, electrolytic deposition is performed using a titanium cathode roller as the cathode to generate a copper deposition layer on the surface of the cathode roller, which is then peeled off to obtain the bend-resistant lithium-ion battery copper foil. The copper sulfate electrolyte contains Cu... 2+ The concentration of copper sulfate electrolyte was 90 g / L~95 g / L, the concentration of H2SO4 was 100 g / L~110 g / L, the temperature of the copper sulfate electrolyte was 48 ℃, and the basic chloride ion concentration was 28 ppm. The current density of constant current electrolysis was 3000 A / m. 2 .
[0030] Example 2: The difference from Example 1 is that the concentration of sodium polydithiopropane sulfonate is 20 ppm, and the mass ratio of wetting agent, accelerator, and grain refiner is 5:10:1. Cu in the copper sulfate electrolyte. 2+ The concentration of copper sulfate electrolyte was 95 g / L, the concentration of H₂SO₄ was 110 g / L, the temperature of the copper sulfate electrolyte was 52℃, and the basic chloride ion concentration was 32 ppm. The current density of constant current electrolysis was 4500 A / m. 2 .
[0031] Example 3: The difference from Example 1 is that it is compounded with 15 ppm of collagen, hydroxyethyl cellulose, polyethylene glycol, disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester, 4 ppm of tetrahydrothiazolyl thione, and the mass ratio of wetting agent, accelerator and grain refiner is 7.5:15:2.
[0032] Example 4: The difference from Example 1 is that it is compounded with 20 ppm of collagen, hydroxyethyl cellulose, polyethylene glycol, disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester, 20 ppm of sodium dithiodipropane sulfonate, 3 ppm of tetrahydrothiazolyl thione, and the mass ratio of wetting agent, accelerator and grain refiner is 10:10:1.5.
[0033] Example 5: The difference from Example 1 is that it is compounded with 20 ppm of collagen, hydroxyethyl cellulose, polyethylene glycol, disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester, 40 ppm of sodium dithiodipropane sulfonate, 3 ppm of tetrahydrothiazolyl thione, and the mass ratio of wetting agent, accelerator and grain refiner is 10:20:1.5.
[0034] Example 6: The difference from Example 1 is that it is compounded with 20 ppm of collagen, hydroxyethyl cellulose, polyethylene glycol, disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester, 40 ppm of sodium dithiodipropane sulfonate, 4 ppm of tetrahydrothiazolyl thione, and the mass ratio of wetting agent, accelerator and grain refiner is 5:10:1.
[0035] Example 7: The difference from Example 1 is that it is compounded with 20 ppm of collagen, hydroxyethyl cellulose, polyethylene glycol, disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester, 3 ppm of tetrahydrothiazolyl thione, and the mass ratio of wetting agent, accelerator and grain refiner is 6.7:10:1.
[0036] Comparative Example 1: The difference from Example 1 is that it is compounded with 25 ppm of collagen, hydroxyethyl cellulose, polyethylene glycol, disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester, 40 ppm of sodium dithiodipropane sulfonate, 6 ppm of tetrahydrothiazolyl thione, and the mass ratio of wetting agent, accelerator and grain refiner is 12.5:20:3.
[0037] Comparative Example 2: The difference from Example 1 is that the concentration of sodium polydisulfide dipropane sulfonate is 12 ppm, and the mass ratio of wetting agent, accelerator and grain refiner is 5:6:1.
[0038] Comparative Example 3: The difference from Example 1 is that the concentration of sodium polydisulfide dipropane sulfonate is 15 ppm, and the mass ratio of wetting agent, accelerator and grain refiner is 5:7.5:1.
[0039] The test results of the 0°R angle bending performance of each sample are shown in Table 2 below.
[0040]
[0041] Based on the test data in Table 2, the following conclusions can be drawn: The formulation of this invention can significantly improve the fatigue fracture resistance potential of copper foil. The wetting agent ensures the uniformity of the deposition interface and eliminates the inducing factors for abnormal local grain growth; the accelerator improves the surface smoothness of the deposited layer; and the grain refiner directly dominates the grain refinement process, improving tensile strength. Under the synergistic effect of these three agents, the grain size distribution of the copper foil is more uniform, effectively eliminating abnormal grains.
[0042] 1. The component ratio is a core parameter for controlling the performance of copper foil. Samples from Examples 1-7 prepared using the ratio range of this invention all showed a tensile strength attenuation rate of less than 20% after bending, achieving excellent bending and fatigue resistance while maintaining high tensile strength. For ultra-high strength copper foil applications, the sample in Example 6, after rigorous bending tests, still showed a tensile strength attenuation rate of 19.46%, verifying that this additive formulation can effectively balance material toughness and fatigue fracture resistance while maintaining ultra-high strength of the copper foil. In Comparative Example 1, the overall additive concentration was higher, resulting in a tensile strength attenuation rate of 49.31% after bending, significantly deteriorating the fatigue fracture resistance. This result indicates that grain refiners need to work synergistically with other components within a reasonable concentration range; excessive addition leads to a decrease in material toughness, which in turn weakens the fatigue fracture resistance of the copper foil.
[0043] 2. The synergistic effect of the compound additive system is indispensable. Comparative samples verified the synergistic necessity of wetting agents, accelerators, and grain refiners. The concentrations of wetting agents and grain refiners in Comparative Example 1 were higher than the limits specified in this invention, and its mechanical properties and fatigue fracture resistance potential were significantly inferior to those of Example 6. The accelerator ratios in Comparative Examples 2 and 3 were insufficient, resulting in a significant increase in the tensile strength attenuation rate after bending and a significant deterioration in fatigue fracture resistance potential, far inferior to the sample of the example with the optimal ratio of this invention. These results confirm that a reasonable ratio of additive components can effectively reduce surface defects and stress concentration sites in copper foil, which is key to improving the fatigue fracture resistance potential of copper foil.
[0044] The grain structure of the smooth and rough surfaces of the copper foil was characterized using electron backscatter diffraction (EBSD), and the results are as follows: Figures 1-12 As shown. Note: In this invention, the smooth surface of the copper foil refers to the surface that is in contact with the cathode roller during the copper foil preparation process; the rough surface refers to the surface that is away from the cathode roller during the copper foil preparation process.
[0045] The comparative samples exhibited uneven grain size distribution, with significant differences in grain size between the smooth and rough surfaces. In contrast, the samples from the embodiments of this invention showed a more uniform grain distribution, with moderate grain size and better microstructure consistency. This homogenized microstructure facilitates stress dispersion, which is the fundamental reason why the copper foil exhibits a higher toughness retention rate in bending tests.
[0046] The morphology of the rough surface of the copper foil was characterized using scanning electron microscopy (SEM), and the results are as follows: Figures 13-15 As shown. Note: Under the condition that other process conditions remain unchanged, the morphology of the smooth surface of the copper foil is mainly determined by the surface quality of the cathode roller, while the morphology of the rough surface of the copper foil is mainly controlled by the additive system.
[0047] In Examples 3 and 5, the ratio of wetting agent to accelerator was 1:2, resulting in a smoother surface texture of the copper foil prepared by both examples, while the surface texture of Comparative Example 3 was significantly rougher. Meanwhile, Example 5 used a higher amount of wetting agent, resulting in a better surface texture than Example 3.
[0048] This invention addresses the industry pain point of fatigue cracking of copper foil caused by volume expansion of silicon-carbon anodes in high-energy-density batteries. It constructs an electrolyte additive system composed of a specific compound wetting agent, accelerator, and grain refiner. By synergistically regulating the electrolytic deposition behavior of copper through multiple components, the grain size distribution can be effectively homogenized, forming a relatively uniform and dense equiaxed crystalline structure on the smooth and matte surface of the copper foil, thus fundamentally improving the fatigue crack resistance of the copper foil. Performance verification results show that the 6μm electrolytic copper foil prepared using this formulation can maintain a high tensile strength of 500MPa~650MPa while achieving a tensile strength reduction rate of less than 20% after bending at a 0°R angle, thus balancing high strength with excellent fatigue fracture resistance.
[0049] The bend-resistant copper foil prepared by this invention can effectively buffer the volumetric alternating stress during the cycling process of silicon-carbon anodes, delay current collector failure, and has significant application value in improving the cycle life and safety reliability of lithium-ion batteries. Furthermore, this additive formulation is highly compatible with existing electrolytic copper foil production processes, requiring no additional modifications to the production line, and possesses good prospects for large-scale promotion.
[0050] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit and principles of the invention. The embodiments disclosed above are merely preferred embodiments of the present invention and are not intended to limit the invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. An electrolyte additive for bend-resistant lithium battery copper foil, characterized in that: The product comprises the following components: a wetting agent composed of collagen, hydroxyethyl cellulose, polyethylene glycol, and disodium salt of fatty alcohol polyoxyethylene ether sulfosuccinate monoester; sodium polydisulfide dipropane sulfonate as an accelerator; and a grain refiner composed of one or more of tetrahydrothiazolyl thiophene and its derivatives. The total concentration of the wetting agent, accelerator, and grain refiner ranges from 2 mg / L to 80 mg / L, and the mass ratio of the wetting agent, accelerator, and grain refiner is (10~20): (20~40): (2~5).
2. A method for preparing bend-resistant lithium-ion battery copper foil, characterized by: Includes the following steps: Add the electrolyte additive for resistant lithium-ion battery copper foil as described in claim 1 to the copper sulfate electrolyte, and stir evenly to obtain the working electrolyte; Under constant current electrolysis conditions, a titanium cathode roller is used as the cathode for electrolytic deposition to generate a copper deposition layer on the surface of the cathode roller. After peeling, a bend-resistant lithium battery copper foil is obtained.
3. The method for preparing the bend-resistant lithium-ion battery copper foil as described in claim 2, characterized in that: Cu in copper sulfate electrolyte 2 + The concentration was 90 g / L~95 g / L, the H2SO4 concentration was 100 g / L~110 g / L, the copper sulfate electrolyte temperature was 50±2 ℃, and the basic chloride ion concentration was 30±2 ppm.
4. The method for preparing the bend-resistant lithium-ion battery copper foil as described in claim 2, characterized in that: The current density of the constant current electrolysis is 3000 A / m. 2 ~4500 A / m 2 .
5. Bending-resistant lithium battery copper foil, characterized by: It is made by the method for preparing the bend-resistant lithium battery copper foil according to any one of claims 2-4.
6. The bend-resistant lithium battery copper foil as described in claim 5, characterized in that: The bend-resistant lithium-ion battery copper foil has a thickness of 6μm and an original tensile strength of 500 MPa~650 MPa.
7. The bend-resistant lithium battery copper foil as described in claim 5, characterized in that: The bending-resistant lithium-ion battery copper foil exhibits a tensile strength attenuation rate of <20% after a 0°R angle bending test.
Citation Information
Patent Citations
Preparation method and additive of electrolytic copper foil for lithium-ion battery with high bending resistance
CN115478305B
Method for improving high-temperature ductility of copper foil by regulating and controlling molecular weight of additive and application
CN119332313A