A process for improving wheel hub coating adhesion using micro-arc oxidation treatment
By using a micro-arc oxidation process to form a porous-rough dual physical anchoring structure on the wheel hub surface, combined with hot water sealing and chemical modification treatment, the problem of easy peeling off of the wheel hub coating is solved, and the adhesion and corrosion resistance are improved. It is suitable for aluminum alloy and magnesium alloy wheels.
Patent Information
- Application Number
- CN202611391700.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to form a highly adhesive coating on the surface of car wheel hubs, resulting in the coating being prone to peeling off, affecting appearance and corrosion resistance.
The micro-arc oxidation process is adopted to form a porous-rough dual physical anchoring structure through gradient pressure increase, and combined with hot water sealing and chemical modification treatment to improve the adhesion between the coating and the micro-arc oxidation film.
It significantly improves the adhesion and salt spray resistance of the wheel hub coating, extends the service life of the wheel hub, and is suitable for aluminum alloy and magnesium alloy wheels.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of automotive wheel hub surface treatment technology, and more specifically, to a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment. Background Technology
[0002] As a key component of a vehicle, automotive wheels not only need to possess sufficient mechanical strength, corrosion resistance, and weather resistance, but also need to have good aesthetics. Corrosion resistance, weather resistance, and aesthetics are largely determined by the coating on the wheel surface. It can be said that the surface coating has a significant impact on the service life and appearance stability of the wheel. However, during long-term service, the surface coating of the wheel is prone to peeling. This not only affects the appearance, but also easily leads to the direct exposure of the wheel substrate, which aggravates wheel corrosion and affects its mechanical properties.
[0003] To address the issue of easy coating peeling off wheel hub surfaces, existing technologies often employ pretreatment processes such as sandblasting, phosphating, and anodizing. However, these processes generally have certain drawbacks, such as: ① Sandblasting: While sandblasting creates a physically rough surface and increases the wheel hub's surface roughness to some extent, it cannot form a chemical interface bond, resulting in limited improvement in coating adhesion. Under humid, hot, or impact conditions, the coating is still prone to peeling. ② Phosphating: Although phosphating is a mature and low-cost process, the resulting phosphating film is thin, has low density, poor corrosion resistance, limited compatibility with organic coatings, and weak chemical bonding. The improvement in coating adhesion is still insufficient, leading to blistering and peeling issues during long-term use. ③ Anodizing:
[0004] The resulting anodic oxide film is porous and has high internal stress. The coating is prone to penetration along the pores, leading to interface cracking and failing to meet high durability requirements.
[0005] In summary, there is an urgent need for a coating process that can form a high-adhesion coating on the wheel hub surface to improve the adhesion of the coating on the wheel hub surface, thereby solving the problem that traditional pretreatment processes cannot ensure that the coating on the wheel hub surface does not peel off. Summary of the Invention
[0006] The purpose of this invention is to provide a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment, aiming to solve the problem that the coating on the wheel hub surface is prone to peeling off during long-term service, which affects the appearance and corrosion resistance of the wheel hub.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solution:
[0008] This invention provides a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment, the process comprising the following steps:
[0009] S1. Wheel hub pre-surface treatment: The wheel hub is degreased, pickled, neutralized and washed with water to remove oil, oxide scale and impurities from the surface of the wheel hub;
[0010] S2. Micro-arc oxidation treatment: The pretreated wheel hub is placed in a metal tank containing electrolyte, with the wheel hub as the anode and the metal tank as the cathode, and micro-arc oxidation is performed using a gradient voltage mode to form a micro-arc oxide film on the surface of the wheel hub.
[0011] S3. Post-treatment of micro-arc oxidation film: The wheel hub after micro-arc oxidation is immersed in hot water for sealing treatment, and then immersed in an activation solution for modification and drying, so as to introduce active functional groups on the surface of micro-arc oxidation film.
[0012] S4. Preparation of wheel hub coating: First, a primer is applied to the surface of the micro-arc oxide film, and after curing, a topcoat is applied. After curing, a wheel hub coating with high adhesion is obtained.
[0013] The present invention proposes a process for improving the adhesion of wheel hub coatings by using micro-arc oxidation treatment. Through a gradient pressure micro-arc oxidation treatment process, the thickness, roughness, and porosity of the micro-arc oxidation film can be controlled to construct a porous-rough dual physical anchoring structure. Then, by using hot water sealing and chemical modification treatment, the subsequent coating and the micro-arc oxidation film can achieve dual enhancement of chemical bonding and physical anchoring, thereby significantly improving the adhesion of the coating.
[0014] The process of this invention can achieve a wheel hub coating adhesion of level 0 and a salt spray resistance of ≥1000h. It is compatible with aluminum alloy and magnesium alloy wheels, and the process is stable and cost-controllable, solving the problems of low adhesion and poor corrosion resistance of traditional processes.
[0015] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: the degreasing process in step S1 is as follows: the wheel hub is immersed in a degreasing solution at 40-60°C for 5-15 minutes of ultrasonic treatment to achieve degreasing;
[0016] The degreasing solution comprises the following components by mass fraction: 5.0–15.0 wt% inorganic compound, 0.1–0.3 wt% nonionic surfactant, and the balance being deionized water; the inorganic compound is selected from at least two of sodium hydroxide, sodium carbonate, and trisodium phosphate.
[0017] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: the pickling process in step S1 is as follows: the wheel hub is immersed in a sulfuric acid solution with a concentration of 10.0-20.0 wt% or a nitric acid solution with a concentration of 5.0-10.0 wt% at room temperature for 1-5 minutes.
[0018] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: the neutralization process in step S1 is as follows: the wheel hub is immersed in a sodium carbonate solution with a concentration of 5.0 to 15.0 wt% at 40 to 50°C for 1 to 5 minutes.
[0019] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: the electrolyte in step S2 comprises the following components by mass fraction: silicate 2.0-4.0 wt%, sodium aluminate 1.0-2.0 wt%, sodium fluoride 0.5-1.5 wt%, potassium hydroxide 0.5-1.0 wt%, nano silica sol 0.5-1.0 wt%, sodium citrate 0.1-0.5 wt%, aminosilane 0.05-0.1 wt%, and the balance being deionized water.
[0020] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: The gradient voltage boosting mode in step S2 is as follows: First stage: voltage 180-250V, current density 3-5A / dm², processing time 1-3 minutes; Second stage: voltage 320-380V, current density 6-10A / dm², processing time 10-15 minutes; Third stage: voltage 420-480V, current density 10-15A / dm², processing time 5-10 minutes.
[0021] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: Step S3, immerse the wheel hub after micro-arc oxidation treatment in hot water at 80-95℃ for sealing treatment for 1-5 minutes, then immerse it in an activation solution for immersion modification for 5-15 minutes, and dry it at 100-120℃ after immersion.
[0022] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: the activation liquid in step S3 includes the following components by mass fraction: 1.0-5.0 wt% silane coupling agent, 0.01-0.1 wt% accelerator, and the balance being a mixed solvent; the accelerator is aluminum dihydrogen phosphate and / or triethanolamine phosphate; the mixed solvent is a mixture of ethanol and water in a volume ratio of (2-4):1.
[0023] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: in step S4, the thickness of the primer coating is 20-40 μm, and after coating, it is cured at 120-150℃ for 20-30 minutes.
[0024] Furthermore, a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment: in step S4, the topcoat coating thickness is 40-60 μm, and after coating, it is cured at 130-150℃ for 20-30 minutes.
[0025] The beneficial effects of this invention are:
[0026] This invention optimizes the formulation of the micro-arc oxidation electrolyte, utilizes a gradient-pressure micro-arc oxidation process and post-treatment processes, and achieves the formation of a high-roughness, high-chemical-activity micro-arc oxidation film layer on the surface of the wheel hub. This significantly improves the bonding strength between the subsequent coating and the wheel hub substrate, achieving an adhesion level of 0 and improving salt spray resistance by more than 50%, thereby effectively extending the service life of the wheel hub. It is suitable for industrial surface treatment of automotive wheel hubs.
[0027] The preferred electrolyte formulation of this invention has the following technical advantages: ① Silicates and sodium aluminate can form a high-hardness and high-density alumina film (micro-arc oxidation film) on the wheel hub surface, giving the film layer the characteristics of being less prone to cracking and less prone to internal fractures that could lead to coating peeling; ② Thanks to the introduction of nano-silica sol, it can participate in film formation, forming a micro-anchored structure with a firm anchoring effect with the subsequent primer, greatly improving the adhesion of the coating; ③ The introduction of aminosilane can be incorporated into the interior of the film layer during the micro-arc oxidation discharge process, giving the inner wall of the film layer pores silane active groups, enhancing the chemical bonding ability with the coating material, and thus improving the coating adhesion.
[0028] This invention also employs a synergistic post-treatment process combining hot water sealing and activation solution modification. Hot water sealing allows the micropores on the surface of the micro-arc oxidation film to undergo a hydration reaction, generating gel-like hydrated aluminum / silicate, which seals the bottom of the deep micropores. This retains the surface openings for the primer to anchor while preventing corrosive media from penetrating into the wheel hub substrate along the through-holes. Meanwhile, the activation solution containing silane coupling agent can form Si─OH on the film surface after silane hydrolysis. This Si─OH then undergoes dehydration condensation with the hydroxyl groups on the surface of the micro-arc oxidation film to form Si-O-Al covalent bonds. The organic functional groups (amino / epoxy, etc.) at the other end of the silane undergo a cross-linking reaction with the primer resin, achieving chemical interfacial bonding, thereby significantly improving the coating adhesion. Detailed Implementation
[0029] The present invention will be further described in detail below with reference to specific embodiments, but the present invention is not limited to the following embodiments. Any non-substantial modifications and adjustments made by those skilled in the art based on the content of the present invention should fall within the protection scope of the present invention.
[0030] Example 1
[0031] This embodiment 1 provides a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment. The process includes the following steps:
[0032] S1. Pre-surface treatment of wheel hubs: Degreasing, pickling, neutralizing, washing with water and drying are performed on aluminum alloy wheel hubs to remove oil, oxide scale and impurities from the surface of the wheel hubs.
[0033] The degreasing process involves immersing the aluminum alloy wheel hub in a degreasing solution at 45°C for 8 minutes of ultrasonic treatment to achieve degreasing. The degreasing solution comprises the following components by mass fraction: 5.0 wt% sodium hydroxide, 2.0 wt% sodium carbonate, 0.2 wt% nonionic surfactant, and the remainder deionized water.
[0034] The pickling process is as follows: the degreased aluminum alloy wheel hub is immersed in a 15.0wt% sulfuric acid solution and soaked at room temperature for 2 minutes;
[0035] The neutralization process is as follows: the pickled aluminum alloy wheel hub is immersed in an 8.0 wt% sodium carbonate solution and soaked at 40°C for 3 minutes; the neutralized aluminum alloy wheel hub is rinsed with deionized water and then dried.
[0036] S2. Micro-arc oxidation treatment: The pretreated aluminum alloy wheel hub is placed in a stainless steel tank containing electrolyte, with the wheel hub as the anode and the metal tank as the cathode, and micro-arc oxidation is performed using a gradient pressure mode to form a micro-arc oxide film on the surface of the wheel hub.
[0037] The electrolyte comprises the following components by mass fraction: sodium silicate 3.0 wt%, sodium aluminate 1.5 wt%, sodium fluoride 1.0 wt%, potassium hydroxide 0.7 wt%, nano silica sol 0.8 wt%, sodium citrate 0.3 wt%, aminosilane 0.08 wt%, and the balance being deionized water.
[0038] Gradient boost: First stage: voltage 200V, current density 4A / dm², processing time 2 minutes; Second stage: voltage 350V, current density 7A / dm², processing time 10 minutes; Third stage: voltage 450V, current density 12A / dm², processing time 5 minutes.
[0039] S3. Post-treatment of micro-arc oxidation film: The wheel hub after micro-arc oxidation is immersed in hot water at 90°C for 3 minutes for sealing treatment, then immersed in activation solution for 5 minutes for modification, and after immersion, it is dried at 110°C for 10 minutes to introduce active functional groups on the surface of micro-arc oxidation film.
[0040] The activation solution comprises the following components by mass fraction: 2.0 wt% silane coupling agent (KH-550), 0.05 wt% aluminum dihydrogen phosphate, and the balance being a mixed solvent, wherein the mixed solvent is a mixture of ethanol and water in a volume ratio of 5:2.
[0041] S4. Preparation of wheel hub coating: First, a 35μm thick epoxy primer is coated on the surface of the micro-arc oxide film and cured at 130℃ for 25 minutes. Then, a 50μm thick topcoat is coated and cured at 150℃ for 20 minutes. After curing, a wheel hub coating with high adhesion is obtained.
[0042] Example 2
[0043] This embodiment 2 provides a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment. The process includes the following steps:
[0044] S1. Pre-surface treatment of wheel hubs: Degreasing, pickling, neutralizing, washing with water and drying are performed on aluminum alloy wheel hubs to remove oil, oxide scale and impurities from the surface of the wheel hubs.
[0045] The degreasing process involves immersing the aluminum alloy wheel hub in a degreasing solution at 50°C and ultrasonically treating it for 5 minutes. The degreasing solution comprises the following components by mass fraction: 3.0 wt% sodium hydroxide, 2.0 wt% sodium carbonate, 1.0 wt% trisodium phosphate, 0.1 wt% nonionic surfactant, and the remainder deionized water. The pickling process involves immersing the degreased aluminum alloy wheel hub in an 8.0 wt% nitric acid solution at room temperature for 3 minutes. The neutralization process involves immersing the pickled aluminum alloy wheel hub in a 5.0 wt% sodium carbonate solution at 45°C for 2 minutes. The neutralized aluminum alloy wheel hub is then rinsed with deionized water and dried.
[0046] S2. Micro-arc oxidation treatment: The pretreated aluminum alloy wheel hub is placed in a stainless steel tank containing electrolyte, with the wheel hub as the anode and the metal tank as the cathode, and micro-arc oxidation is performed using a gradient pressure mode to form a micro-arc oxide film on the surface of the wheel hub.
[0047] The electrolyte comprises the following components by mass fraction: 2.0 wt% potassium silicate, 1.0 wt% sodium aluminate, 1.5 wt% sodium fluoride, 1.0 wt% potassium hydroxide, 0.5 wt% nano silica sol, 0.2 wt% sodium citrate, 0.05 wt% aminosilane, and the balance being deionized water.
[0048] Gradient boost: First stage: voltage 180V, current density 3A / dm², processing time 3 minutes; Second stage: voltage 320V, current density 6A / dm², processing time 12 minutes; Third stage: voltage 425V, current density 10A / dm², processing time 8 minutes.
[0049] S3. Post-treatment of micro-arc oxidation film: The wheel hub after micro-arc oxidation is immersed in hot water at 85°C for 2 minutes for sealing treatment, then immersed in activation solution for 13 minutes for modification, and after immersion, it is dried at 105°C for 12 minutes to introduce active functional groups on the surface of micro-arc oxidation film.
[0050] The activation solution comprises the following components by mass fraction: 3.5 wt% silane coupling agent (KH-560), 0.02 wt% aluminum dihydrogen phosphate, 0.01 wt% triethanolamine phosphate, and the balance being a mixed solvent, wherein the mixed solvent is a mixture of ethanol and water in a volume ratio of 7:3.
[0051] S4. Preparation of wheel hub coating: First, a 20μm thick epoxy primer is coated on the surface of the micro-arc oxide film and cured at 120℃ for 20 minutes. Then, a 45μm thick topcoat is coated and cured at 130℃ for 25 minutes. After curing, a wheel hub coating with high adhesion is obtained.
[0052] Example 3
[0053] This embodiment 3 provides a process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment. The process includes the following steps:
[0054] S1. Pre-surface treatment of wheel hubs: Degreasing, pickling, neutralizing, washing with water and drying are performed on aluminum alloy wheel hubs to remove oil, oxide scale and impurities from the surface of the wheel hubs.
[0055] The degreasing process involves immersing the aluminum alloy wheel hub in a degreasing solution at 60°C and ultrasonically treating it for 15 minutes. The degreasing solution comprises the following components by mass fraction: 5.0 wt% sodium hydroxide, 5.0 wt% sodium carbonate, 3.0 wt% trisodium phosphate, 0.3 wt% nonionic surfactant, and the remainder deionized water. The pickling process involves immersing the degreased aluminum alloy wheel hub in a 10.0 wt% sulfuric acid solution at room temperature for 5 minutes. The neutralization process involves immersing the pickled aluminum alloy wheel hub in a 15.0 wt% sodium carbonate solution at 50°C for 3 minutes. The neutralized aluminum alloy wheel hub is then rinsed with deionized water and dried.
[0056] S2. Micro-arc oxidation treatment: The pretreated aluminum alloy wheel hub is placed in a stainless steel tank containing electrolyte, with the wheel hub as the anode and the metal tank as the cathode, and micro-arc oxidation is performed using a gradient pressure mode to form a micro-arc oxide film on the surface of the wheel hub.
[0057] The electrolyte comprises the following components by mass fraction: sodium silicate 4.0 wt%, sodium aluminate 2.0 wt%, sodium fluoride 0.5 wt%, potassium hydroxide 0.6 wt%, nano silica sol 1.0 wt%, sodium citrate 0.4 wt%, aminosilane 0.1 wt%, and the balance being deionized water.
[0058] Gradient boost: First stage: voltage 250V, current density 5A / dm², processing time 1 minute; Second stage: voltage 380V, current density 8A / dm², processing time 10 minutes; Third stage: voltage 470V, current density 15A / dm², processing time 5 minutes.
[0059] S3. Post-treatment of micro-arc oxidation film: The wheel hub after micro-arc oxidation is immersed in hot water at 80°C for 5 minutes for sealing treatment, then immersed in activation solution for 8 minutes for modification, and after immersion, it is dried at 120°C for 10 minutes to introduce active functional groups on the surface of micro-arc oxidation film.
[0060] The activation solution comprises the following components by mass fraction: 5.0 wt% silane coupling agent (KH-550), 0.1 wt% triethanolamine phosphate, and the balance being a mixed solvent, wherein the mixed solvent is a mixture of ethanol and water in a volume ratio of 3:1.
[0061] S4. Preparation of wheel hub coating: First, a 40μm thick epoxy primer is coated on the surface of the micro-arc oxide film and cured at 150℃ for 25 minutes. Then, a 60μm thick topcoat is coated and cured at 135℃ for 30 minutes. After curing, a wheel hub coating with high adhesion is obtained.
[0062] Comparative Example 1
[0063] The difference between Comparative Example 1 and Example 1 is that the post-treatment process of the micro-arc oxidation film in Comparative Example 1 does not use hot water sealing treatment, while the rest is the same as in Example 1.
[0064] Comparative Example 2
[0065] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses a traditional phosphating process, while the rest is the same as Example 1.
[0066] test:
[0067] The performance of the wheel hub coatings of Examples 1-3 and Comparative Examples 1-2 was tested, and the results are shown in Table 1 below:
[0068] Table 1 shows the performance test results of Examples 1-3 and Comparative Examples 1-2.
[0069]
[0070] In Table 1, the coating adhesion was tested according to GB / T 9286-1998 standard, the central salt spray resistance was tested according to GB / T10125-2012 standard, and the coating surface roughness was tested using a roughness tester.
[0071] As can be seen from the test results in Table 1, the hot water sealing process used in this invention not only improves the adhesion of the coating but also enhances its corrosion resistance. This invention's process is also significantly superior to traditional phosphating processes, greatly improving the adhesion and corrosion resistance of the wheel hub coating. This invention's process, through optimized electrolyte, gradient pressure boosting, and post-treatment, achieves the preparation of a highly active, high-roughness micro-arc oxidation layer on the wheel hub surface. By employing a physical anchoring and chemical bonding mechanism, it significantly improves the coating's adhesion, solving the problem of easy coating peeling, which greatly affects the wheel hub's appearance and corrosion resistance.
[0072] The above are merely preferred embodiments provided by the present invention and are not intended to limit the present invention. For those skilled in the art, any obvious improvements made without departing from the concept of the present invention should be within the protection scope of the present invention.
Claims
1. A process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment, characterized in that, The process includes the following steps: S1. Wheel hub pre-surface treatment: The wheel hub is degreased, pickled, neutralized and washed with water to remove oil, oxide scale and impurities from the surface of the wheel hub; S2. Micro-arc oxidation treatment: The pretreated wheel hub is placed in a metal tank containing electrolyte, with the wheel hub as the anode and the metal tank as the cathode, and micro-arc oxidation is performed using a gradient voltage mode to form a micro-arc oxide film on the surface of the wheel hub. S3. Post-treatment of micro-arc oxidation film: The wheel hub after micro-arc oxidation is immersed in hot water for sealing treatment, and then immersed in an activation solution for modification and drying, so as to introduce active functional groups on the surface of micro-arc oxidation film. S4. Preparation of wheel hub coating: First, a primer is applied to the surface of the micro-arc oxide film, and after curing, a topcoat is applied. After curing, a wheel hub coating with high adhesion is obtained.
2. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, The degreasing process in step S1 is as follows: the wheel hub is immersed in a degreasing solution at 40-60°C for 5-15 minutes of ultrasonic treatment to achieve degreasing; The degreasing solution comprises the following components by mass fraction: 5.0–15.0 wt% inorganic compound, 0.1–0.3 wt% nonionic surfactant, and the balance being deionized water; the inorganic compound is selected from at least two of sodium hydroxide, sodium carbonate, and trisodium phosphate.
3. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, The pickling process in step S1 is as follows: the wheel hub is immersed in a sulfuric acid solution with a concentration of 10.0-20.0 wt% or a nitric acid solution with a concentration of 5.0-10.0 wt% for 1-5 minutes at room temperature.
4. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, The neutralization process in step S1 is as follows: the wheel hub is immersed in a sodium carbonate solution with a concentration of 5.0 to 15.0 wt% at 40 to 50°C for 1 to 5 minutes.
5. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, The electrolyte in step S2 comprises the following components by mass fraction: 2.0–4.0 wt% silicate, 1.0–2.0 wt% sodium aluminate, 0.5–1.5 wt% sodium fluoride, 0.5–1.0 wt% potassium hydroxide, 0.5–1.0 wt% nano silica sol, 0.1–0.5 wt% sodium citrate, 0.05–0.1 wt% aminosilane, and the balance being deionized water.
6. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, The gradient boost mode in step S2 is as follows: First stage: voltage 180-250V, current density 3-5A / dm², processing time 1-3 minutes; Second stage: voltage 320-380V, current density 6-10A / dm², processing time 10-15 minutes; Third stage: voltage 420-480V, current density 10-15A / dm², processing time 5-10 minutes.
7. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, Step S3: Immerse the wheel hub after micro-arc oxidation treatment in hot water at 80-95℃ for sealing treatment for 1-5 minutes, then immerse it in an activation solution for immersion modification for 5-15 minutes, and dry it at 100-120℃ after immersion.
8. A process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1 or 7, characterized in that, The activation solution in step S3 comprises the following components by mass fraction: 1.0-5.0 wt% silane coupling agent, 0.01-0.1 wt% accelerator, and the balance being a mixed solvent; the accelerator is aluminum dihydrogen phosphate and / or triethanolamine phosphate; the mixed solvent is prepared by mixing ethanol and water in a volume ratio of (2-4):
1.
9. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, In step S4, the thickness of the primer coating is 20-40 μm, and after coating, it is cured at 120-150℃ for 20-30 minutes.
10. The process for improving the adhesion of wheel hub coatings using micro-arc oxidation treatment according to claim 1, characterized in that, In step S4, the topcoat thickness is 40–60 μm, and after coating, it is cured at 130–150 °C for 20–30 minutes.