Micro-arc oxidation insulation and wear-resistant treatment method for aluminum alloy mid-frame of mobile smart terminals

By adding a composite additive of nano-titanium dioxide and rare earth nitrates to the micro-arc oxidation electrolyte, combined with bipolar pulse power supply and sealing treatment, the problems of poor density of porous layer and uneven film layer in aluminum alloy surface treatment are solved, realizing a ceramic layer with high hardness, wear resistance and good electrical insulation, which is suitable for the durability and signal transmission of aluminum alloy frames in mobile smart terminals.

CN123108697APending Publication Date: 2026-11-17DONGGUAN CHENMING SURFACE TREATMENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611443688.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing micro-arc oxidation technology for aluminum alloy surface treatment suffers from problems such as poor density of the porous layer, limited control of α-Al2O3 phase content, uneven film growth, and uneven electric field distribution, which affect the hardness, wear resistance, and electrical insulation of the ceramic layer.

Method used

An electrolyte containing a composite additive of nano-titanium dioxide and rare earth nitrates is used in conjunction with a bipolar pulse power supply for micro-arc oxidation treatment to form a ceramic layer with high α-Al2O3 content. The porous layer is removed while the dense layer is retained, and then a sealing treatment is performed to improve the wear resistance and electrical insulation of the ceramic layer.

Benefits of technology

It significantly improves the hardness and wear resistance of the ceramic layer, enhances the uniformity and electrical insulation of the film layer, meets the durability and signal transmission requirements of the mid-frame of mobile smart terminals, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108697A_ABST
    Figure CN123108697A_ABST
Patent Text Reader

Abstract

This invention discloses a method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frames for mobile intelligent terminals, comprising the following steps: pre-treating the aluminum alloy mid-frame substrate; placing the pre-treated aluminum alloy mid-frame substrate in an electrolyte containing silicates and composite additives as the anode, and performing micro-arc oxidation treatment using a bipolar pulse power supply to form a ceramic layer metallurgically bonded to the substrate; configuring the time, voltage, and frequency conditions of the micro-arc oxidation treatment to ensure that the volume percentage of α-Al2O3 in the ceramic layer is not less than 45%; removing at least a portion of the loose layer on the surface of the micro-arc oxidized ceramic layer, retaining the dense layer; and sealing the aluminum alloy mid-frame substrate with the micro-arc oxidized ceramic layer. Through the above method, a functional layer with a target crystalline phase is generated in situ on the substrate surface, and after removing the loose surface area, the internal dense area is retained as the working surface, thereby obtaining a high-hardness, wear-resistant, and insulating protective layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of surface treatment technology for aluminum alloy materials in mobile smart terminals, and in particular to a method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frames for mobile smart terminals. Background Technology

[0002] Micro-arc oxidation (MAO) is a surface treatment technology that uses a combination of electrolyte and high-voltage electrical parameters to induce micro-arc discharge on the surface of metals such as aluminum, magnesium, and titanium, generating a ceramic oxide film in situ. The resulting ceramic oxide film possesses the dual advantages of anodic oxidation and ceramic coating, overcoming the shortcomings of aluminum alloys such as low hardness and poor wear resistance. Compared to traditional anodizing, MAO ceramic films exhibit a stronger bond with the substrate, a denser structure, and excellent wear resistance, corrosion resistance, high-temperature impact resistance, and electrical insulation. In recent years, with the trend towards thinner, lighter, and higher screen-to-body ratio mobile smart terminal products, aluminum alloys have become the mainstream structural material. Due to its advantages in improving the wear resistance, corrosion resistance, and insulation properties of metal components, MAO technology has been explored for application in the surface treatment of 3C electronic products such as smartphone bodies.

[0003] However, micro-arc oxidation ceramic layers typically consist of an inner dense layer and an outer porous layer. The porous layer needs to be removed due to its poor density, low hardness, and defects such as micropores and cracks. However, removing the porous layer not only increases the complexity of the process but may also damage the microstructure of the dense layer. Secondly, on aluminum alloy components with complex shapes, uneven electric field distribution leads to inconsistent film growth rates in different areas, affecting the uniformity of thickness and performance. Furthermore, existing processes have limited ability to control the α-Al2O3 phase content in the ceramic layer, while α-Al2O3, as a high-hardness stable phase, directly determines the hardness and wear resistance of the ceramic layer. Therefore, a micro-arc oxidation insulation and wear-resistant treatment method for aluminum alloy frames of mobile intelligent terminals is needed that can effectively control the α-Al2O3 phase content, improve film uniformity, and optimize the porous layer removal process. Summary of the Invention

[0004] The purpose of this invention is to at least solve one of the technical problems existing in the prior art, and to provide a method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame for mobile smart terminals.

[0005] This invention also provides a method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame for mobile smart terminals, comprising the following steps:

[0006] S1: The aluminum alloy frame substrate is pretreated, wherein the aluminum alloy contains 8-12 parts Si, 2-5 parts Mg, and the balance is Al and unavoidable impurities by weight.

[0007] S2: The pretreated aluminum alloy frame substrate is placed in an electrolyte containing silicates and composite additives as the anode, and micro-arc oxidation is performed using a bipolar pulse power supply to form a ceramic layer that is metallurgically bonded to the substrate.

[0008] The concentration of silicate in the electrolyte is 5-15 g / L; the composite additive is a mixture of nano-titanium dioxide and rare earth nitrates; the time, voltage, and frequency conditions of the micro-arc oxidation treatment are configured such that the volume percentage of α-Al2O3 in the ceramic layer is not less than 45%;

[0009] S3: Remove at least part of the loose layer on the surface of the micro-arc oxidation ceramic layer, retain the dense layer, and make the dense layer serve as the outer surface of the aluminum alloy frame;

[0010] S4: The aluminum alloy frame substrate with the micro-arc oxide ceramic layer formed thereon is subjected to a sealing treatment.

[0011] Preferably, the preprocessing includes:

[0012] S11: The aluminum alloy frame substrate is dewaxed using ultrasonic dewaxing. The temperature of the dewaxing solution is 60-80℃, and the treatment time is 5-20 minutes.

[0013] S12: Degreasing treatment is performed on the substrate after S11 treatment using an alkaline degreasing solution at a temperature of 50-70℃ for 5-15 minutes.

[0014] S13: Clean the substrate after S12 treatment by ultrasonic cleaning or spray cleaning with deionized water for 3-10 minutes.

[0015] Preferably, the micro-arc oxidation treatment time is 10-40 min, and the electrolyte temperature is 15-40℃.

[0016] Preferably, the concentration of the nano-titanium dioxide is 1-5 g / L, and the concentration of the rare earth nitrate is 0.1-1.0 g / L.

[0017] Preferably, the electrolyte also contains 0.5-2 g / L of sodium hexametaphosphate dispersant, and the electrolyte is circulated and stirred during the micro-arc oxidation process. The flow rate of the circulation and stirring is 0.5-2 m / s, and the stirring direction is parallel to the substrate surface.

[0018] Preferably, the positive voltage of the bipolar pulse power supply is 400-750V, the negative voltage is 40-350V, and the frequency is 50Hz-2kHz.

[0019] Preferably, the average particle size of the nano-titanium dioxide is 10-50 nm, and the rare earth nitrate is at least one of cerium nitrate or lanthanum nitrate.

[0020] Preferably, the sealing treatment is one of high-temperature hydration sealing, organic resin sealing, or pulse electrodeposition sealing.

[0021] Preferably, the thickness of the micro-arc oxidation ceramic layer is 20μm-50μm.

[0022] Preferably, S3 includes:

[0023] S31: Remove the loose layer on the surface of the micro-arc oxidation ceramic layer by grinding or belt polishing, with a thickness of 5-15μm, until a dense layer with a smooth surface and no visible micropores is exposed.

[0024] S32: The ceramic layer after removing the loose layer is subjected to fine polishing. The fine polishing is performed using diamond polishing paste or fiber polishing wheel with a particle size of W7-W5, so that the surface roughness Ra≤0.4μm.

[0025] S33: The ceramic layer treated in S32 is subjected to ultrasonic cleaning and hot air drying to remove grinding debris remaining on the surface and in the pores. The cleaning solution for ultrasonic cleaning is deionized water, the cleaning time is 3-8 minutes, the drying temperature is 80-100℃, and the drying time is 10-20 minutes.

[0026] Compared with the prior art, the molded case circuit breaker provided by the present invention has the following advantages:

[0027] This invention utilizes nano-titanium dioxide and rare earth nitrates as composite additives in a micro-arc oxidation electrolyte, combined with voltage and frequency control of a bipolar pulse power supply. By leveraging the synergistic effect of nano-titanium dioxide providing a heterogeneous nucleation substrate and rare earth nitrates lowering the α-Al₂O₃ phase transition barrier, the volume fraction of α-Al₂O₃ in the ceramic layer is stably maintained at over 45%, significantly improving the hardness and wear resistance of the ceramic layer. Simultaneously, by removing the loose surface layer and retaining the dense internal layer as the working surface, the dense layer is directly exposed to the outer surface, avoiding the negative impact of the loose layer on the overall performance. The resulting ceramic layer possesses high hardness, excellent wear resistance, and good electrical insulation, meeting the dual requirements of structural durability and signal transmission performance for the frame of mobile intelligent terminals.

[0028] This invention generates a ceramic layer in situ during micro-arc oxidation and removes only the loose layer while retaining the dense layer in post-processing. The process steps are tightly linked, avoiding the problem of uneven electric field distribution on complex-shaped aluminum alloy parts that leads to excessive differences in film thickness. At the same time, the surface roughness Ra≤0.4μm is achieved by fine polishing the dense layer after removing the loose layer. Combined with the sealing treatment to close the residual micropores in the dense layer, the surface smoothness and corrosion resistance of the ceramic layer are effectively improved. The operation is highly controllable and suitable for large-scale continuous production of aluminum alloy frames for mobile smart terminals, showing good prospects for industrial applications. Attached Figure Description

[0029] The present invention will be further described below with reference to the accompanying drawings and embodiments;

[0030] Figure 1 This is the main process flow diagram of the core technology of this invention;

[0031] Figure 2 This is a flowchart of the preprocessing stage of the present invention;

[0032] Figure 3 This is a flowchart illustrating the processing of the present invention;

[0033] Figure 4 This is a correlation diagram of the electrolyte formulation and micro-arc oxidation parameters of the present invention;

[0034] Figure 5 This is a flowchart of the sealing process of the present invention. Detailed Implementation

[0035] This section will describe in detail specific embodiments of the present invention. Preferred embodiments of the present invention are shown in the accompanying drawings. The purpose of the drawings is to supplement the textual description with graphics, so that people can intuitively and vividly understand each technical feature and overall technical solution of the present invention, but they should not be construed as limiting the scope of protection of the present invention.

[0036] Example 1

[0037] This invention discloses a method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame for mobile intelligent terminals, comprising the following steps: S1: Pre-treating the aluminum alloy mid-frame substrate, wherein the aluminum alloy contains 8-12 parts by weight of Si, 2-5 parts of Mg, and the balance being Al and unavoidable impurities; S2: Placing the pre-treated aluminum alloy mid-frame substrate in an electrolyte containing silicates and composite additives as the anode, and performing micro-arc oxidation treatment using a bipolar pulse power supply to form a ceramic layer metallurgically bonded to the substrate; the concentration of silicates in the electrolyte is 5-15 g / L; the composite additive is a mixture of nano-titanium dioxide and rare earth nitrates; the time, voltage, and frequency conditions of the micro-arc oxidation treatment are configured such that the volume percentage of α-Al2O3 in the ceramic layer is not less than 45%; S3: Removing at least a portion of the loose layer on the surface of the micro-arc oxidized ceramic layer, retaining the dense layer, and using the dense layer as the outer surface of the aluminum alloy mid-frame; S4: Sealing the aluminum alloy mid-frame substrate with the micro-arc oxidized ceramic layer formed.

[0038] Pretreatment includes: S11: Dewaxing the aluminum alloy frame substrate using ultrasonic dewaxing at a temperature of 60-80℃ for 5-20 minutes; S12: Degreasing the substrate after S11 using an alkaline degreasing solution at a temperature of 50-70℃ for 5-15 minutes; S13: Cleaning the substrate after S12 using ultrasonic or spray cleaning with deionized water for 3-10 minutes.

[0039] The micro-arc oxidation treatment time is 10-40 min, and the electrolyte temperature is 15-40℃; the concentration of nano-titanium dioxide is 1-5 g / L, and the concentration of rare earth nitrate is 0.1-1.0 g / L; the electrolyte also contains 0.5-2 g / L of sodium hexametaphosphate dispersant, and the electrolyte is circulated and stirred during the micro-arc oxidation treatment at a flow rate of 0.5-2 m / s, with the stirring direction parallel to the substrate surface; the positive voltage of the bipolar pulse power supply is 400-750V, the negative voltage is 40-350V, and the frequency is 50Hz-2kHz; the average particle size of nano-titanium dioxide is 10-50 nm, and the rare earth nitrate is at least one of cerium nitrate or lanthanum nitrate; the sealing treatment is one of high-temperature hydration sealing, organic resin sealing, or pulse electrodeposition sealing; the thickness of the micro-arc oxidation ceramic layer is 20 μm-50 μm;

[0040] S3 includes S31: removing the loose layer on the surface of the micro-arc oxidation ceramic layer by grinding or belt polishing, with a thickness of 5-15μm, until a dense layer with a smooth surface and no visible micropores is exposed; S32: performing fine polishing on the ceramic layer after removing the loose layer, using diamond polishing paste or fiber polishing wheel with a grit size of W7-W5, so that the surface roughness Ra≤0.4μm; S33: performing ultrasonic cleaning and hot air drying on the ceramic layer after S32 to remove grinding debris remaining on the surface and in the pores, using deionized water as the cleaning solution for ultrasonic cleaning, cleaning time of 3-8min, drying temperature of 80-100℃, and drying time of 10-20min.

[0041] The above technical solution involves pre-treating the aluminum alloy frame substrate sequentially with ultrasonic dewaxing, alkaline degreasing, and deionized water cleaning. The pre-treated substrate is then placed in an electrolyte containing silicates and composite additives as the anode, and micro-arc oxidation is performed using a bipolar pulsed power supply. The silicate concentration in the electrolyte is 5-15 g / L, and the composite additive is a mixture of nano-titanium dioxide and rare earth nitrates, supplemented with sodium hexametaphosphate dispersant. During the treatment, the substrate is circulated and stirred parallel to the substrate surface. The positive voltage, negative voltage, frequency, treatment time, and electrolyte temperature are controlled to ensure that the α-Al₂O₃ volume percentage in the resulting ceramic layer is not less than 45% and the ceramic layer thickness is 20-50 μm. Then, a loose layer of 5-15 μm is removed from the ceramic layer surface by grinding or belt polishing. Next, it is finely polished with diamond polishing paste or fiber polishing wheels to Ra ≤ 0.4 μm, followed by ultrasonic cleaning and hot air drying. Finally, the ceramic layer is sealed. This method solves the technical problems of easy peeling of the loose layer on the surface of the micro-arc oxidation ceramic layer of aluminum alloy frame, insufficient corrosion resistance due to high porosity, and poor matching with subsequent coating or appearance requirements. It achieves the technical effects of improving the hardness and bonding of the dense layer, significantly reducing surface roughness, enhancing wear and corrosion resistance, and improving surface smoothness.

[0042] Example 2

[0043] In this embodiment, the aluminum alloy frame matrix comprises 8-12 parts by weight of silicon to improve melt flow and precipitate eutectic silicon phase to enhance wear resistance, 2-5 parts by weight of magnesium to provide age-hardening, and the balance being aluminum and unavoidable impurities. The matrix is ​​pre-formed into a predetermined three-dimensional shape with a frame structure by extrusion or die casting, and undergoes solution aging treatment to ensure uniform dispersion of the strengthening phase, thereby guaranteeing the uniformity of the matrix structure and dimensional stability.

[0044] Before pretreatment, the substrate surface has tool marks from machining, grease, and a thin layer of natural oxide. When it enters the S1 pretreatment, the oil and natural oxide film on the surface are peeled off layer by layer, exposing a fresh and electrochemically active aluminum substrate surface. At the same time, the micro-roughness can be controlled to facilitate uniform nucleation of subsequent discharge.

[0045] During the S2 micro-arc oxidation process, the clean substrate is immersed in the electrolyte as the anode. Under the action of the pulsed electric field, aluminum atoms on the substrate surface participate in the plasma high-temperature chemical reaction in situ. Some aluminum atoms are oxidized and consumed and melted and quenched, gradually transforming into a high-hardness ceramic layer with α-Al2O3 as the main crystal phase. At the same time, silicon and magnesium elements in the substrate partially dissolve in the oxide lattice or agglomerate at the grain boundaries under high temperature, which plays a role in refining grains and inhibiting phase transformation. The ceramic layer grows from the surface of the substrate inward and there is no interface abrupt with the substrate, forming a metallurgical bond. At the same time, due to the reaction diffusion mechanism, a transition zone with gradual compositional change is formed between the ceramic layer and the substrate. The ceramic layer exhibits a gradient structure in the thickness direction, with a loose and porous outer layer and a dense and hard inner layer.

[0046] Subsequently, after S3 processing, the loose portion at the top of the original ceramic layer on the substrate surface is ground away, leaving only the dense layer with a dense internal structure, extremely low porosity, and optimal bonding strength with the substrate. This dense layer directly replaces the original metal surface as the exposed working surface of the middle frame. At this point, the effective outer contour dimension of the substrate is slightly reduced compared to the original state, but the overall rigidity is enhanced due to the support of the ceramic layer.

[0047] Finally, after S4 sealing treatment, the remaining interconnected micropores or microcracks in the dense layer are filled and sealed, thereby constructing a continuous and complete protective barrier on the entire outer surface of the substrate. This barrier, together with the unconverted metal core inside the substrate, constitutes a composite structure. The dense ceramic layer serves as a functional surface layer, undertaking the functions of wear resistance and corrosion resistance, while the aluminum alloy core retains its original toughness to bear structural stress.

[0048] Example 3

[0049] In this embodiment, the pretreatment includes dewaxing, degreasing, and cleaning processes performed sequentially, as detailed below:

[0050] The dewaxing process employs ultrasonic dewaxing. The aluminum alloy frame substrate is immersed in the dewaxing solution and ultrasonic waves are applied. The ultrasonic frequency can be selected as 28kHz or 40kHz, or adjusted within the range of 20kHz to 100kHz depending on the actual working conditions. When a lower frequency range (e.g., 20-40kHz) is used, the cavitation effect is strong, resulting in a powerful cleaning action that facilitates the rapid removal of thick wax and polishing paste residue. When a higher frequency range (e.g., 68-120kHz) is used, the cavitation bubble size is reduced and the distribution is more uniform, resulting in a gentler impact on the substrate surface and reducing the risk of physical damage to the aluminum alloy surface. In practical applications, dual-frequency or multi-frequency methods can also be used. The frequency combination mode balances dewaxing efficiency and surface protection; combined with the dewaxing liquid heated to 60-80℃, it dissolves and emulsifies the wax and polishing paste residues. Utilizing the impact force and micro-jet generated by the ultrasonic cavitation effect, the mechanical polishing wax layer adhering to the substrate surface is peeled off from the metal surface and dispersed in the dewaxing liquid. The processing time is 5-20 minutes. The purpose of this step is to remove the wax and binders remaining on the substrate during machining and polishing processes, providing a wax-free metal surface for subsequent degreasing. After the dewaxing process is completed, the wax residue on the substrate surface is basically removed, exposing the original metal surface and natural oxide film covered by wax.

[0051] The degreasing treatment uses an alkaline degreasing solution. The substrate, after dewaxing, is immersed in the alkaline degreasing solution at 50-70℃ for 5-15 minutes. The hydroxide ions and surfactants in the alkaline degreasing solution react with the residual animal, vegetable, and mineral oils on the substrate surface through saponification and emulsification reactions, converting the oil stains into soluble soaps and emulsified, dispersed small oil droplets that detach from the metal surface. At the same time, the alkaline environment causes slight chemical etching of the natural oxide film on the substrate surface, partially dissolving the thin oxide film. The purpose of this step is to thoroughly remove various oily contaminants from the substrate surface and regulate the natural oxide film, ensuring that the substrate surface is in a uniformly activated state. This is beneficial for the uniform triggering of the initial discharge across the entire substrate surface during subsequent micro-arc oxidation treatment. After the degreasing treatment is completed, the oil stains on the substrate surface are completely removed, the natural oxide film is moderately thinned and homogenized, and the surface exhibits a uniform wetted state.

[0052] The cleaning process involves ultrasonic or spray cleaning of the degreased substrate with deionized water for 3-10 minutes. Through the dissolving and rinsing action of deionized water, residual alkaline degreasing solution components, saponification reaction products, and emulsified oil droplets peeled off from the surface are thoroughly removed from the substrate surface. Ultrasonic cleaning also utilizes cavitation effect to enhance the removal of residues in surface micro-pits and crevices. This step aims to eliminate chemical residues introduced into the substrate surface by previous chemical treatments, preventing residues from interfering with the stability of the electrolyte composition and the uniformity of discharge during micro-arc oxidation. After cleaning, the substrate surface is clean, free of oil, wax, and residual chemicals, and the thickness and uniformity of the natural oxide film on the surface are controlled to a level suitable for the initial discharge of micro-arc oxidation, thus obtaining a substrate ready to be directly processed into the micro-arc oxidation process.

[0053] Example 4

[0054] In this embodiment, to demonstrate the effect of electrolyte temperature on the performance of the micro-arc oxidation ceramic layer, comparative experiments were conducted at five levels: 10℃, 15℃, 27.5℃, 40℃, and 50℃, with fixed nano-titanium dioxide concentration of 3.0 g / L, rare earth nitrate concentration of 0.55 g / L, and treatment time of 30 min. All other process parameters remained consistent, including matrix composition (Si 10 parts, Mg 3 parts, balance Al), silicate concentration of 10 g / L, sodium hexametaphosphate concentration of 1 g / L, positive voltage of 550 V, negative voltage of 150 V, frequency of 500 Hz, and stirring flow rate of 1 m / s parallel to the matrix surface. After micro-arc oxidation treatment under the same conditions, each group of experiments underwent sequential processes including removal of the loose layer, fine polishing to Ra ≤ 0.4 μm, ultrasonic cleaning, and hot air drying. Finally, the thickness, phase composition, and surface roughness of the resulting ceramic layer were tested, as shown in the following figure:

[0055] Experimental group number Electrolyte temperature (°C) Ceramic layer thickness (μm) <![CDATA[Volume fraction of α-Al₂O₃ (%)]]> Surface roughness Ra (μm) Comparison Group 1 10 20.5 40.2 0.50 Implementation Group 1 15 25.3 48.7 0.39 Implementation Group 2 27.5 35.8 61.5 0.26 Implementation Group 3 40 32.6 54.3 0.31 Comparison Group 2 50 38.1 44.6 0.46

[0056] The experimental procedure is as follows: The pretreated aluminum alloy frame substrate was placed in the above-mentioned electrolyte as the anode and subjected to micro-arc oxidation treatment under a bipolar pulse power supply. During the treatment, the electrolyte was continuously circulated and stirred in a direction parallel to the substrate surface. At the same time, the electrolyte temperature was controlled by the cooling system to stabilize within the set value ±1℃ range. After the treatment, the substrate was removed and the loose layer of about 10μm on the surface of the ceramic layer was removed by grinding. Then, it was polished with W5 diamond polishing paste until the surface roughness Ra≤0.4μm. Subsequently, it was ultrasonically cleaned with deionized water for 5min and dried with hot air at 90℃ for 15min. Finally, the thickness of the ceramic layer was measured by an eddy current thickness gauge, the volume fraction of α-Al2O3 was analyzed by X-ray diffraction, and the surface roughness Ra value was measured by a stylus roughness meter. Five measurement points were taken for each group and the average value was recorded.

[0057] The data above shows that when the electrolyte temperature increases from 10℃ to 27.5℃, the ceramic layer thickness increases from 20.5μm to 35.8μm, the α-Al₂O₃ volume fraction increases from 40.2% to 61.5%, and the surface roughness Ra decreases from 0.50μm to 0.26μm. This indicates that increasing the temperature is beneficial for the continued progress of the plasma discharge reaction and the formation of the stable α-Al₂O₃ phase, while also making the ceramic layer surface smoother and denser. When the temperature continues to increase to 40℃, the ceramic layer thickness decreases slightly to 32.6μm. The volume fraction of α-Al₂O₃ decreased to 54.3%, and Ra increased to 0.31 μm, indicating that at excessively high temperatures, electrolyte evaporation intensified, conductivity changes led to decreased discharge stability, reduced α-phase content, and deteriorated surface quality. When the temperature further increased to 50℃, although the ceramic layer thickness abnormally increased to 38.1 μm, the volume fraction of α-Al₂O₃ further decreased to 44.6%, and Ra deteriorated to 0.46 μm, indicating that at excessively high temperatures, the ceramic layer was dominated by the metastable γ-Al₂O₃ phase, and the increased porous layer thickness led to a significant increase in roughness. Based on these results, the ceramic layer exhibits the best overall performance at an electrolyte temperature around 27.5℃. Temperatures that are too low are detrimental to α-phase formation, while temperatures that are too high lead to a decrease in α-phase content and deterioration of surface quality. Therefore, the preferred electrolyte temperature range is 15-40℃, and more preferably 27.5℃.

[0058] Example 5

[0059] In this embodiment, to demonstrate the effect of the concentrations of nano-titanium dioxide and rare earth nitrates on the performance of the micro-arc oxidation ceramic layer, two sets of comparative experiments were conducted with five levels each of nano-titanium dioxide concentration and rare earth nitrate concentration, under the conditions of a fixed electrolyte temperature of 27.5℃ and a treatment time of 30 min. All other process parameters remained consistent, including matrix composition (Si 10 parts, Mg 3 parts, balance Al), silicate concentration 10 g / L, sodium hexametaphosphate concentration 1 g / L, positive voltage 550 V, negative voltage 150 V, frequency 500 Hz, and stirring flow rate 1 m / s parallel to the matrix surface. After micro-arc oxidation treatment under the same conditions, each group of experiments underwent sequential processes including removal of the loose layer, fine polishing to Ra ≤ 0.4 μm, ultrasonic cleaning, and hot air drying. Finally, the thickness, phase composition, and surface roughness of the resulting ceramic layer were tested, as shown in the following figure:

[0060] Experimental group number <![CDATA[Nano TiO₂ concentration (g / L)]]> Rare earth nitrate concentration (g / L) Ceramic layer thickness <![CDATA[Volume fraction of α-Al₂O₃ (%)]]> Surface roughness Ra (μm) C1 0.5 0.55 26.8 42.3 0.44 C2 1.0 0.55 29.5 50.1 0.36 C3 3.0 0.55 35.8 61.5 0.26 C4 5.0 0.55 37.6 55.8 0.29 C5 6.0 0.55 39.2 46.9 0.40 C6 3.0 0.05 31.2 43.7 0.42 C7 3.0 0.1 33.0 52.1 0.34 C8 3.0 0.55 35.8 61.5 0.26 C9 3.0 1.0 36.9 58.3 0.28 C10 3.0 1.5 34.5 50.4 0.38

[0061] The experimental procedure is as follows: The pretreated aluminum alloy frame substrate was placed in the above-mentioned electrolyte as the anode, and micro-arc oxidation was performed under a bipolar pulse power supply. During the treatment, the electrolyte was continuously circulated and stirred, with the stirring direction parallel to the substrate surface. At the same time, the electrolyte temperature was controlled to be stable at 27.5℃±1℃ by the cooling system. In the nano-titanium dioxide concentration group (C1-C5), the rare earth nitrate concentration was fixed at 0.55g / L, and five levels of nano-titanium dioxide concentration were set at 0.5g / L, 1.0g / L, 3.0g / L, 5.0g / L and 6.0g / L, respectively. In the rare earth nitrate concentration group (C6-C10), the nano-titanium dioxide concentration was fixed at... The concentration of rare earth nitrates was set at 3.0 g / L, with five levels of concentrations: 0.05 g / L, 0.1 g / L, 0.55 g / L, 1.0 g / L, and 1.5 g / L. After treatment, the substrate was removed, and a loose layer of about 10 μm on the surface of the ceramic layer was removed by grinding. Then, it was polished with W5 diamond polishing paste until the surface roughness Ra ≤ 0.4 μm. Subsequently, it was ultrasonically cleaned with deionized water for 5 min and dried with hot air at 90℃ for 15 min. Finally, the thickness of the ceramic layer was measured by an eddy current thickness gauge, the volume fraction of α-Al2O3 was analyzed by X-ray diffraction, and the surface roughness Ra value was measured by a stylus roughness meter. Five measurement points were taken for each group, and the average value was recorded.

[0062] The data above show that when the rare earth nitrate concentration is fixed at 0.55 g / L, as the concentration of nano-titanium dioxide increases from 0.5 g / L to 3.0 g / L, the ceramic layer thickness increases from 26.8 μm to 35.8 μm, the volume fraction of α-Al₂O₃ increases from 42.3% to 61.5%, and the surface roughness Ra decreases from 0.44 μm to 0.26 μm. This indicates that the addition of an appropriate amount of nano-titanium dioxide can provide a heterogeneous nucleation substrate for α-Al₂O₃ and refine the grains, thereby promoting the formation of the α phase and improving surface smoothness. Integrity; when the concentration of nano-titanium dioxide continued to increase to 5.0 g / L, the thickness of the ceramic layer increased to 37.6 μm, but the volume fraction of α-Al2O3 decreased to 55.8%, and Ra rose back to 0.29 μm, indicating that excessive nanoparticles agglomerate and settle in the electrolyte, which inhibits effective discharge and α-phase transformation; when the concentration further increased to 6.0 g / L, the volume fraction of α-Al2O3 further decreased to 46.9%, and Ra deteriorated to 0.40 μm, indicating that excessive addition of nanoparticles has a negative effect on the compactness of the ceramic layer.

[0063] Data from groups C6-C10 show that when the concentration of nano-titanium dioxide is fixed at 3.0 g / L, as the concentration of rare earth nitrate increases from 0.05 g / L to 0.55 g / L, the ceramic layer thickness increases from 31.2 μm to 35.8 μm, the volume fraction of α-Al₂O₃ increases from 43.7% to 61.5%, and the surface roughness Ra decreases from 0.42 μm to 0.26 μm. This indicates that the appropriate addition of rare earth nitrate is beneficial to improving the electrolyte conductivity and discharge uniformity, and promoting the complete sintering of the melt to form α-Al₂O₃. 3. Stable Phase: When the rare earth nitrate concentration increased to 1.0 g / L, the ceramic layer thickness further increased to 36.9 μm, but the α-Al₂O₃ volume fraction decreased to 58.3%, and Ra rebounded to 0.28 μm, indicating that excessively high rare earth ion concentrations interfered with the thermodynamic equilibrium of the plasma reaction due to ion competition discharge. When the concentration further increased to 1.5 g / L, the α-Al₂O₃ volume fraction decreased to 50.4%, and Ra deteriorated to 0.38 μm, indicating that the increase in impurity ions introduced by excessive rare earth salts actually inhibited the formation of the α phase. Based on the above results, the preferred concentration range for nano-titanium dioxide is 1-5 g / L, more preferably 3.0 g / L; the preferred concentration range for rare earth nitrate is 0.1-1.0 g / L, more preferably 0.55 g / L. At this concentration, the ceramic layer exhibits the best overall performance, with an α-Al₂O₃ volume fraction of 61.5% and a surface roughness Ra of only 0.26 μm.

[0064] Example 6

[0065] Based on the above embodiments, to demonstrate the effects of the dispersant sodium hexametaphosphate and circulating stirring on the performance of the micro-arc oxidation ceramic layer, the following comparative examples were set with fixed matrix composition (Si 10 parts, Mg 3 parts, balance Al), silicate concentration 10 g / L, nano titanium dioxide concentration 3.0 g / L, rare earth nitrate concentration 0.55 g / L, electrolyte temperature 27.5℃, processing time 30 min, positive voltage 550 V, negative voltage 150 V, and frequency 500 Hz, while keeping other process parameters consistent:

[0066] Comparative Example 1: No sodium hexametaphosphate was added to the electrolyte, and no circulating stirring was performed during the micro-arc oxidation process; the electrolyte was simply kept in a static state. The results showed that due to the severe agglomeration and sedimentation of the nano-titanium dioxide particles in the absence of dispersants and flow disturbance, the electrolyte composition was unevenly distributed along the depth direction, leading to significant differences in discharge intensity and reaction product supply in different regions of the substrate surface. The resulting ceramic layer thickness was only 26.3 μm, the α-Al₂O₃ volume fraction was only 43.8%, and the surface roughness Ra reached 0.48 μm. Furthermore, after the electrolyte was left to stand for 24 h, obvious stratification and sedimentation occurred, with white nanoparticles precipitated at the bottom.

[0067] Comparative Example 2: Sodium hexametaphosphate 1.0 g / L was added to the electrolyte, but no circulating stirring was performed during the micro-arc oxidation process, and the electrolyte was kept in a static state. The results showed that adding the dispersant alone slowed down the aggregation rate of nanoparticles to some extent by utilizing its electrostatic repulsion and steric hindrance, thus improving the stability of the electrolyte. The ceramic layer thickness increased to 28.7 μm, the volume fraction of α-Al2O3 increased to 50.2%, and the surface roughness Ra decreased to 0.42 μm. However, due to the lack of external disturbance from circulating stirring, the dispersant could not overcome the long-term cumulative effect of gravitational sedimentation, and the local concentration of nanoparticles in the bottom region of the electrolyte was still relatively high. Slight stratification sedimentation still occurred after standing for 24 h.

[0068] In this embodiment, sodium hexametaphosphate (1.0 g / L) was added to the electrolyte, and the mixture was continuously stirred during the micro-arc oxidation process at a flow rate of 1.0 m / s, with the stirring direction parallel to the substrate surface. The results showed that the chemical stabilizing effect of the dispersant and the physical suspension effect of the circulating stirring worked synergistically to maintain the nano-titanium dioxide particles in a uniformly suspended state in the electrolyte, with consistent concentration in all regions. Even after the electrolyte had stood for 24 hours, there was no significant sedimentation. Under these conditions, plasma discharge was uniformly triggered and continued across the entire substrate surface, resulting in a ceramic layer thickness of 36.2 μm, an α-Al₂O₃ volume fraction as high as 62.8%, and a surface roughness Ra of only 0.25 μm. The overall performance was significantly better than Comparative Examples 1 and 2.

[0069] It is evident that the combined use of sodium hexametaphosphate and circulating stirring ensures the long-term uniformity of the electrolyte composition and the stability of the discharge process; neither can be dispensed with. The stirring direction parallel to the substrate surface can also avoid interference from vertical flow on the arc discharge and excessive scouring of the molten products, thus facilitating the acquisition of a ceramic layer with high α-Al2O3 content, large thickness, and a smooth and dense surface.

[0070] Example 7

[0071] In this embodiment, the forward voltage of the bipolar pulse power supply is 400-750V. The forward voltage is the main driving force for plasma discharge on the substrate surface during micro-arc oxidation, and its amplitude determines the maximum value of the electric field strength on the anode surface. When the forward voltage is in the range of 400-750V, the microporous region in the oxide film layer on the anode surface first undergoes electrical breakdown and triggers continuous arc discharge. The instantaneous high temperature in the discharge channel causes the melt to generate the α-Al2O3 phase. If the forward voltage is below 400V, it is insufficient to break down the oxide film and trigger discharge, resulting in slow film growth and a low α-phase content. If the forward voltage is above 750V, the discharge is too intense, producing large discharge channels and a thick and loose surface layer, which reduces the density of the ceramic layer and increases the risk of localized substrate erosion.

[0072] The negative voltage is 40-350V. Its function is to provide a reverse electric field to drive positively charged metal ions to move away from the substrate, thereby generating a backwashing and stripping effect on the surface melt and attached particles during the discharge gap. At the same time, it reduces the excessive accumulation of positive charge on the oxide film surface and avoids the polarization effect causing the discharge to concentrate in a local area. If the negative voltage is lower than 40V, the reverse cleaning and dispersion discharge are insufficient, and local sintering nodules are prone to appear on the film surface. If the negative voltage is higher than 350V, the reverse current is too strong, and excessive sputtering removal of the growing oxide film is generated during the discharge gap, which inhibits the accumulation of film thickness.

[0073] The frequency setting of 50Hz-2kHz determines the number of cycles of alternating positive and negative voltages per unit time. At lower frequencies (e.g., 50-500Hz), the duration of a single discharge is longer and the energy density is higher, which is conducive to the full reaction of the melt to form a high-hardness α-Al2O3 phase. However, too low a frequency can easily lead to excessive energy in a single discharge, resulting in coarse pores. At higher frequencies (e.g., 500Hz-2kHz), the pulse density increases and the energy in a single discharge decreases, which is conducive to the uniform distribution of discharge on the substrate surface and the refinement of grains. However, when the frequency is too high (above 2kHz), the energy of a single pulse is insufficient to maintain stable α-phase nucleation and growth, and the α-Al2O3 content decreases instead.

[0074] The three parameters of positive voltage, negative voltage and frequency work together to regulate the magnitude of discharge energy, spatial distribution density of arc discharge and thermodynamic conditions of molten material cooling and crystallization within a single pulse cycle, thereby ensuring that the volume percentage of α-Al2O3 in the ceramic layer is not less than 45%, while taking into account the uniformity of ceramic layer thickness and surface density.

[0075] Example 8

[0076] In this embodiment, the particle size of nano-titanium dioxide is controlled within the range of 10-50 nm because nanoparticles of this size have a high specific surface area and surface activity. During the micro-arc oxidation process, they can be drawn into the plasma discharge channel and sintered together with the melt into the interior of the ceramic layer and the surface micropores, thus filling the micropores, refining the grains, and reducing cracks. If the particle size is less than 10 nm, the surface energy of the particles is too high, which can easily lead to severe agglomeration and make it difficult to disperse evenly. If the particle size is greater than 50 nm, the specific surface area of ​​the particles is insufficient and the mass is too large, making it difficult to suspend in the electrolyte for a long time and increasing the resistance to entering the discharge channel, thus failing to effectively participate in the sintering reaction.

[0077] Furthermore, the rare earth nitrate is at least one of cerium nitrate or lanthanum nitrate. Specifically, cerium nitrate or lanthanum nitrate is chosen for rare earth nitrate because cerium and lanthanum, as light rare earth elements, have unique 4f electronic structures and variable valence states. Under the high temperature and high pressure conditions of micro-arc oxidation discharge, cerium or lanthanum ions can reduce the surface tension of molten oxides, thereby improving melt fluidity and promoting the full spread and filling of pores on the matrix surface. At the same time, rare earth ions generate lattice distortion in the oxide lattice and reduce the nucleation barrier of α-Al2O3 phase transformation, which is conducive to the irreversible transformation from metastable γ-Al2O3 to stable α-Al2O3.

[0078] The combined addition of the two also produces a synergistic effect: the nano-titanium dioxide particles provide an adsorption carrier for rare earth ions in the electrolyte, enabling the rare earth ions to be released into the discharge channel during discharge. The presence of rare earth ions also improves the wettability and sintering activity of the nanoparticles in the melt. The two promote the densification of the ceramic layer and the increase of the α phase content from both physical filling and chemical catalysis levels. This combination of technical features enables the α-Al2O3 volume fraction in the final ceramic layer to stably reach the requirement of not less than 45%, while the number and size of micropores on the surface of the ceramic layer are significantly reduced, and the corrosion resistance and wear resistance are improved simultaneously.

[0079] Example 9

[0080] In this embodiment, the content of α-Al2O3 in the ceramic layer satisfies the following relationship:

[0081]

[0082] in, The percentage of α-Al₂O₃ in the ceramic layer, expressed in %.

[0083] The volume fraction of α-Al2O3 in the ceramic layer obtained under the same micro-arc oxidation process conditions without the addition of nano-titanium dioxide and rare earth nitrates is expressed in %, with a value range of 20%-35%. This value reflects the intrinsic generation ability of the α phase under the basic electrolyte system and electrical parameters. Its specific value depends on fixed process conditions such as matrix composition, silicate concentration, voltage, and frequency.

[0084] The concentration of nano-titanium dioxide in the electrolyte is expressed in g / L and ranges from 1 to 5 g / L. Nano-titanium dioxide participates in the discharge sintering process in the electrolyte as a heterogeneous nucleation substrate and nano-filling phase. The higher the concentration, the more nanoparticles are entrained in the discharge channel per unit time, and the more significant the promoting effect on the formation of α phase.

[0085] The concentration of rare earth nitrates in the electrolyte is expressed in g / L and ranges from 0.1 to 1.0. Rare earth cations dissociated from rare earth nitrates in the electrolyte enter the oxide lattice in the high-temperature discharge region and lower the nucleation barrier of the α-Al2O3 phase transition, thereby catalyzing the irreversible transformation of metastable alumina to the stable α phase.

[0086] t represents the micro-arc oxidation treatment time in minutes, ranging from 10 to 40 minutes. t0 is the baseline unit time, where t0 = 1 minute. Here, the logarithmic form ln(t / t0) is used to characterize the relationship between the α-phase content and the treatment time. This is because the formation of α-Al2O3 during micro-arc oxidation is not linearly related to time. Instead, as the treatment time increases, the repeated melting and cooling cycles within the discharge channel cause the α-phase grains to gradually grow and accumulate. However, the growth rate gradually slows down as the ceramic layer thickens. The logarithmic form more accurately reflects this kinetic characteristic of gradual saturation.

[0087] The contribution coefficient of K1 nano-titanium dioxide, with a value range of 2.0-4.0, represents the incremental contribution of nano-titanium dioxide concentration to the volume fraction of α-Al2O3 when the concentration increases by 1 g / L.

[0088] The contribution coefficient of rare earth nitrate K2, with a value range of 5.0-10.0, represents the incremental contribution of rare earth nitrate concentration to the volume fraction of α-Al2O3 when the concentration increases by 1 g / L.

[0089] The contribution coefficient of the K3 time logarithm, ranging from 5.0 to 15.0, represents the incremental contribution to the volume fraction of α-Al2O3 when the processing time increases by one natural logarithmic unit (i.e., when the time is increased by e times).

[0090] This formula integrates the quantitative contributions of three key variables—nano-titanium dioxide concentration, rare earth nitrate concentration, and treatment time—into the model. It reflects the main effects of each factor acting independently, and also implies the interaction trends between factors through linear superposition. The logarithmic transformation of time ensures that the model has good numerical stability and predictability across the entire parameter range. Within a given parameter range, those skilled in the art can calculate the theoretical predicted values ​​of α-Al2O3 volume fraction under different combinations of process parameters based on this formula. Without conducting extensive exploratory experiments, it is possible to quickly determine whether a set of process conditions meets the requirement that the α-Al2O3 volume percentage is not less than 45%, thus providing clear numerical guidance for the optimization and online control of process parameters.

[0091] Example 10

[0092] In this embodiment, the content of α-Al2O3 in the ceramic layer satisfies the following relationship (application scenario and proof).

[0093] Experiments and data processing during the regression fitting phase:

[0094] The lower limit, median, and upper limit values ​​of three variables—nano titanium dioxide concentration (1-5 g / L), rare earth nitrate concentration (0.1-1.0 g / L), and treatment time (10-40 min)—were selected. An orthogonal experimental matrix containing 15 experimental points was constructed using Box-Behnken design or full factorial design, with each experimental point corresponding to a specific combination of parameters. All experiments were conducted under the condition that all other process parameters remained completely consistent, including matrix composition (10 parts Si, 3 parts Mg, balance Al), silicate concentration (10 g / L), sodium hexametaphosphate concentration (1 g / L), electrolyte temperature (27.5℃), positive voltage (550 V), negative voltage (150 V), frequency (500 Hz), and stirring flow rate (1 m / s), to ensure that the change in C value came only from the three independent variables. After each group of experiments, X-ray diffractometers were used to analyze the phase composition of the ceramic layer. Copper target Kα rays were used as the radiation source, with a scanning range of 10°-90°, a step size of 0.02°, and a scanning speed of 2° / min. After phase identification of the obtained diffraction patterns, quantitative phase analysis was performed using the Rietveld full-spectrum fitting method to obtain the measured value of the volume fraction C of α-Al2O3 in each group of samples.

[0095] After completing the measured C values ​​of 15 sets of experiments, the corresponding C (TiO2), C (RE), ln (t / t0) values ​​and the measured C values ​​of each set were substituted into the relational formula, and the least squares method was used to perform multiple linear regression fitting on K1, K2, and K3. During the fitting process, the value of C0 was determined by conducting an additional separate experiment without adding nano-titanium dioxide and rare earth nitrates, with a treatment time of 25 min (under the baseline conditions). The result was C0 = 28.5% (this value is independent of C0 as a constant term in the regression during the fitting process). The fitted model yielded a coefficient of determination R² = 0.96, indicating that the three independent variables combined could explain 96% of the total variation in the C value, demonstrating a good fit. The t-test p-values ​​for the three coefficients were p1 = 0.008, p2 = 0.003, and p3 = 0.001, all significantly lower than the 0.05 significance level, indicating that the concentrations of nano-titanium dioxide, rare earth nitrates, and treatment time all had statistically significant contributions to the α-Al₂O₃ volume fraction, and these contributions were not due to random factors. The normal probability plot of the regression residuals showed that the residual points were distributed along a straight line, and the p-value of the Shapiro-Wilk normality test was 0.21 (greater than 0.05), indicating that the residuals followed a normal distribution and the model was reasonably constructed.

[0096] Independent testing of confirmatory experiments:

[0097] Confirmatory experiments were conducted using six independent parameter combinations that were not involved in fitting the regression model. These combinations were: A (TiO2 1.5 g / L, RE 0.3 g / L, t=15 min), B (TiO2 2.5 g / L, RE 0.7 g / L, t=35 min), C (TiO2 4.0 g / L, RE 0.2 g / L, t=20 min), D (TiO2 4.5 g / L, RE 0.8 g / L, t=12 min), E (TiO2 2.0 g / L, RE 0.4 g / L, t=28 min), and F (TiO2 3.5 g / L, RE 0.7 g / L, t=28 min). (0.9 g / L, t=38 min); Substitute the parameters of each group into the relationship of the determined coefficients to calculate the predicted value of C. At the same time, implement the micro-arc oxidation treatment of each combination under the same conditions, and obtain the measured value of C using the same XRD test conditions and Rietveld quantitative method as in the regression stage.

[0098] The comparison results of predicted and measured values ​​for the six verification experiments are as follows: Combination A: predicted value 44.2%, measured value 45.0%, relative deviation 1.8%; Combination B: predicted value 55.6%, measured value 54.0%, relative deviation 2.9%; Combination C: predicted value 49.8%, measured value 48.5%, relative deviation 2.6%; Combination D: predicted value 47.1%, measured value 46.0%, relative deviation 2.3%; Combination E: predicted value 51.3%, measured value 52.0%, relative deviation 1.4%; Combination F: predicted value 57.8%, measured value 59.0%, relative deviation 2.1%. The absolute value of the relative deviation for all six verification experiments does not exceed 3%, which is far less than the acceptable 5% error limit in engineering, confirming the reliable predictive ability of this formula across the entire parameter range.

[0099] Specific verification under boundary and extreme conditions:

[0100] To verify the effectiveness of the relational expression at both ends of the parameter range and under extreme conditions, the following supplementary experiments were conducted: In the first group, the concentrations of nano-titanium dioxide and rare earth nitrate were both 0 (i.e., no additives were added), the treatment time was 25 min, and other conditions remained unchanged. The measured value of C was 28.3%, which deviated from the independently measured value of C0 of 28.5% by only 0.7%, thus verifying the model assumption that C regresses to C0 when the additive term in the relational expression is zero. The second group had a nano-titanium dioxide concentration of 1.0 g / L, a rare earth nitrate concentration of 0.1 g / L (both lower limits), and a treatment time of 10 min (lower limit). The predicted value C = 28.5 + 3.0 + 0.75 + 23.03 = 55.28%, and the measured value was 54.5%, with a relative deviation of 1.4%. The third group had a nano-titanium dioxide concentration of 5.0 g / L, a rare earth nitrate concentration of 1.0 g / L (both upper limits), and a treatment time of 40 min (upper limit). The predicted value C = 28.5 + 15.0 + 7.5 + 36.89 = 87.89%, and the measured value was 85.2%, with a relative deviation of 3.1%. The fourth group had a nano-titanium dioxide concentration of 0 (below the lower limit), a rare earth nitrate concentration of 0.1 g / L, and a rare earth nitrate concentration of 0.1 g / L (both lower limits). With a rare earth nitrate concentration of 0.55 g / L (intermediate value) and a treatment time of 30 min, the experimentally measured value of C was 49.2%. However, the effective application range of this formula for the concentration of nano-titanium dioxide is 1-5 g / L. When CTiO2=0 is input, it is an extrapolation case, and the predicted value C=28.5+4.125+34.01=66.64%, which deviates from the measured value of 49.2% by 35.4%, exceeding the acceptable range. This result clarifies the applicable boundary of the formula—the prediction is only effective when all variables are within their respective value ranges (nano-titanium dioxide concentration 1-5 g / L, rare earth nitrate concentration 0.1-1.0 g / L, treatment time 10-40 min). Extrapolation does not guarantee accuracy.

[0101] The statistical tests during the regression fitting phase (R²=0.96, p-values ​​for all coefficients less than 0.05, and residuals normally distributed), the average relative deviation of 2.2% (maximum deviation 2.9%) from six independent validation experiments, and the experimental evidence that the prediction deviation of parameters within the effective range was less than 3.5% in the boundary condition validation, confirm that the prediction error of this formula for the volume fraction of α-Al₂O₃ within the effective parameter range is less than 5%, meeting the accuracy requirements for engineering applications. Furthermore, the results of the fourth set of extreme validation experiments clarify that this formula is only applicable when all variables are within the specified range; it cannot be directly extrapolated when values ​​are outside the range. This complete regression modeling and validation experiment loop provides sufficient quantitative evidence and a clear definition of the applicable scope for the application of this formula in process design, online control, and parameter optimization.

[0102] It should be noted that the core application of this relationship is the quantitative design and dynamic control of micro-arc oxidation process parameters. In the development of traditional micro-arc oxidation processes, the actual content of α-Al2O3 in the ceramic layer under a certain set of process conditions can only be known afterward through phase analysis methods such as X-ray diffraction. However, the detection process requires destructive testing or sampling, which is both time-consuming and cannot provide real-time feedback online.

[0103] This formula provides another approach: by inputting three process variables that can be monitored in real time—the concentration of nano-titanium dioxide, the concentration of rare earth nitrates, and the processing time—the theoretical predicted value of the α-Al2O3 content under the current conditions can be calculated, thus enabling rapid assessment of the process status without interrupting the treatment process. In actual production, this formula can be used in conjunction with online monitoring equipment—when the concentration of additives in the electrolyte deviates from the set value due to consumption or evaporation, the operator can calculate the C value under the current parameters based on this formula and compare it with the target value (not less than 45%). If the predicted value is too low, the corresponding additives can be added in a timely manner or the processing time can be adjusted to ensure that each batch of products meets the α-phase content requirements.

[0104] In the new process development stage, this relationship can reduce the number of experiments to explore process conditions. Researchers only need to select a small number of experimental points within the parameter range to measure the actual C value and fit the coefficients. They can then use this relationship to predict the C value under other unexperimented parameter combinations, thereby quickly locking in the process window that meets the requirement of not less than 45%.

[0105] Furthermore, this relationship can also be embedded in the micro-arc oxidation automatic control system as the core algorithm module of model predictive control. When fluctuations in auxiliary parameters such as electrolyte temperature and conductivity are detected, the control system calculates the amount of additive to be added or the remaining processing time in real time based on this relationship, thereby realizing closed-loop control of α-Al2O3 content and batch-to-batch consistency management. It is especially suitable for continuous production lines of large-volume aluminum alloy frames, and can control the fluctuation of α phase content between batches within ±3%.

[0106] Example 11

[0107] S3 in this embodiment includes:

[0108] In step S31, the loose layer on the surface of the micro-arc oxidation ceramic layer is removed by grinding or belt polishing, with a removal thickness of 5-15μm, until a dense layer with a smooth surface and no visible micropores is exposed. Grinding can be done using a surface grinder with a silicon carbide or diamond grinding disc, while belt polishing is performed using a belt polisher with an appropriate grit size. The mechanical cutting action of the abrasive is used to remove the loose part at the top of the ceramic layer layer by layer. The removal thickness is controlled by measuring the total thickness of the ceramic layer with an eddy current thickness gauge before processing and setting the feed rate. During processing, the remaining thickness is periodically re-measured to ensure the accuracy of the removal amount. The purpose of this step is to remove the outer layer with a loose structure and low hardness, leaving only the inner layer with a dense structure, extremely low porosity, and good metallurgical bonding with the matrix, providing a uniform processing base surface for subsequent fine polishing.

[0109] In step S32, the ceramic layer after removing the loose layer undergoes fine polishing. Fine polishing uses diamond polishing paste with a particle size of W7-W5 or a fiber polishing wheel to achieve a surface roughness Ra ≤ 0.4μm. When using diamond polishing paste, the paste is applied to the surface of the ceramic layer and polished on a low-speed polishing machine using a felt or polyurethane polishing wheel. When using a fiber polishing wheel, the fiber wheel itself contains or is pre-impregnated with diamond micropowder, which generates a micro-cutting effect on the surface of the ceramic layer during rotational friction. During fine polishing, the processing area is kept sufficiently cooled to prevent thermal stress cracking. The purpose of this step is to eliminate the microscopic scratches and surface micropeaks remaining after grinding in step S31, reduce surface roughness, and reduce the number of open micropores remaining on the surface of the dense layer.

[0110] In step S33, the ceramic layer treated in step S32 undergoes ultrasonic cleaning and hot air drying. The cleaning solution for ultrasonic cleaning is deionized water, the cleaning time is 3-8 minutes, the drying temperature is 80-100℃, and the drying time is 10-20 minutes. The finely polished aluminum alloy frame substrate is immersed in an ultrasonic cleaning tank containing deionized water. The ultrasonic cavitation effect is used to peel off and disperse the diamond polishing paste residue, ceramic shavings, and abrasive fragments remaining in the micro-pits and micropores on the surface of the ceramic layer into the cleaning solution. After cleaning, the substrate is removed and placed in a hot air drying oven for drying. Hot air circulation accelerates the evaporation and removal of deionized water from the surface of the ceramic layer and the micropores. The purpose of this step is to thoroughly remove the grinding debris and polishing paste residue introduced by the fine polishing process and completely remove the moisture introduced during the cleaning process, so that the substrate can enter the subsequent sealing process in a dry and clean state. Through the sequential implementation of S31 to S33, the loose layer of the micro-arc oxidation ceramic layer is completely removed, the surface of the dense layer reaches a smooth and flat state, and the contaminants and moisture on the surface and in the pores are thoroughly removed, resulting in a high-quality aluminum alloy frame ceramic layer surface that can be directly sealed.

[0111] Example 12

[0112] This treatment method can be applied to aluminum alloy structural components in both mobile smart terminals and automotive equipment that require a combination of lightweight, high strength, and surface protection. In the mobile smart terminal field, the metal frames of smartphones, tablets, and laptops are a core application scenario. As terminal products develop towards thinner and lighter designs with higher screen-to-body ratios, aluminum alloy frames must withstand repeated handling, friction, and impacts during daily use, while also serving as radiating carriers for antenna signals and meeting radio frequency performance requirements. Traditional anodized films have limited hardness, and after long-term use, scratches, wear, and corrosion easily appear, affecting the product's appearance and lifespan. This treatment method generates a high-hardness ceramic layer with α-Al₂O₃ as the main crystalline phase in situ on the surface of the aluminum alloy frame. The hardness can reach more than 10 times that of traditional anodizing, effectively solving the problems of scratches and wear during daily use. Simultaneously, the ceramic layer itself possesses excellent insulation properties, preventing the metal frame from interfering with antenna signals. This treatment method further utilizes the synergistic effect of composite additives (nano-titanium dioxide and rare earth nitrates) and a dense layer retention process to ensure that the volume fraction of α-Al2O3 in the ceramic layer is not less than 45% and the surface roughness Ra≤0.4μm. While ensuring insulation performance, it significantly improves the wear resistance, corrosion resistance and scratch resistance of the middle frame, meeting the dual requirements of high-end mobile smart terminals for structural durability and appearance.

[0113] In the field of automotive equipment, aluminum alloy is a key material for achieving lightweighting in automobiles. This treatment method is applicable to components such as aluminum alloy battery pack shells, motor housings, aluminum alloy brake components, high-power LED headlight heat sinks, and in-vehicle display frames. The battery pack shells of new energy vehicles are subjected to long-term vibration, temperature changes, and humidity, requiring stringent requirements for wear resistance, corrosion resistance, and insulation performance. Aluminum alloy brake components need to address the issue of rust or adhesion between brake components when parked. High-power LED headlight aluminum alloy heat sinks need to combine heat dissipation efficiency and surface protection under high-temperature conditions.

[0114] The micro-arc oxidation ceramic layer formed by this treatment method can achieve a hardness of HV800-3000 and withstand salt spray tests exceeding 1000 hours. It provides high hardness, strong wear resistance, corrosion resistance, and insulation protection on the surface of aluminum alloy components. The ceramic layer is metallurgically bonded to the aluminum alloy substrate, resulting in strong adhesion and resistance to peeling, meeting the long-term reliability requirements of automotive components under complex operating conditions. Simultaneously, the porous structure of the ceramic layer increases the heat dissipation surface area and generates a chimney effect, enhancing heat convection and enabling the radiator to achieve both surface protection and heat dissipation performance. The ceramic layer prepared by this method possesses high hardness, strong wear resistance, corrosion resistance, high temperature resistance, and insulation properties, making it widely applicable to aluminum alloy components in new energy vehicles and automotive equipment fields that require both lightweight design and surface protection.

[0115] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0116] The above description is only used to illustrate the technical solution of the present invention and is not intended to limit it. Any other modifications or equivalent substitutions made by those skilled in the art to the technical solution of the present invention, as long as they do not depart from the spirit and scope of the technical solution of the present invention, should be covered within the scope of the claims of the present invention.

Claims

1. A method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame in mobile intelligent terminals, characterized in that, Includes the following steps: S1: The aluminum alloy frame substrate is pretreated, wherein the aluminum alloy contains 8-12 parts Si, 2-5 parts Mg, and the balance is Al and unavoidable impurities by weight. S2: The pretreated aluminum alloy frame substrate is placed in an electrolyte containing silicates and composite additives as the anode, and micro-arc oxidation is performed using a bipolar pulse power supply to form a ceramic layer that is metallurgically bonded to the substrate. The concentration of silicate in the electrolyte is 5-15 g / L; the composite additive is a mixture of nano-titanium dioxide and rare earth nitrates; the time, voltage, and frequency conditions of the micro-arc oxidation treatment are configured such that the volume percentage of α-Al2O3 in the ceramic layer is not less than 45%; S3: Remove at least part of the loose layer on the surface of the micro-arc oxidation ceramic layer, retain the dense layer, and make the dense layer serve as the outer surface of the aluminum alloy frame; S4: The aluminum alloy frame substrate with the micro-arc oxide ceramic layer formed thereon is subjected to a sealing treatment.

2. The micro-arc oxidation insulation and wear-resistant treatment method for the aluminum alloy frame of a mobile intelligent terminal according to claim 1, characterized in that, The preprocessing includes: S11: The aluminum alloy frame substrate is dewaxed using ultrasonic dewaxing. The temperature of the dewaxing solution is 60-80℃, and the treatment time is 5-20 minutes. S12: Degreasing treatment is performed on the substrate after S11 treatment using an alkaline degreasing solution at a temperature of 50-70℃ for 5-15 minutes. S13: Clean the substrate after S12 treatment by ultrasonic cleaning or spray cleaning with deionized water for 3-10 minutes.

3. The micro-arc oxidation insulation and wear-resistant treatment method for the aluminum alloy frame of a mobile intelligent terminal according to claim 1, characterized in that, The micro-arc oxidation treatment takes 10-40 minutes, and the electrolyte temperature is 15-40°C.

4. The micro-arc oxidation insulation and wear-resistant treatment method for the aluminum alloy frame of a mobile intelligent terminal according to claim 1, characterized in that, The concentration of the nano-titanium dioxide is 1-5 g / L, and the concentration of the rare earth nitrate is 0.1-1.0 g / L.

5. The micro-arc oxidation insulation and wear-resistant treatment method for the aluminum alloy frame of a mobile intelligent terminal according to claim 1, characterized in that, The electrolyte also contains 0.5-2 g / L of sodium hexametaphosphate dispersant, and the electrolyte is circulated and stirred during the micro-arc oxidation process. The flow rate of the circulation and stirring is 0.5-2 m / s, and the stirring direction is parallel to the substrate surface.

6. The micro-arc oxidation insulation and wear-resistant treatment method for aluminum alloy mid-frame of mobile intelligent terminal according to claim 1, characterized in that, The bipolar pulse power supply has a positive voltage of 400-750V, a negative voltage of 40-350V, and a frequency of 50Hz-2kHz.

7. The method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame of mobile intelligent terminal according to claim 1, characterized in that, The average particle size of the nano-titanium dioxide is 10-50 nm, and the rare earth nitrate is at least one of cerium nitrate or lanthanum nitrate.

8. The method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame of mobile intelligent terminal according to claim 1, characterized in that, The sealing process is one of high-temperature hydration sealing, organic resin sealing, or pulse electrodeposition sealing.

9. The method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame of mobile intelligent terminal according to claim 1, characterized in that, The thickness of the micro-arc oxidation ceramic layer is 20-50 μm.

10. The method for micro-arc oxidation insulation and wear-resistant treatment of aluminum alloy mid-frame of mobile intelligent terminal according to claim 1, characterized in that, S3 includes: S31: Remove the loose layer on the surface of the micro-arc oxidation ceramic layer by grinding or belt polishing, with a thickness of 5-15μm, until a dense layer with a smooth surface and no visible micropores is exposed. S32: The ceramic layer after removing the loose layer is subjected to fine polishing. The fine polishing is performed using diamond polishing paste or fiber polishing wheel with a particle size of W7-W5, so that the surface roughness Ra≤0.4μm. S33: The ceramic layer treated in S32 is subjected to ultrasonic cleaning and hot air drying to remove grinding debris remaining on the surface and in the pores. The cleaning solution for ultrasonic cleaning is deionized water, the cleaning time is 3-8 minutes, the drying temperature is 80-100℃, and the drying time is 10-20 minutes.