Additive for electrolytic copper foil, electrolyte and application thereof
By using a combination of additives including sodium polydithiopropanesulfonate, sodium N,N-dimethyldithioformamide propanesulfonate, polyethylene glycol-epoxychloropropane copolymer, hydroxypropyl methylcellulose, and nano carbon dots, the problem of decomposition of traditional additives under high temperature and high current density was solved, achieving high temperature stability and efficient deposition of copper foil, and reducing production costs.
Patent Information
- Application Number
- CN202611475937.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional electrolytic copper foil additives are prone to oxidation and decomposition under high temperature and high current density conditions, resulting in coarse copper foil crystals and poor thickness uniformity, which affects the consistency of lithium battery cells and increases production costs.
A combination of additives, including sodium dithiodipropanesulfonate, sodium N,N-dimethyldithioformamide propanesulfonate, polyethylene glycol-epoxychloropropane copolymer, hydroxypropyl methylcellulose, and carbon nanodots, was used to improve high-temperature stability and copper foil deposition efficiency through the synergistic effect of N and S co-doped carbon nanodots.
At high temperatures of 65-75℃ and high current densities of 6000-10000A/m², the additive decomposition rate is less than 5%, the copper foil thickness uniformity is ≤±4.2%, the tensile strength is ≥410MPa, and the elongation is ≥15.8%, which reduces electrolyte maintenance costs and improves production stability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to an additive for electrolytic copper foil, its electrolyte, and its application, belonging to the field of electrolytic copper foil technology. Background Technology
[0002] In the production of electrolytic copper foil, additives are key factors in controlling the crystal quality, surface morphology, and mechanical properties of the copper foil. With the development of lithium batteries towards higher energy densities, higher requirements are being placed on the thickness uniformity, tensile strength, and elongation of the copper foil.
[0003] Traditional electrolytic copper foil additives are typically only suitable for operation at relatively low electrolyte temperatures of 45-55℃. Increasing the electrolyte temperature can improve electrolyte conductivity, allowing for higher current densities, and simultaneously accelerate copper ion diffusion and copper dissolution rates, significantly improving copper foil deposition efficiency. However, at high temperatures (>65℃), commercially available conventional additives are prone to oxidation, hydrolysis, and decomposition, resulting in coarse copper foil crystals. This not only limits further increases in deposition rate but also causes poor copper foil thickness uniformity (copper foil thickness deviation rate ≥±8%), directly affecting the consistency of lithium battery cells. Furthermore, the large-scale decomposition of additives at high temperatures generates byproducts, requiring frequent electrolyte purification and replacement, significantly increasing production costs.
[0004] Currently, commonly used additives in the industry, such as gelatin-based, ordinary polyether-based, and single organic sulfonate-based additives, exhibit poor stability under high temperature and high current density conditions, making them unsuitable for modern high-speed, high-temperature electrolytic copper foil production lines. Most existing patents only involve compounding organic sulfonates and polyethers, failing to balance high-temperature stability with the mechanical and morphological properties of copper foil. Therefore, developing an additive system suitable for high-temperature electrolysis conditions is particularly important. Summary of the Invention
[0005] This invention addresses the problems of traditional electrolytic copper foil additives decomposing and failing under high-temperature environments and being unable to adapt to high-current-density production conditions, by providing an additive for electrolytic copper foil, its electrolyte, and its application.
[0006] In this invention, the amount of nano carbon dots used is calculated based on the weight content of total organic carbon in the solution; Doping amount is calculated as mass doping amount.
[0007] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: An additive for electrolytic copper foil comprises the following components in parts by weight: Sodium dithiopropane sulfonate 10-30 parts, sodium N,N-dimethyldithioformamide propane sulfonate 20-40 parts, polyethylene glycol-epoxychloropropane copolymer 20-30 parts, hydroxypropyl methylcellulose 5-15 parts, and nano carbon dots 0.1-1 parts.
[0008] Preferably, the number average molecular weight of the polyethylene glycol-epoxychloropropane copolymer (CAS: 72207-80-8) is 8000-15000.
[0009] Preferably, the surface of the nanocarbon dots has carboxyl and sulfonic acid functional groups, the average particle size is 2-8 nm as measured by transmission electron microscopy (TEM), and they exist in an aqueous solution with a total organic carbon (TOC) content of 15.6-20.8 g / L. The quantitative analysis by ICP-MS shows that the S doping amount is 3.1-6.2% and the N doping amount is 8.8-12.6%.
[0010] The present invention also provides an electrolyte for preparing electrolytic copper foil, comprising the above-mentioned additives for electrolytic copper foil.
[0011] Preferably, the amount of the additive for electrolytic copper foil added to the electrolyte is 10-50 mg / L.
[0012] Preferably, the electrolyte contains the following components at the following concentrations: Copper ions 80-120 g / L, sulfuric acid 90-130 g / L, chloride ions 30-80 mg / L.
[0013] The present invention also provides the application of the above-mentioned additives for electrolytic copper foil in the preparation of electrolytic copper foil.
[0014] Preferably, the process conditions for preparing electrolytic copper foil include: electrolyte temperature 65-75 ℃, current density 6000-10000 A / m².
[0015] The present invention also provides the application of the above-mentioned electrolyte in the preparation of electrolytic copper foil.
[0016] The present invention also provides an electrolytic copper foil, the raw materials for which include the aforementioned additives for electrolytic copper foil or the aforementioned electrolyte.
[0017] The beneficial effects of this invention are as follows: The additive provided by this invention exhibits significantly improved high-temperature and long-term stability at 65-75℃ and 6000-10000 A / m. 2After continuous electrolysis for 240 hours under high current density conditions, the decomposition rate was less than 5%, which is significantly better than the traditional gelatin-polyether system, the system with organic components exceeding the scope of this invention by weight, and the ordinary nano carbon dot system containing only carboxyl groups without N and S doping. This indicates that the present invention effectively inhibits the oxidation and hydrolytic decomposition of additives at high temperatures through the synergistic effect of sulfur-containing brightening / leveling components, polyether-cellulose inhibiting components, and N and S co-doped nano carbon dots. It can maintain the effective component concentration for a long time, avoid frequent purification and replacement of electrolyte due to the large amount of additive decomposition, thereby reducing electrolyte maintenance costs and reducing production fluctuations.
[0018] The overall performance of copper foil is improved simultaneously and its process adaptability is good: the additives of this invention can be used at 65-75℃ and 6000-10000 A / m 2 It can be used stably under certain conditions (traditional additives are usually only suitable for 45-55℃), with an addition amount of only 10-50 mg / L. All components are conventional commercially available raw materials. It can be applied directly without modifying existing high-temperature and high-speed electrolytic copper foil production lines, and can significantly improve the deposition efficiency of electrolytic copper foil. Detailed Implementation
[0019] The principles and features of the present invention are described below. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.
[0020] Unless otherwise specified, the raw materials used in the specific embodiments of the present invention are all obtained through conventional commercial channels.
[0021] In a specific embodiment of the present invention, the surface of the nano-carbon dots has carboxyl and sulfonic acid functional groups. Transmission electron microscopy (TEM) shows an average particle size of 2-8 nm. The solution contains a total organic carbon (TOC) content of 15.6-20.8 g / L. ICP-MS quantifies the S doping amount to be 3.1-6.2% and the N doping amount to be 8.8-12.6%. Example 1: An additive for electrolytic copper foil and its application An additive for electrolytic copper foil is prepared by mixing the following components in the indicated weight ratios: 20 parts of sodium dithiodipropane sulfonate, 30 parts of sodium N,N-dimethyldithiocarbamate propane sulfonate, 25 parts of polyethylene glycol-epoxychloropropane copolymer (number average molecular weight 10,000), 10 parts of hydroxypropyl methylcellulose, and 0.5 parts of nano carbon dots (particle size 5 nm, TOC 20.8 g / L, S doping 3.1%, N doping 12.6%). Add 14.5 parts of deionized water to the additive for electrolytic copper foil, stir and dissolve at 50°C for 2 hours to obtain the additive solution for electrolytic copper foil.
[0022] To contain Cu 2+ 100 g / L, H2SO4 110 g / L, Cl - The above-mentioned additive solution for electrolytic copper foil was added to a solution containing 50 mg / L components to make the concentration of the additive for electrolytic copper foil 30 mg / L, thus obtaining an electrolytic copper foil electrolyte containing the additive.
[0023] Copper foil electrolytic deposition was performed using an electrolytic copper foil electrolyte. Electrolysis conditions: temperature 70℃, current density 8000 A / m²; cathode roller speed: 3.3 m / min; preparation thickness: 15 μm.
[0024] Example 2 An additive for electrolytic copper foil and its application An additive for electrolytic copper foil is prepared by mixing the following components in the indicated weight ratios: 15 parts of sodium dithiodipropane sulfonate, 38 parts of sodium N,N-dimethyldithiocarbamate propane sulfonate, 20 parts of polyethylene glycol-epoxychloropropane copolymer (number average molecular weight 10,000), 14.5 parts of hydroxypropyl methylcellulose, and 0.15 parts of nano carbon dots (particle size 3 nm, TOC 15.6 g / L, S doping 6.2%, N doping 8.8%). Add 12.35 parts of deionized water to the additive for electrolytic copper foil, stir and dissolve at 50°C for 2 hours to obtain the additive solution for electrolytic copper foil.
[0025] To contain Cu 2+ 80 g / L, H2SO4 120 g / L, Cl - The above-mentioned additive solution for electrolytic copper foil was added to a 40 mg / L solution to make the concentration of the additive for electrolytic copper foil 15 mg / L, thus obtaining the electrolytic copper foil electrolyte.
[0026] Copper foil electrolytic deposition was performed using an electrolytic copper foil electrolyte. Electrolysis conditions: temperature 75℃, current density 6500 A / m²; cathode roller speed: 2.8 m / min; preparation thickness: 18 μm.
[0027] Example 3 An additive for electrolytic copper foil and its application An additive for electrolytic copper foil is prepared by mixing the following components in the indicated weight ratios: 25.6 parts of sodium dithiopropane sulfonate, 20 parts of sodium N,N-dimethyldithioformamide propane sulfonate, 29 parts of polyethylene glycol-epoxychloropropane copolymer (number average molecular weight 10000), 5 parts of hydroxypropyl methylcellulose, and 0.95 parts of nano carbon dots (particle size 8 nm, TOC 18.2 g / L, S doping 4.4%, N doping 9.8%). Add 19.45 parts of deionized water to the additive for electrolytic copper foil, and stir to dissolve at 50°C for 2 hours to obtain the additive solution for electrolytic copper foil.
[0028] To contain Cu 2+ 120 g / L, H2SO4 100 g / L, Cl - The above-mentioned additive solution for electrolytic copper foil was added to a solution containing 75 mg / L components to make the concentration of the additive for electrolytic copper foil 45 mg / L, thus obtaining an electrolyte for electrolytic copper foil.
[0029] Copper foil electrolytic deposition was performed using an electrolytic copper foil electrolyte. Electrolysis conditions: temperature 66℃, current density 9500 A / m²; cathode roller speed 4.12 m / min; preparation thickness 12 μm.
[0030] Comparative Example 1 Gelatin-polyether additives were prepared by mixing the following components in the indicated weight ratios: 25 parts gelatin, 45 parts polyethylene glycol (molecular weight 10000), 15 parts thiourea, and 15 parts sodium polydisulfide dipropane sulfonate. The resulting powder was a comparative additive.
[0031] Add 20 parts of deionized water to the above-mentioned comparative additive powder, stir and dissolve at 50°C to prepare a stock solution.
[0032] Gelatin-polyether additives were obtained; To contain Cu 2+ 100 g / L, H2SO4 110 g / L, Cl - The above solution was added to a solution containing 50 mg / L of the additive to make the concentration of the additive for electrolytic copper foil 30 mg / L, thus obtaining the electrolyte for electrolytic copper foil.
[0033] Copper foil electrolytic deposition was performed using an electrolytic copper foil electrolyte. Electrolysis conditions: temperature 70℃, current density 8000 A / m²; cathode roller speed: 4 m / min; preparation thickness: 12 μm.
[0034] Comparative Example 2 The only difference between this comparative example and Example 1 is the component ratio in the additive for electrolytic copper foil. Specifically, 35 parts of sodium dithiodipropane sulfonate, 18 parts of sodium N,N-dimethyldithioformamide propane sulfonate, 35 parts of polyethylene glycol-epoxychloropropane copolymer (number average molecular weight 10,000), 4 parts of hydroxypropyl methylcellulose, and 1.2 parts of nano carbon dots (particle size 5 nm, TOC 20.8 g / L, S doping 3.1%, N doping 12.6%) are mixed to obtain the additive for electrolytic copper foil.
[0035] Comparative Example 3 The only difference between this comparative example and Example 1 is the component ratio in the additive for electrolytic copper foil. Specifically, 8 parts of sodium dithiodipropane sulfonate, 42 parts of sodium N,N-dimethyldithioformamide propane sulfonate, 18 parts of polyethylene glycol-epoxychloropropane copolymer (number average molecular weight 10000), 16 parts of hydroxypropyl methylcellulose, and 0.08 parts of nano carbon dots (particle size 5 nm, TOC 20.8 g / L, S doping 3.1%, N doping 12.6%) are mixed to obtain the additive for electrolytic copper foil.
[0036] Comparative Example 4 The only difference between this comparative example and Example 1 is the content of functional groups on the carbon dots.
[0037] Ordinary carboxyl-modified nanocarbon dots were used: with a particle size of 5 nm, only carboxyl functional groups on the surface, a TOC of 20.7 g / L, and no S or N doping; the weight parts of all other organic components, electrolyte composition, additive concentration, and electrolysis process conditions were all consistent with those in Example 1.
[0038] Test case For the test samples of the examples and comparative examples, the relevant test methods in IPC-TM-650 were followed. Specifically, the total thickness of the copper foil was determined according to IPC-TM-650 2.2.12.1, and the relative deviation of multiple sampling points was expressed as ±x%. The tensile strength and elongation were determined according to IPC-TM-650 2.4.18, with 5 samples taken in each direction and the average value of each direction taken. Rz (DIN) was measured using a contact profilometer according to IPC-TM-650 2.2.17A.
[0039] The results are shown in Table 1.
[0040] Table 1. Data from Examples and Comparative Examples
[0041] Based on the above, it can be seen that Examples 1-3 of the present invention are products provided by the present invention; under high temperature and high current density conditions of 66-75℃, the decomposition rate of additives in 240h continuous cycles is less than 5%; the copper foil thickness uniformity is ≤±4.2%, the tensile strength is ≥410MPa, the elongation is ≥15.8%, and Rz≤1.82μm, with the best overall performance. Comparative Example 1 is the existing technology system of traditional gelatin-polyether, without functionalized nano carbon dots; the additives under high temperature conditions undergo severe decomposition, with a decomposition rate as high as 21.4%; the copper foil thickness uniformity is poor, the mechanical properties are significantly reduced, and the roughness is increased, proving that the traditional system cannot be adapted to high-temperature long-cycle production. The weight proportions of each component of the additives used in Comparative Examples 2 and 3 exceeded the protection range defined by this invention, and the components could not form optimal synergy; the decomposition rate of the additives increased to more than 10%; the uniformity of copper foil thickness, tensile strength, elongation and roughness deteriorated simultaneously, proving that the specific weight proportions of this invention are a necessary condition for achieving the effects of this invention. Comparative Example 4 was simply replaced with ordinary carbon dots containing only carboxyl groups and no N or S doping, and the organic component distribution ratio was exactly the same as in Example 1; however, it lacked the N and S co-doped multifunctional group synergy, and the additive decomposition rate increased to 9.2%. The copper foil thickness uniformity, mechanical properties, and surface roughness all deteriorated significantly, proving that the N and S co-doped multifunctional group nano carbon dots specified in this invention are the key components for achieving the high temperature stability and high performance of the copper foil in this invention.
[0042] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. An additive for electrolytic copper foil, characterized by, The components include the following parts by weight: Sodium dithiopropane sulfonate 10-30 parts, sodium N,N-dimethyldithioformamide propane sulfonate 20-40 parts, polyethylene glycol-epoxychloropropane copolymer 20-30 parts, hydroxypropyl methylcellulose 5-15 parts, and nano carbon dots 0.1-1 parts; The total organic carbon content of the nano carbon dots is 15.6-20.8 g / L, and the quantitative analysis by ICP-MS shows that the S mass doping content is 3.1-6.2% and the N mass doping content is 8.8-12.6%.
2. The additive for electrolytic copper foil according to claim 1, characterized by, The number-average molecular weight of the polyethylene glycol-epoxychloropropane copolymer is 8000-15000.
3. The additive for electrolytic copper foil according to claim 1, characterized by, The nano carbon dots have a particle size of 2-8 nm and contain carboxyl and sulfonic acid functional groups on their surface.
4. An electrolytic solution for producing an electrolytic copper foil, characterized by comprising: It contains the additives for electrolytic copper foil as described in any one of claims 1-3.
5. The electrolyte according to claim 4, characterized in that, The amount of additive used in the electrolytic copper foil is 10-50 mg / L.
6. The electrolyte of claim 4, wherein, It contains the following concentrations of ingredients: Copper ions 80-120 g / L, sulfuric acid 90-130 g / L, chloride ions 30-80 mg / L.
7. The use of the additive for electrolytic copper foil as described in any one of claims 1-3 or the electrolyte as described in claim 4 in the preparation of electrolytic copper foil.
8. Use according to claim 7, characterized in that, The process conditions for preparing the electrolytic copper foil include: electrolyte temperature 65-75 ℃, current density 6000-10000 A / m 2 .
9. An electrolytic copper foil, characterized by, The raw materials for its preparation include the additives for electrolytic copper foil as described in any one of claims 1-3 or the electrolyte as described in claim 4.