A method for micro-arc oxidation of magnesium alloy battery casing

By forming a dense Mg2SiO4/MgO ceramic structure on the surface of the magnesium alloy battery casing, the corrosion and insulation failure problems of the magnesium alloy battery casing in humid environments are solved, improving the corrosion resistance and insulation of the battery and extending its service life.

CN123108699APending Publication Date: 2026-11-17深圳市安美科化学技术有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610617133.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Magnesium alloy battery casings are prone to corrosion and insulation failure in humid environments, leading to short circuits. Existing technologies struggle to effectively address their corrosion resistance and insulation issues.

Method used

A dense Mg2SiO4/MgO ceramic structure is formed on the surface of a magnesium alloy battery casing using a micro-arc oxidation method. A dense oxide film is then formed using a gradient boost power supply and silicate sealing technology, which enhances corrosion resistance and insulation.

Benefits of technology

It improves the corrosion resistance and insulation resistance of magnesium alloy battery casings, extends battery life, and solves the problems of corrosion and insulation failure of magnesium alloy battery casings in humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108699A_ABST
    Figure CN123108699A_ABST
Patent Text Reader

Abstract

The application discloses a magnesium alloy battery shell micro-arc oxidation method, aiming at significantly improving its corrosion resistance, insulation and surface bonding strength, the process is carried out in an alkaline silicate electrolyte, by optimizing the electrolyte composition (containing Na2SiO3, KF and stabilizing additives) and electrical parameters (voltage, frequency, duty cycle), a dense and uniform ceramic oxide film is grown on the magnesium alloy surface in situ. The results show that: the obtained coating is mainly composed of MgO and Mg2SiO4 phases, the thickness can reach 20-40 microns, and has a typical porous structure (the porosity is significantly reduced after sealing treatment); the coating has high bonding strength with the substrate, the corrosion resistance time of neutral salt spray test (NSS) is more than 500 hours, the insulation resistance is greater than 100 MΩ, and the electrolyte erosion is effectively isolated. The process significantly improves the long-term reliability of the magnesium alloy battery shell under complex working conditions, and provides key technical support for the development of new energy automobile lightweight battery package.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery casing surface treatment technology, specifically a micro-arc oxidation method for magnesium alloy battery casings. Background Technology

[0002] Magnesium alloys are ideal materials for power battery casings due to their excellent lightweight properties, but their poor corrosion resistance limits their practical application. Magnesium alloys have a density only 2 / 3 that of aluminum alloys, significantly reducing battery weight. However, magnesium alloys are chemically reactive, easily corroded, and the resulting oxide film is porous and has poor insulation, making them highly susceptible to short circuits. Furthermore, magnesium alloys have a low potential, making them prone to galvanic corrosion and pitting corrosion in humid environments, leading to battery casing failure. Especially during battery charging and discharging, an insulating passivation film easily forms on the anode surface, accelerating battery corrosion.

[0003] To address this issue, we propose a micro-arc oxidation method for magnesium alloy battery casings to solve the problems of corrosion and insulation failure in humid and electrolyte environments. Summary of the Invention

[0004] The purpose of this invention is to provide a wear-resistant silver plating protective agent and its preparation method to solve the problems mentioned in the background art.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a micro-arc oxidation method for magnesium alloy battery casings, comprising the following steps:

[0006] S1: Pretreatment: The magnesium alloy battery casing is first polished step by step using 400#, 800#, 1200# and 2000# sandpaper, and then mechanically polished until the surface roughness Ra≤0.4μm;

[0007] S2: Degreasing: Immerse the battery casing in a solution of 30g / L NaOH, 20g / L Na2CO3, 20g / L Na3PO4, and ultrasonically clean it for 10 minutes at 60-70℃. After degreasing, rinse thoroughly with deionized water to ensure that there is no residual alkali or oil on the surface.

[0008] S3: Preparation of alkaline electrolyte: Weigh 10-15g / L Na2SiO3, 5-10g / L KF, and 1-3g / L KOH, add 3-5ml of sodium ethylenediaminetetraacetate and triethanolamine in a 1:1 ratio, add the above components to deionized water in sequence, stir until completely dissolved, mix evenly, and let stand for 10-15min for later use.

[0009] S4: Micro-arc oxidation treatment: The stainless steel plate is used as the cathode and the magnesium alloy battery casing is used as the anode. The mixture is placed in an alkaline silicate electrolyte and a stepped pulse boost power supply is applied.

[0010] S5: Water washing: Rinse the magnesium alloy battery casing formed by micro-arc oxidation in S4 with deionized water.

[0011] S6: Sealing treatment: Immerse the battery casing formed by micro-arc oxidation in a 0.5-2.0 g / L Na2SiO3 solution for 15-30 min at a temperature of 80-90℃.

[0012] Preferably, the alkaline silicate electrolyte is prepared with the following composition and concentration: sodium silicate (Na2SiO3) 10–20 g / L, potassium fluoride (KF) 5–10 g / L, sodium hydroxide (NaOH) or potassium hydroxide (KOH) 1–3 g / L, and a mixture of sodium ethylenediaminetetraacetate and triethanolamine 2–5 mL / L.

[0013] Preferred parameters for the bipolar pulse power supply in micro-arc oxidation are: positive voltage: 400–600V, negative voltage: 50–150V, frequency: 500–1000Hz, duty cycle: 20%–40%, and processing time: 20–40min.

[0014] Preferably, the process also includes post-treatment: sealing the micro-arc oxidized battery casing in hot water at a temperature of 80–95°C for 15–30 minutes.

[0015] Preferably, the organic complexing agent additive is a mixture of sodium ethylenediaminetetraacetate and triethanolamine (CT-3) at a concentration of 3–4 mL / L.

[0016] Preferably, the pulse power supply in step S4 adopts a gradient boost mode: the first stage 0–5 min: positive voltage 400–450V, negative voltage 50–80V; the second stage 5–20 min: positive voltage 500–550V, negative voltage 100–120V; the third stage 20–40 min: positive voltage 550–600V, negative voltage 120–150V.

[0017] Preferably, the thickness of the micro-arc oxidation coating is 20–40 μm, the phase composition includes MgO and Mg2SiO4, and the porosity is ≤8% (after sealing).

[0018] Preferably, 0.5–2 g / L sodium silicate is added as a sealing agent in the hot water sealing treatment.

[0019] Magnesium alloy battery casings prepared by micro-arc oxidation method have a neutral salt spray corrosion resistance time ≥500h; surface insulation resistance ≥100MΩ (500VDC); and coating-substrate bonding strength ≥50MPa.

[0020] The following performance tests were performed on the treated samples:

[0021] Coating thickness: Measured using an eddy current thickness gauge or metallographic method.

[0022] Porosity: Assessed by image analysis (SEM).

[0023] Neutral salt spray test: conducted according to GB / T10125 standard.

[0024] Insulation resistance: Measured using an insulation resistance tester (500VDC).

[0025] Bond strength: Tested using the scratch test.

[0026] Compared with the prior art, the beneficial effects of the present invention are:

[0027] (1) The three-layer dense 20-40μm Mg2SiO4 / MgO ceramic structure formed by the gradient voltage (400-600V) of the present invention effectively prevents the diffusion of Cl-, and its salt spray resistance can reach 500h, which solves the perforation problem caused by electrolyte penetration. Moreover, the gradient voltage makes the heat distribution uniform and eliminates film cracks (SEM test).

[0028] (2) The present invention uses silicate sealing technology (0.5-2.0g / LNa2SiO3) to compress the final porosity to ≤8% and reduce the corrosion current density to 3.2×10-7A / cm2 (electrochemical test).

[0029] (3) The insulation resistance of the magnesium alloy battery casing formed by the present invention is ≥100MΩ, which is 20 times more than that of bare magnesium alloy, exceeding the national requirement of 50MΩ for battery casing, thus eliminating the short circuit problem of the battery.

[0030] (4) The dense oxide film formed by the present invention has a coating adhesion of ≥50MPa (scratch test), ensuring that the battery does not peel off or fail during discharge.

[0031] In summary, this invention employs a stepped pulse boost power supply micro-arc oxidation method to form a dense oxide film on the surface of the magnesium alloy battery casing, enhancing the corrosion resistance of the magnesium alloy battery casing and solving the insulation failure problem of magnesium alloy batteries in humid environments. Moreover, the generated oxide film significantly reduces the reaction rate between the magnesium alloy casing and the lithium-ion battery, greatly improving the battery's lifespan. Attached Figure Description

[0032] Figure 1 This is a flowchart of the micro-arc oxidation method for the magnesium alloy battery casing of the present invention. Detailed Implementation

[0033] The following will clearly and completely describe exemplary embodiments of the present invention. Unless otherwise defined, the technical or scientific terms used in this invention should have the ordinary meaning understood by one of ordinary skill in the art. All embodiments described below use the AZ91D magnesium alloy battery casing.

[0034] Reference Figure 1 As shown, this invention provides a micro-arc oxidation method for magnesium alloy battery casings, the specific operation steps of which are as follows:

[0035] Example 1:

[0036] S1: Pretreatment: First, use 400#, 800#, 1200# and 2000# sandpaper to grind the magnesium alloy battery casing step by step, and finally perform mechanical polishing until the surface roughness Ra≤0.4μm;

[0037] S2: Degreasing: Immerse the battery casing in a solution of 30g / L NaOH, 20g / L Na2CO3, 20g / L Na3PO4, and ultrasonically clean it for 10 minutes at 60-70℃. After degreasing, rinse thoroughly with deionized water to ensure that there is no residual alkali and oil on the surface.

[0038] S3: Preparation of alkaline electrolyte: Weigh 15g / L Na2SiO3, 8g / L KF, and 2g / L KOH, add 3ml of sodium ethylenediaminetetraacetate and triethanolamine in a compound ratio, add the above components to deionized water in sequence, stir until completely dissolved, mix evenly, and let stand for 15min.

[0039] S4: Micro-arc oxidation treatment: A stainless steel plate is used as the cathode and a magnesium alloy battery casing is used as the anode. The battery is placed in an alkaline silicate electrolyte, and then a stepped pulse boost power supply is applied. The voltage is as follows: 0-5 min: positive voltage 430V, negative voltage 60V; 5-20 min: positive voltage 520V, negative voltage 110V; 20-40 min: positive voltage 580V, negative voltage 130V, frequency 800Hz, duty cycle 30%.

[0040] S5: Rinse the magnesium alloy battery casing formed by micro-arc oxidation in S4 with deionized water.

[0041] S6: Sealing treatment: Immerse the battery casing formed by micro-arc oxidation in a 2.0 g / L Na2SiO3 solution for 30 min at a temperature of 90 °C;

[0042] The coating thickness of the membrane measured in this example is 32 μm, the porosity is 5%, the insulation resistance is 135 MΩ, and the neutral salt spray test duration is 580 h. With optimized electrolyte ratio and precisely controlled gradient voltage parameters, a high-performance micro-arc oxidation ceramic coating was successfully prepared on the surface of the AZ91D magnesium alloy battery shell. Its performance is excellent and comprehensively surpasses the existing technology.

[0043] Example 2:

[0044] S1: Pretreatment: First, use 400#, 800#, 1200# and 2000# sandpaper to grind the magnesium alloy battery casing step by step, and finally perform mechanical polishing until the surface roughness Ra≤0.4μm;

[0045] S2: Degreasing: Immerse the battery casing in a solution of 30g / L NaOH, 20g / L Na2CO3, 20g / L Na3PO4, and ultrasonically clean it for 10 minutes at 60-70℃. After degreasing, rinse thoroughly with deionized water to ensure that there is no residual alkali and oil on the surface.

[0046] S3: Preparation of alkaline electrolyte: Weigh 10g / L Na2SiO3, 5g / L KF, and 1g / L KOH, add 3ml of sodium ethylenediaminetetraacetate and triethanolamine in a compound ratio, add the above components to deionized water in sequence, stir until completely dissolved, mix evenly, and let stand for 15min.

[0047] S4: Micro-arc oxidation treatment: A stainless steel plate is placed in an alkaline silicate electrolyte, with a magnesium alloy battery casing as the anode. Then, a stepped pulse boost power supply is applied: 0-5 min: positive voltage 400V, negative voltage 50V; 5-20 min: positive voltage 500V, negative voltage 100V; 20-40 min: positive voltage 600V, negative voltage 100V, frequency 800Hz, duty cycle 30%.

[0048] S5: Rinse the magnesium alloy battery casing formed by micro-arc oxidation in S4 with deionized water.

[0049] S6: Sealing treatment: Immerse the battery casing formed by micro-arc oxidation in a 0.5 g / L Na2SiO3 solution for 30 min at a temperature of 90 °C.

[0050] The membrane coating thickness measured in this example is 35 μm, porosity is 7%, insulation resistance is 108 MΩ, and neutral salt spray test duration is 500 h. It still meets the limits (≥500 h, ≥100 MΩ) at the lower limit of electrolyte concentration (Na2SiO3 10 g / L, CT-32 mL / L) and the upper limit of voltage (600 V), salt spray time (502 h) and insulation resistance (108 MΩ).

[0051] Example 3:

[0052] S1: Pretreatment: First, use 400#, 800#, 1200# and 2000# sandpaper to grind the magnesium alloy battery casing step by step, and finally perform mechanical polishing until the surface roughness Ra≤0.4μm.

[0053] S2: Degreasing: Immerse the battery casing in a solution of 30g / L NaOH, 20g / L Na2CO3, 20g / L Na3PO4, and ultrasonically clean it for 10 minutes at 60-70℃. After degreasing, rinse thoroughly with deionized water to ensure that there is no residual alkali or oil on the surface.

[0054] S3: Preparation of alkaline electrolyte: Weigh 8g / L Na2SiO3, 3g / L KF, and 2g / L KOH, add 2ml of sodium ethylenediaminetetraacetate and triethanolamine in a compound ratio, add the above components to deionized water in sequence, stir until completely dissolved, mix evenly, and let stand for 15min.

[0055] S4: Micro-arc oxidation treatment: A stainless steel plate is used as the cathode, and a magnesium alloy battery casing is used as the anode. The cells are immersed in an alkaline silicate electrolyte, and then a stepped pulse boost power supply is applied. From 0-5 min: positive voltage 420V, negative voltage 60V; from 5-20 min: positive voltage 540V, negative voltage 115V; from 20-40 min: positive voltage 590V, negative voltage 140V, frequency 800Hz, duty cycle 30%.

[0056] S5: Rinse the magnesium alloy battery casing formed by micro-arc oxidation in S4 with deionized water.

[0057] S6: Sealing treatment: Immerse the battery casing formed by micro-arc oxidation in deionized water (without sodium silicate) solution for 30 minutes at a temperature of 90℃.

[0058] The membrane coating thickness measured in this example is 24 μm, porosity is 10%, insulation resistance is 95 MΩ, and neutral salt spray test duration is 485 h. This demonstrates that at concentrations slightly below the lower limit, by adjusting electrical parameters, a coating with a certain protective capability (485 h of salt spray) can still be obtained at the lowest cost.

[0059] Table 1 Comparison of Film Coating Test Data

[0060] Example Coating thickness Porosity Insulation resistance neutral salt spray test duration Example 1 32μm 5% 135MΩ 580h Example 2 35μm 7% 108MΩ 500h Example 3 24μm 10% 95MΩ 485h

[0061] Comparative Example 1: With a constant forward voltage of 550V and other conditions the same as in Example 1, the prepared battery casing underwent a neutral salt spray test for 280 hours, and cracks appeared in the coating.

[0062] This comparative example illustrates that using constant pressure under high pressure conditions can lead to coating damage due to excessive energy.

[0063] Comparative Example 2: No mixture of sodium ethylenediaminetetraacetate and triethanolamine was added to the electrolyte preparation. All other conditions were the same as in Example 1. The prepared battery casing underwent a neutral salt spray test for 380 hours, and the coating adhesion strength was 18 MPa.

[0064] This comparative example demonstrates that the absence of the sodium ethylenediaminetetraacetate and triethanolamine mixture leads to a significant decrease in coating density and substrate adhesion.

[0065] In summary, gradient voltage control achieves high performance and a defect-free coating, while the additive mixture of sodium ethylenediaminetetraacetate and triethanolamine inhibits crack formation, and silicate sealing significantly reduces the coating's porosity. This invention, through a triple technological innovation of gradient voltage control, composite electrolyte, and silicate sealing, comprehensively surpasses existing technologies in corrosion resistance, insulation, adhesion, and environmental friendliness. The resulting micro-arc oxidation film layer for magnesium alloy battery casings effectively solves the problems of corrosion resistance and insulation failure in humid environments, demonstrating promising development prospects.

[0066] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method for micro-arc oxidation of magnesium alloy battery casing, characterized in that, Includes the following steps: S1: Pretreatment: The magnesium alloy battery casing is first polished step by step using 400#, 800#, 1200# and 2000# sandpaper, and then mechanically polished until the surface roughness Ra≤0.4μm; S2: Degreasing: Immerse the battery casing in a solution of 30g / L NaOH, 20g / L Na2CO3, 20g / L Na3PO4, and ultrasonically clean it for 10 minutes at 60-70℃. After degreasing, rinse thoroughly with deionized water to ensure that there is no residual alkali or oil on the surface. S3: Preparation of alkaline electrolyte: Weigh 10-15g / L Na2SiO3, 5-10g / L KF, and 1-3g / L KOH, add 3-5ml of sodium ethylenediaminetetraacetate and triethanolamine in a 1:1 ratio, add the above components to deionized water in sequence, stir until completely dissolved, mix evenly, and let stand for 10-15min for later use. S4: Micro-arc oxidation treatment: The stainless steel plate is used as the cathode and the magnesium alloy battery casing is used as the anode. The mixture is placed in an alkaline silicate electrolyte and a stepped pulse boost power supply is applied. S5: Water washing: Rinse the magnesium alloy battery casing formed by micro-arc oxidation in S4 with deionized water. S6: Sealing treatment: Immerse the battery casing formed by micro-arc oxidation in a 0.5-2.0 g / L Na2SiO3 solution for 15-30 min at a temperature of 80-90℃.

2. The micro-arc oxidation method for magnesium alloy battery casing according to claim 1, characterized in that: Prepare an alkaline silicate electrolyte with the following composition and concentration: Na₂SiO₃ 10–20 g / L, KF 5–10 g / L, NaOH or KOH 1–3 g / L, and a mixture of sodium ethylenediaminetetraacetate and triethanolamine 2–5 mL / L.

3. The micro-arc oxidation method for magnesium alloy battery casing according to claim 1, characterized in that: Bipolar pulse power supply parameter control for micro-arc oxidation: positive voltage: 400–600V, negative voltage: 50–150V, frequency: 500–1000Hz, duty cycle: 20%–40%, processing time: 20–40min.

4. The micro-arc oxidation method for magnesium alloy battery casing according to claim 1, characterized in that: Post-treatment: The battery casing after micro-arc oxidation is sealed in hot water at a temperature of 80–95℃ for 15–30 minutes.

5. The micro-arc oxidation method for magnesium alloy battery casing according to claim 1, characterized in that: The mixture of sodium ethylenediaminetetraacetate and triethanolamine is an organic complexing agent additive with a concentration of 3–4 mL / L.

6. The micro-arc oxidation method for magnesium alloy battery casing according to claim 3, characterized in that: The pulse power supply in step S4 adopts a gradient boost mode: the first stage 0–5 min: positive voltage 400–450V, negative voltage 50–80V; Second stage 5–20 min: positive voltage 500–550V, negative voltage 100–120V; Third stage 20–40 min: positive voltage 550–600V, negative voltage 120–150V.

7. The micro-arc oxidation method for magnesium alloy battery casing according to claim 1, characterized in that: The thickness of the micro-arc oxidation coating is 20–40 μm, and the phase composition includes MgO and Mg2SiO4. After sealing, the porosity is ≤8%.

8. The micro-arc oxidation method for magnesium alloy battery casing according to claim 4, characterized in that: 0.5–2 g / L sodium silicate is added as a sealing agent in the hot water sealing process.

9. The micro-arc oxidation method for magnesium alloy battery casing according to claim 1, characterized in that: The following performance tests were performed on the treated samples: Coating thickness: Measured using an eddy current thickness gauge or metallographic method; Porosity: assessed using image analysis; Neutral salt spray test: Performed according to standard; Insulation resistance: Measured using an insulation resistance tester; Bond strength: Tested using the scratch test.

10. The magnesium alloy battery casing prepared by the method according to any one of claims 1–9, characterized in that: Resistance to neutral salt spray corrosion ≥500h; surface insulation resistance ≥100MΩ; coating-substrate bonding strength ≥50MPa.