Preparation method of corrosion-resistant micro-arc oxidation silane composite film on aluminum alloy

By controlling the electrolyte and electrical parameters through micro-arc oxidation treatment, combined with hydroxylation pretreatment and cathodic electrodeposition of silane for pore sealing, a corrosion-resistant micro-arc oxidation silane composite film layer for aluminum alloy was prepared. This solved the corrosion and cracking problems of aluminum alloy protective coatings in the plasma environment of an etching machine, improved the corrosion resistance and bonding strength of the film layer, and extended the service life of the components.

CN123108694APending Publication Date: 2026-11-17PENGLIN TECHNOLOGY IND (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611566024.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing aluminum alloy protective coatings are prone to corrosion, cracking, and peeling under conditions such as etching machine plasma special gas, vacuum thermal cycling, and plasma bombardment, resulting in particulate contamination, which makes it difficult to meet the requirements of long service life and low particulate contamination.

Method used

By controlling the electrolyte composition and electrical parameters for micro-arc oxidation treatment, combined with hydroxylation pretreatment and cathodic electrodeposition of silane for pore sealing, a dense corrosion-resistant micro-arc oxidation silane composite film layer of aluminum alloy is prepared, which enhances the film layer bonding strength and density.

Benefits of technology

It significantly improves the corrosion resistance of the film, extends the service life of aluminum alloy parts, reduces the risk of corrosion and particle release, and is suitable for long-term use in the plasma special gas environment of etching machines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108694A_ABST
    Figure CN123108694A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a corrosion-resistant micro-arc oxidation silane composite film on aluminum alloy, mainly comprising three steps: First, after pretreatment such as substrate grinding and degreasing, micro-arc oxidation is performed to form a film. Using aluminum alloy as the anode and stainless steel as the cathode, a ceramic substrate film is prepared in a sodium silicate-based electrolyte. Next, hydrothermal hydroxylation treatment is performed at 80-100℃ and pH 7-11 for 5-60 minutes to increase the hydroxyl bonding sites in the film. Then, a KH560 / DTMS silane hydrolysate is prepared, with potassium nitrate potentially added. The workpiece is used as the cathode, and platinum as the anode for electrodeposition sealing. Finally, the film is cured at 100-120℃ to obtain the composite film. The hydroxylation pretreatment enhances the silane bonding strength, and cathode electrodeposition promotes silane condensation within the pores, strengthening the sealing effect. In a 5% hydrochloric acid hydrogen bubble corrosion test, the optimal process achieves a hydrogen bubble appearance time of 310 minutes, exhibiting significantly better corrosion resistance than a single micro-arc oxidation film or an impregnated silane sealing film. This reduces particle release and extends the service life of components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy surface treatment technology, specifically relating to a method for preparing a corrosion-resistant micro-arc oxidation silane composite film layer for aluminum alloys. Background Technology

[0002] Aluminum alloys possess excellent specific strength, thermal conductivity, machinability, and weldability, making them a key material for manufacturing components of vacuum chambers in semiconductor etching machines. The aluminum alloy chambers, liners, and spray heads inside the etching machine operate under the special corrosive gas environment of plasma for extended periods. The surfaces of these components are prone to corrosion, and the particulate impurities generated by corrosion can directly cause wafer scrap. Therefore, there is an urgent need to develop aluminum alloy protective coatings adapted to the corrosive conditions of plasma.

[0003] Currently, the mainstream protective coatings for aluminum alloys include two types: hard anodizing coatings and micro-arc oxidation ceramic coatings. Hard anodizing is performed in a low-temperature, high-voltage acidic electrolyte environment, generating an in-situ aluminum oxide protective film on the aluminum alloy substrate surface, consisting of a barrier layer and a porous layer. The film phase is mainly the metastable θ-Al₂O₃ phase, exhibiting good film-substrate adhesion and low production cost. Micro-arc oxidation applies high voltage to the electrolyte, relying on the micro-area spark discharge effect to generate a ceramic film mainly composed of α-Al₂O₃ and γ-Al₂O₃ on the aluminum alloy surface. The film exhibits a structure characterized by a dense inner layer and a porous outer layer, with a metallurgical bond between the film and the substrate, resulting in high hardness and high wear resistance.

[0004] However, both of the above-mentioned coatings inevitably generate structural defects such as micropores and microcracks during the film formation process. The microstructure of the film is greatly affected by the electrolyte composition and electrical process parameters. The Al2O3 film obtained by hard anodizing is mainly composed of the metastable θ-Al2O3 phase, which lacks hardness and chemical stability. It has a fast etching rate in plasma environment and a short service life. The film contains micropores, cracks, and even through-holes. The corrosion free radicals generated by plasma can penetrate the defects and reach the aluminum substrate interface, inducing interfacial corrosion and film peeling. At the same time, the film is brittle and is prone to cracking and failure under vacuum thermal cycling and plasma particle bombardment.

[0005] While micro-arc oxidation ceramic films exhibit high hardness and good impact resistance, the spark discharge film formation process generates numerous micropores and microcracks, increasing the contact area between the film and the plasma corrosion medium. Corrosion free radicals can penetrate these defects to the aluminum substrate interface, initiating interfacial corrosion, film peeling, and releasing particulate contaminants. Simply adjusting the electrolyte composition and electrical parameters is insufficient to simultaneously address the thickness, phase composition, and pore structure of the micro-arc oxidation film. Existing sealing methods are mostly developed for salt spray, acid / alkali, and atmospheric corrosion conditions, lacking solutions for preparing aluminum alloy protective coatings specifically for the unique plasma gas environment of semiconductor etching machines. This makes it difficult to simultaneously meet the practical requirements of long service life and low particulate contamination for components. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing a corrosion-resistant micro-arc oxidation silane composite film on aluminum alloys, which solves the technical problems of existing aluminum alloy protective coatings being prone to corrosion, cracking and peeling, and particle contamination under etching machine plasma special gas, vacuum thermal cycling, and plasma bombardment conditions, thereby improving the plasma corrosion resistance of aluminum alloy parts in etching machines.

[0007] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing a corrosion-resistant micro-arc oxidation silane composite film layer on aluminum alloy, the specific steps of which are as follows: Step 1: Preparation of the micro-arc oxidation film on aluminum alloy: The aluminum alloy surface is sequentially polished, degreased, rinsed with deionized water, and dried. The aluminum alloy is placed in an electrolyte as the anode, and a stainless steel plate is used as the cathode. By adjusting the electrolyte composition and electrical parameters, the aluminum alloy is subjected to micro-arc oxidation treatment to prepare a micro-arc oxidation film on its surface. The electrolyte composition is: 3 g / L ~ 15 g / L sodium silicate, 1 g / L ~ 5 g / L sodium hydroxide, and 0 g / L ~ 5 g / L sodium aluminate. The electrical parameters include: positive current density 1 ~ 10 A / dm2; negative current density 1 ~ 10 A / dm2; frequency 100 ~ 1000 Hz; positive duty cycle 20 ~ 50; negative duty cycle 20 ~ 40; oxidation time: 30 ~ 240 min. Step 2: Pretreatment of the micro-arc oxidation film surface with hydroxylation: The treatment is carried out in a beaker containing deionized water at a temperature of 80℃~100℃. The pH of the deionized water is adjusted to 7~11 using NaOH, and the reaction time is controlled at 5 min~60 min. Heating is performed using an electric heating mantle. After the reaction is complete, the aluminum alloy is removed, rinsed with deionized water, and then dried with cold air. Step 3: Micro-arc oxidation silanization sealing treatment: First, a silane solution is prepared, and then the electrodeposition apparatus is assembled. The aluminum alloy micro-arc oxidation film is placed in the silane solution as the cathode, and a platinum electrode is used as the anode. By controlling the deposition potential and time, defects in the aluminum alloy micro-arc oxidation film are sealed. Then, the sample is removed and cured. The silane solution is composed of silane, deionized water, and anhydrous ethanol after hydrolysis, with 0~0.001 mol / L KNO3 added.

[0008] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention achieves higher density micro-arc oxidation ceramic substrate film by synergistically controlling the thermodynamic and kinetic conditions of micro-arc oxidation film formation through electrolyte composition and electrical parameters, thereby reducing the original defects of the film from the source.

[0009] 2. Before silane sealing, a hydroxylation hydrothermal pretreatment process is added to increase the number of hydroxyl groups on the surface of the micro-arc oxidation ceramic film, providing more chemical bonding sites for silane molecules and significantly improving the bonding strength between the silane sealing layer and the micro-arc oxidation substrate film.

[0010] 3. Silane sealing is achieved by using cathodic electrodeposition. The cathodic polarization increases the local pH inside the pores of the micro-arc oxidation film, promoting the condensation reaction of silane. Potassium nitrate is added to the silane solution, and nitrate ions preferentially undergo cathodic reduction reaction, inhibiting the cathodic hydrogen evolution side reaction. At the same time, it enhances the local alkalization effect inside the pores, greatly improving the sealing effect of pore defects and further improving the overall density and corrosion resistance of the composite film.

[0011] 4. The composite film prepared by this invention is suitable for etching machine plasma special gas, vacuum thermal cycling, plasma bombardment, and airflow scouring conditions, which can reduce the risk of component corrosion and particle release, and extend the service life of aluminum alloy components in semiconductor etching equipment. This invention uses a 5% hydrochloric acid hydrogen bubble accelerated corrosion test to evaluate the corrosion resistance of the film. Under the optimal process of this invention, the hydrogen bubble appearance time can reach the level of 310 minutes, which is much higher than that of single micro-arc oxidation film and ordinary impregnated silane sealing film. Attached Figure Description

[0012] Figure 1 This is a schematic diagram of the overall process framework of this method; Figure 2 Schematic diagram of hydrogen bubble experimental results for 6061 aluminum alloy micro-arc oxidation film, micro-arc oxidation silanization composite film and hydrothermal treatment micro-arc oxidation silanization composite film. Figure 3 The images show the surface morphology, cross-sectional morphology, and elemental distribution of the micro-arc oxidation film, the micro-arc oxidation silanization composite film, and the hydrothermally treated micro-arc oxidation silanization composite film of 6061 aluminum alloy. Detailed Implementation

[0013] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0014] Example 1: After micro-arc oxidation of 6061 aluminum alloy, hydrothermal treatment is used to pre-treat the micro-arc oxidation film with hydroxylation and silane sealing.

[0015] 1. Preparation of micro-arc oxidation film on aluminum alloy: First, the aluminum alloy surface is polished with 150#, 400#, 1000#, and 2000# sandpaper, and treated with anhydrous ethanol and deionized water; the micro-arc oxidation electrolyte composition is selected as 4 g / L sodium silicate, 2 g / L sodium hydroxide, and 1 g / L sodium aluminate; the electrical parameters include: positive current density 4 A / dm2; negative current density 3 A / dm2; frequency 840 Hz; positive duty cycle 30, negative duty cycle 25; oxidation time: 80 min; 2. Pretreatment of micro-arc oxidation film surface hydroxylation: The treatment is carried out in a beaker containing deionized water at a temperature of 95℃, a pH of 7 for the deionized water, and a reaction time of 60 min. An electric heating mantle is used for heating. After the reaction is complete, the aluminum alloy is removed, rinsed with deionized water, and then dried with cold air. 3. Micro-arc oxidation silanization sealing treatment: First, prepare a silane solution by mixing 100ml of silane KH560, 150ml of deionized water, and 150ml of anhydrous ethanol. Adjust the pH of the solution to 5 with acetic acid and hydrolyze for 12 hours. Add 0.02g of KNO3 and stir until homogeneous to obtain the silane solution. Place the aluminum alloy micro-arc oxidation film layer in the silane solution as the cathode and a platinum electrode as the anode. The deposition potential is -1 V vs. SCE, and the deposition time is 20 minutes. This seals the defects in the aluminum alloy micro-arc oxidation film layer. Then, remove the sample, dry it with cold air, and cure it in a 100℃ oven for 30 minutes.

[0016] In the semiconductor manufacturing process, the hydrogen bubble test using a 5% HCl solution is commonly used as a rapid method for evaluating the corrosion resistance of protective coatings on aluminum alloys used in etching machines. For example... Figure 2 As shown, hydrogen bubbles appeared in the aluminum alloy micro-arc oxidation film within 0.6 minutes, indicating that the micro-arc oxidation film is prone to corrosion due to defects. After silane sealing treatment, the time for hydrogen bubble appearance significantly increased to 223 minutes, demonstrating that silane sealing is highly effective in sealing defects in the micro-arc oxidation film and significantly improves its corrosion resistance (e.g., ...). Figure 3(Silane film formation seals defects). Simultaneously, after hydroxylation pretreatment of the micro-arc oxidation film layer followed by silane sealing, the time for hydrogen bubble appearance was further prolonged, indicating that the hydroxylation pretreatment improved the silane sealing effect (e.g., Figure 3 The silane significantly improves the defect sealing effect, further enhancing the density and corrosion resistance of the micro-arc oxidation silane composite film.

[0017] Example 2: The difference from Example 1 is that after the micro-arc oxidation treatment of 6061 aluminum alloy, silane sealing treatment is directly used, and the silane solution does not contain KNO3.

[0018] 1. Preparation of micro-arc oxidation film on aluminum alloy: First, the aluminum alloy surface is polished with 150#, 400#, 1000#, and 2000# sandpaper, and treated with anhydrous ethanol and deionized water; the micro-arc oxidation electrolyte composition is selected as 4 g / L sodium silicate, 2 g / L sodium hydroxide, and 1 g / L sodium aluminate; the electrical parameters include: positive current density 4 A / dm2; negative current density 3 A / dm2; frequency 840 Hz; positive duty cycle 30, negative duty cycle 25; oxidation time: 80 min; 2. Micro-arc oxidation silanization sealing treatment: First, prepare a silane solution by mixing 100ml of silane KH560, 150ml of deionized water, and 150ml of anhydrous ethanol. Adjust the pH of the solution to 5 with acetic acid and hydrolyze for 12 hours, stirring until homogeneous to obtain the silane solution. Place the aluminum alloy micro-arc oxidation film layer in the silane solution as the cathode and a platinum electrode as the anode. The deposition potential is -1.0V vs. SCE, and the deposition time is 20 minutes to seal the defects in the aluminum alloy micro-arc oxidation film layer. Then, remove the sample, dry it with cold air, and cure it in a 120℃ oven for 30 minutes.

[0019] After the above process, the hydrogen bubble test of the micro-arc oxidation film with 5% HCl after silanization treatment took approximately 49 minutes. Compared with Example 1, the hydrogen bubble test result was significantly reduced, indicating that the depolarization reaction of KNO3 in the silane solution can enhance the silanization treatment effect and improve the corrosion resistance of the micro-arc oxidation / silane composite film.

[0020] Example 3: The difference from Example 1 is that after the micro-arc oxidation treatment of 6061 aluminum alloy, a hydroxylation pretreatment is performed, followed by direct silane sealing treatment by impregnation.

[0021] 1. Preparation of micro-arc oxidation film on aluminum alloy: First, the aluminum alloy surface is polished with 150#, 400#, 1000#, and 2000# sandpaper, and treated with anhydrous ethanol and deionized water; the micro-arc oxidation electrolyte composition is selected as 4 g / L sodium silicate, 2 g / L sodium hydroxide, and 1 g / L sodium aluminate; the electrical parameters include: positive current density 4 A / dm2; negative current density 3 A / dm2; frequency 840 Hz; positive duty cycle 30, negative duty cycle 25; oxidation time: 80 min; 2. Pretreatment of micro-arc oxidation film surface hydroxylation: The treatment is carried out in a beaker containing deionized water at a temperature of 95℃, a pH of 7 for the deionized water, and a reaction time of 60 min. An electric heating mantle is used for heating. After the reaction is complete, the aluminum alloy is removed, rinsed with deionized water, and then dried with cold air. 3. Micro-arc oxidation silanization sealing treatment: First, prepare a silane solution by mixing 100ml of silane KH560, 150ml of deionized water, and 150ml of anhydrous ethanol. Adjust the pH of the solution to 5 with acetic acid, hydrolyze for 12 hours, and stir until homogeneous to obtain the silane solution. Use the silane impregnation method to seal the micro-arc oxidation film layer with silane for 20 minutes. Then, remove the sample, dry it with cold air, and cure it in a 120℃ oven for 30 minutes.

[0022] After treatment using the above process, the hydrogen bubble test of the micro-arc oxidation film with 5% HCl after silanization took approximately 35 minutes. Compared with Example 1, the hydrogen bubble test result was significantly reduced, indicating that applying a cathode potential during silanization can enhance the pH value of the silane solution at the through-pores of the micro-arc oxidation film, promote the silane condensation reaction, enhance the silanization effect, and improve the corrosion resistance of the micro-arc oxidation / silane composite film.

[0023] Example 4: The difference from Example 1 is that the micro-arc oxidation process and the silane solution system have been changed.

[0024] 1. Preparation of micro-arc oxidation film on aluminum alloy: First, the aluminum alloy surface is polished with 150#, 400#, 1000#, and 2000# sandpaper, and treated with anhydrous ethanol and deionized water; the micro-arc oxidation electrolyte composition is selected as 6 g / L sodium silicate and 2 g / L sodium hydroxide; the electrical parameters include: positive current density 3 A / dm2; negative current density 2 A / dm2; frequency 400 Hz; positive duty cycle 50, negative duty cycle 30; oxidation time: 120 min; 2. Micro-arc oxidation silanization sealing treatment: First, prepare a silane solution by mixing 60 ml of silane DTMS, 20 ml of deionized water, and 180 ml of anhydrous ethanol. Adjust the pH of the solution to 5 with acetic acid and hydrolyze for 24 hours, stirring thoroughly to obtain the silane solution. Place the aluminum alloy micro-arc oxidation film layer in the silane solution as the cathode and a platinum electrode as the anode. The deposition potential is -1.2 V vs. SCE, and the deposition time is 20 min. This seals the defects in the aluminum alloy micro-arc oxidation film layer. Then, remove the sample, dry it with cold air, and cure it in a 120℃ oven for 30 min. Simultaneously, a comparative method using silane impregnation to seal the micro-arc oxidation film layer with silane is used, with a sealing time of 20 min and a curing time of 30 min in a 120℃ oven.

[0025] After treatment with the above-mentioned micro-arc oxidation process, the defects in the micro-arc oxidation film layer increased. The hydrogen bubble test of the micro-arc oxidation coating with 5% HCl after silanization treatment by electrodeposition was about 60 min, while that after silanization treatment by immersion was about 15 min. This indicates that the structure of the micro-arc oxidation film layer itself, the hydroxylation pretreatment, the electrodeposition, and the KNO3 in the silane solution all have a significant impact on the corrosion resistance of the micro-arc oxidation / silane composite film layer.

[0026] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an anticorrosive micro-arc oxidation silane composite film layer of an aluminum alloy, characterized in that, The specific steps include the following: S1. Preparation of aluminum alloy micro-arc oxidation film; The surface of the aluminum alloy workpiece is pretreated by grinding, degreasing, rinsing with deionized water, and drying. The treated aluminum alloy workpiece is used as the anode and the stainless steel plate is used as the cathode. They are then immersed in the electrolyte to carry out micro-arc oxidation treatment, and a micro-arc oxidation film is generated on the surface of the aluminum alloy workpiece. S2, Hydroxylation pretreatment of micro-arc oxidation film layer The aluminum alloy workpieces that have undergone micro-arc oxidation were placed in deionized water with a pH of 7.11 for hydrothermal hydroxylation treatment at a temperature of 80℃-100℃ for a reaction time of 5 min-60 min. After treatment, the workpieces were removed, rinsed with deionized water, and then dried with cold air. Sodium hydroxide was used to adjust the pH of the deionized water. S3, Electrodeposition of silane for sealing and curing Preparation of silane working solution: Mix silane, deionized water and anhydrous ethanol, adjust the pH and hydrolyze completely. Add 0~0.001mol / L potassium nitrate to the hydrolyzed system and stir until homogeneous to obtain silane working solution. Setting up an electrodeposition apparatus: A pre-hydroxylated aluminum alloy workpiece is used as the cathode and a platinum electrode is used as the anode. Both are immersed in a silane working solution. The deposition potential and deposition time are controlled, and the micro-arc oxide film layer pore defects are sealed by cathode electrodeposition. After sealing, the workpiece is removed, dried, and then cured to obtain a micro-arc silane composite film.

2. The method for preparing the corrosion-resistant micro-arc oxidation silane composite film on aluminum alloy according to claim 1, characterized in that, The electrolyte comprises: sodium silicate 3g / L~15g / L, sodium hydroxide 1g / L~5g / L, and sodium aluminate 0g / L~5g / L.

3. The method of claim 1, wherein the method further comprises the step of: applying a layer of a silane compound on the surface of the aluminum alloy substrate. The parameters for the micro-arc oxidation treatment are configured as follows: positive current density 1-10 A / dm, negative current density 1-10 A / dm, power frequency 100-1000 Hz, positive duty cycle 20-50, negative duty cycle 20-40, and oxidation treatment time 30-240 min.

4. The method of claim 1, wherein the method further comprises the step of: 5 applying a layer of a silane compound on the surface of the aluminum alloy substrate prior to the step of applying the electrolyte solution. 10 In step S1, the polishing process uses 150#, 400#, 1000#, and 2000# sandpaper in sequence for polishing; degreasing is performed using anhydrous ethanol and ultrasonic degreasing.

5. The method of claim 1, wherein the method further comprises the step of: 5.

1. applying a layer of a silane compound on the surface of the aluminum alloy substrate. In step S3, KH560 or DTMS is selected as the silane; acetic acid is used to adjust the pH of the mixture to 46 during the hydrolysis process, and the hydrolysis time is 1224h.

6. The method of claim 1, wherein the method further comprises the step of: In step S3, the deposition potential for electrodeposition is 1.0 V to 1.2 V, and the deposition time is 20 min.

7. The method of claim 1, wherein the method further comprises the step of: applying a layer of a silane compound on the surface of the aluminum alloy after the step of applying the layer of the ceramic compound on the surface of the aluminum alloy. The curing conditions in step S3 are: oven temperature 100-120℃, heat preservation curing for 30 minutes.