A method for removing oxide scale from steel using plasma electrolytic machining based on overpotential
By employing an overpotential-based plasma electrolytic machining method, combined with high-pressure gas film self-sustaining discharge and dynamic cavitation stripping technology, the problem of removing dense oxide scale from high-temperature alloys and steels has been solved, achieving complete oxide scale removal and surface finishing, thus improving production efficiency and environmental friendliness.
Patent Information
- Application Number
- CN202611447022.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional processes are difficult to completely remove the dense oxide scale from high-temperature alloys and steel, and also have problems such as damage to the substrate and poor environmental performance.
An overpotential-based plasma electrolytic processing method is adopted. Through the coupling mechanism of high-pressure gas film self-sustaining discharge, interface lattice activation, dynamic cavitation stripping and substrate passivation leveling, the oxide scale is removed by using an overpotential voltage of 380VDC~400VDC. After removal, the voltage is reduced to the conventional potential for surface finishing.
It achieves complete removal of oxide scale and integrated surface finishing, avoiding damage to the substrate and reducing environmental risks and waste liquid treatment costs.
Smart Images

Figure CN123108712A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal surface treatment technology, and relates to a method for removing oxide scale from steel based on overpotential plasma electrolytic processing, specifically involving the process of removing oxide scale from the surface of steel after thermal oxidation. Background Technology
[0002] After forging, rolling, and heat treatment, metals such as steel and high-temperature alloys will form a multi-layered dense composite heavy oxide scale on their surface: the surface of steel is mainly composed of a thick layer of iron oxide interspersed with grain boundary oxide layer, while high-temperature alloys form a nickel, chromium, and aluminum composite spinel-type hard oxide layer. This type of oxide scale has high hardness, dense structure, and tight adhesion to the substrate, making it difficult to completely remove by conventional treatment methods.
[0003] Traditional mechanical grinding processes rely on high-speed impact of abrasives to physically peel off oxide scale. This process can only remove loose surface oxide scale and cannot peel off embedded oxide layers and spinel hard oxide scale within grain boundaries. At the same time, mechanical impact can cause plastic deformation of the surface of steel and high-temperature alloys, forming a work-hardened layer. It can also easily cause defects such as embedded abrasive particles, edge collapse, and incomplete treatment of dead corners in the internal cavity, which can damage the surface integrity and dimensional accuracy of components.
[0004] Pickling relies on the strong corrosive effect of strong acid to indiscriminately dissolve oxide scale and metal matrix. It has extremely low efficiency in removing dense spinel oxide scale from high-temperature alloys, requiring high concentration of strong acid and long-term immersion. During the process, steel is prone to hydrogen embrittlement failure, and high-temperature alloys are prone to pitting corrosion and element segregation loss. In addition, it generates a large amount of acid mist, heavy metal hazardous waste liquid, and has extremely poor environmental protection and process safety, making it unsuitable for high-end precision alloy components.
[0005] Traditional electrochemical polishing relies on the anodic dissolution effect of a viscous liquid film, which is only suitable for smoothing slightly oxidized and clean metal surfaces. When faced with a thick layer of heavy oxide scale after heat treatment, the dense oxide layer will block the current and block the electrochemical reaction, resulting in descaling failure and a mottled oxide layer remaining on the surface. It is completely unsuitable for processing raw components after heat treatment.
[0006] Plasma electropolishing differs from traditional single physical or chemical processes. Conventional plasma electropolishing technology operates at voltages within the stable breakdown range of the gas sheath, typically 260V~320V, to maintain a continuous and stable vapor layer. Relying on plasma micro-discharge, cavitation impact, and selective electrochemical dissolution, oxide scale protrusions are preferentially peeled off, resulting in a low substrate removal rate and primarily polishing and leveling. Under conventional voltages, plasma electropolishing technology is insufficient for removing thick, dense, continuously thermally processed oxide scale. When the oxide scale is too thick, the gas sheath struggles to stably break down the oxide film, leading to a low removal rate and localized residues, often requiring pre-peeling / acid pickling. Furthermore, conventional plasma electropolishing technology suffers from long processing times and low production efficiency; when the oxide scale has defects such as pores or peeling, it is difficult to peel off oxide scale in recessed areas. Summary of the Invention
[0007] To address four major industry pain points—the difficulty in removing hard spinel oxide scale from high-temperature alloys, the easy damage during descaling of high-strength steel, the incomplete descaling of complex structures, and the poor environmental friendliness of traditional processes—this invention provides a method for removing steel oxide scale using plasma electrolytic machining based on overpotential. This method involves no substrate loss and no surface modification defects throughout the entire process, simultaneously completing oxide scale removal and surface finishing, significantly shortening the process flow and making it suitable for the stable industrial production of batches of precision metal components. Furthermore, this invention uses an environmentally friendly electrolyte solution free of strong acids, reducing the emissions of highly polluting waste gas and wastewater from traditional pickling processes, minimizing harm to the natural environment and human production and activities, while also reducing the cost of waste gas and wastewater purification.
[0008] This invention provides a method for removing oxide scale from steel using plasma electrolytic machining based on overpotential, wherein the workpiece is used as the anode and the electrolytic bath is used as the cathode; the process flow is as follows: parts mounting – electrolyte heating – power supply connection – overpotential polishing – conventional potential polishing – deionized water rinsing – inspection; Specifically, the steps include the following: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: Inject the prepared (NH4)2SO4 solution with a mass concentration of 3%~3.5% into the polishing tank, start the tank heating and temperature control system, raise the temperature of the electrolyte and maintain it stably within the process set temperature range (80℃~95℃), and ensure the electrolyte temperature is uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power on: Immerse the mounted parts into the electrolyte, confirming that the immersion depth is 120mm~130mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode, establish a stable electrolytic electric field, and provide electrical energy for the subsequent electrochemical reaction; S4 Overpotential Polishing: The power supply voltage is linearly increased to the set value of 380VDC~400VDC at a rate of 100VDC / s and held for 100s-150s. The high overpotential electrolysis is used to pre-treat the surface of the parts. Through strong electrolysis, the oxide scale, rust, welding slag and other surface impurities on the surface of the parts are quickly peeled off and dissolved, completing the removal of loose oxide scale and providing a clean base for uniform oxide scale removal. S5 Conventional Potential Polishing: The voltage is linearly reduced from the overpotential value to the range of 290VDC~310VDC at a rate of 100VDC / s and maintained for 450s-500s. Stable parameters and electrolyte environment are maintained to form a uniform electrolyte plasma discharge layer on the surface of the part. The high energy effect of the plasma in the micro-area is used to selectively dissolve and polish the micro protrusions on the surface of the part, gradually reducing the surface roughness and achieving mirror-level smoothness and uniform surface morphology. S6 Deionized Water Cleaning: After fine polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and place them in flowing deionized water for thorough rinsing to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S7 Inspection: Conduct quality inspection on the cleaned and dried parts to check for rust, pitting, and over-polishing defects, thus completing the entire processing process.
[0009] After the above oxide scale removal process, the surface of the obtained parts has a uniform bright metallic color and no oxide scale residue.
[0010] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention uses overpotential plasma electropolishing technology with an initial voltage of 380VDC~400VDC, which is higher than the conventional working window (>320VDC, entering the overpotential range). It utilizes the violent fluctuation of the gas sheath to significantly improve the breakdown strength, and takes advantage of the stronger characteristics of plasma shock waves and micro-area thermal shock to achieve oxide scale removal. After the thicker oxide scale on the surface is basically removed, the working voltage is reduced to the conventional voltage to remove the thinner, denser oxide scale on the surface.
[0011] This invention proposes a method for removing steel oxide scale based on overpotential plasma electrolytic processing. The electrolyte used is an environmentally friendly salt solution, without the use of acid-containing solutions, resulting in no waste acid generation. This method is environmentally friendly, reduces waste liquid treatment costs, and improves the working environment for pickling. Attached Figure Description
[0012] Figure 1 Schematic diagram of the oxide scale structure on the surface of steel; Figure 2 The macroscopic morphology of GH4169 alloy before and after removal of oxide scale by conventional plasma electropolishing in Comparative Example 1 is shown; where (a) is the macroscopic morphology before removal of oxide scale of GH4169 alloy, and (b) is the macroscopic morphology after removal of oxide scale of GH4169 alloy. Figure 3 The macroscopic morphology of GH907 alloy before and after removal of oxide scale by plasma electrolytic polishing in Comparative Example 2 is shown in (a) and (b) respectively. Figure 4 The macroscopic morphology of GH4169 alloy before and after removal of oxide scale by plasma electrolytic polishing in Comparative Example 3 is shown in (a) and (b) respectively. Figure 5 The images show the macroscopic morphology of the martensitic stainless steel before and after the removal of the oxide scale in Example 1; where (a) is the macroscopic morphology of the martensitic stainless steel before the removal of the oxide scale, and (b) is the macroscopic morphology of the martensitic stainless steel after the removal of the oxide scale. Figure 6 The images show the macroscopic morphology of 304 stainless steel before and after oxide scale removal in Example 2; where (a) is the macroscopic morphology of 304 stainless steel before oxide scale removal, and (b) is the macroscopic morphology of 304 stainless steel after oxide scale removal. Figure 7 The image shows the macroscopic morphology of GH4169 before oxide scale removal in Example 3. Figure 8 The image shows the macroscopic morphology of GH4169 after oxide scale removal in Example 3. Detailed Implementation
[0013] The steel targeted by this invention is a material that has undergone hot working or hot oxidation, and its surface oxide scale structure is as follows: Figure 1 As shown, due to the high oxidation temperature, the oxide scale is composed of multiple layers of oxides. The outermost layer is a loose oxide scale, which is mainly formed by the high thickness of the oxide scale and the inconsistent thermal expansion with the matrix, resulting in cracking and loosening, thus adhering to the outermost layer. The middle layer is a spinel mixed oxide layer, and the bottom layer is a dense oxide layer. The middle and bottom layers have high density and strong bonding with the matrix, making them difficult to remove during the polishing process.
[0014] Plasma electropolishing achieves efficient oxide scale removal through a four-in-one coupling mechanism of high-pressure gas film self-sustaining discharge, interface lattice activation, dynamic cavitation exfoliation, and substrate passivation and leveling, which differs from traditional single physical bombardment or chemical dissolution mechanisms. The workpiece is immersed in a low-temperature environmentally friendly electrolyte as the anode. Under the action of a critical high-voltage electric field, the electrolyte on the workpiece surface vaporizes instantaneously, forming a uniformly coated insulating vapor film. After the electric field continuously breaks down the gas film, a global micro-plasma discharge field is generated, and high-energy plasma microbeams preferentially act on the surface insulating oxide scale.
[0015] To address the dense lattice structure of heavy oxide coatings, this invention utilizes an overpotential voltage of 380VDC~400VDC to continuously bombard the lattice defects and grain boundary regions of the oxide layer with high-energy plasma particles. This breaks the stable lattice bond energy of spinel oxides and thick iron oxide layers, dissolving the interlayer bonding forces and the intercalation structure with the metal matrix, causing the intact heavy oxide coating to develop dense microcracks and gradually loosen. Simultaneously, the instantaneous micro-regional high temperature and weak electrochemical activation effect at the discharge interface further weaken the stability of the oxide coating. Combined with the trace cavitation shear force generated by the periodic collapse of the gas film, the oxide coating is peeled off entirely in a layered manner, rather than dissolved layer by layer.
[0016] Once the oxide scale is completely removed and the pure metal substrate is exposed, the voltage is reduced to a normal potential. At this point, the electric field distribution on the workpiece surface tends to be uniform, and the plasma action mechanism automatically switches to a micro-selective leveling mode. This mode preferentially ablates the micro-protrusions on the substrate surface and simultaneously forms a transient passivation film on the leveled substrate surface. This effectively avoids problems such as excessive corrosion of steel, chromium depletion in high-temperature alloy substrates, and element loss, achieving integrated processing of complete removal of heavy oxide scale and non-damaging finishing of the substrate.
[0017] This invention provides a method for removing oxide scale from steel using plasma electrolytic machining based on overpotential, where the workpiece serves as the anode and the electrolytic bath as the cathode. The process flow is as follows: part mounting – electrolyte heating – power connection – overpotential polishing – conventional potential polishing – deionized water rinsing – inspection; Specifically, the steps include the following: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: Inject the prepared (NH4)2SO4 solution with a mass concentration of 3%~3.5% into the polishing tank, start the tank heating and temperature control system, raise the temperature of the electrolyte and maintain it stably within the process set temperature range (80℃~95℃), and ensure the electrolyte temperature is uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power on: Immerse the mounted parts into the electrolyte, confirming that the immersion depth is 120mm~130mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode, establish a stable electrolytic electric field, and provide electrical energy for the subsequent electrochemical reaction; S4 Overpotential Polishing: The power supply voltage is linearly increased to the set value of 380VDC~400VDC at a rate of 100VDC / s and held for 100s-150s. The high overpotential electrolysis is used to pre-treat the surface of the parts. Through strong electrolysis, the oxide scale, rust, welding slag and other surface impurities on the surface of the parts are quickly peeled off and dissolved, completing the removal of loose oxide scale and providing a clean base for uniform oxide scale removal. S5 Conventional Potential Polishing: The voltage is linearly reduced from the overpotential value to the range of 290VDC~310VDC at a rate of 100VDC / s and maintained for 450s-500s. Stable parameters and electrolyte environment are maintained to form a uniform electrolyte plasma discharge layer on the surface of the part. The high energy effect of the plasma in the micro-area is used to selectively dissolve and polish the micro protrusions on the surface of the part, gradually reducing the surface roughness and achieving mirror-level smoothness and uniform surface morphology. S6 Deionized Water Cleaning: After fine polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and place them in flowing deionized water for thorough rinsing to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S7 Inspection: Conduct quality inspection on the cleaned and dried parts to check for rust, pitting, and over-polishing defects, thus completing the entire processing process.
[0018] The present invention will be further described below with reference to embodiments and comparative examples.
[0019] Example 1: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: The prepared (NH4)2SO4 solution with a mass concentration of 3% is injected into the polishing tank. The tank heating and temperature control system is started to raise the temperature of the electrolyte and maintain it stably within the process set temperature range of 85℃. The electrolyte temperature is ensured to be uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power On: Immerse the mounted parts into the electrolyte, confirm that the immersion depth is 120mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode, establish a stable electrolytic electric field, and provide electrical energy for the subsequent electrochemical reaction. S4 Overpotential Polishing: The power supply voltage is linearly increased to the set value of 380VDC at a rate of 100VDC / s and held for 150s. The high overpotential electrolysis is used to pre-treat the surface of the parts. Through strong electrolysis, the oxide scale, rust, welding slag and other surface impurities on the surface of the parts are quickly peeled off and dissolved, and the loose oxide scale is removed, providing a clean base for uniform oxide scale removal. S5 Conventional Potential Polishing: The voltage is linearly reduced from the overpotential value to 310VDC at a rate of 100VDC / s and held for 500s to maintain stable parameters and electrolyte environment, forming a uniform electrolyte plasma discharge layer on the surface of the part. Utilizing the high-energy effect of the plasma in the micro-area, the micro-protrusions on the surface of the part are selectively dissolved and polished, gradually reducing the surface roughness and achieving mirror-level smoothness and uniform surface morphology. S6 Deionized Water Cleaning: After fine polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and place them in flowing deionized water for thorough rinsing to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S7 Inspection: Perform quality inspection on the cleaned and dried parts, checking for rust, pitting, and over-polishing defects to ensure the entire processing cycle is complete. The method described in this embodiment is used to remove the oxide scale from martensitic stainless steel after thermal oxidation, such as... Figure 5 As shown, before removal, the surface of martensitic stainless steel is covered with grayish-brown oxide scale from thermal oxidation. After overpotential electrolyte plasma processing, the surface oxide scale is completely removed, and the surface is bright and mirror-like.
[0020] Example 2: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: Inject the prepared (NH4)2SO4 solution with a mass concentration of 3.5% into the polishing tank, start the tank heating and temperature control system, raise the temperature of the electrolyte and maintain it stably within the process set temperature range of 80℃, and ensure the electrolyte temperature is uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power on: Immerse the mounted parts into the electrolyte, confirm that the immersion depth is 120mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode, establish a stable electrolytic electric field, and provide electrical energy for the subsequent electrochemical reaction; S4 Overpotential Polishing: The power supply voltage is linearly increased to the set value of 390VDC at a rate of 100VDC / s and held for 130s. The high overpotential electrolysis is used to pre-treat the surface of the parts. Through strong electrolysis, the oxide scale, rust, welding slag and other surface impurities on the surface of the parts are quickly peeled off and dissolved, and the loose oxide scale is removed, providing a clean base for uniform oxide scale removal. S5 Conventional Potential Polishing: The voltage is linearly reduced from the overpotential value to 300VDC at a rate of 100VDC / s and held for 470s to maintain stable parameters and electrolyte environment, forming a uniform electrolyte plasma discharge layer on the surface of the part. Utilizing the high-energy effect of the plasma in the micro-area, the micro-protrusions on the surface of the part are selectively dissolved and polished, gradually reducing the surface roughness and achieving mirror-level smoothness and uniform surface morphology. S6 Deionized Water Cleaning: After fine polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and place them in flowing deionized water for thorough rinsing to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S7 Inspection: Conduct quality inspection on the cleaned and dried parts to check for rust, pitting, and over-polishing defects, thus completing the entire processing process.
[0021] The method described in this embodiment is used to remove the oxide scale from 304 stainless steel after hot oxidation, such as... Figure 6 As shown, before removal, the surface of 304 stainless steel is covered with black oxide scale after thermal oxidation. The oxide scale is densely distributed. After overpotential electrolyte plasma processing, the surface oxide scale is completely removed, and the surface is bright and mirror-like.
[0022] Example 3: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: The prepared (NH4)2SO4 solution with a mass concentration of 3% is injected into the polishing tank. The tank heating and temperature control system is started to raise the temperature of the electrolyte and maintain it stably within the process set temperature range of 95℃. The electrolyte temperature is ensured to be uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power On: Immerse the mounted parts in the electrolyte to a depth of 130mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode to establish a stable electrolytic electric field and provide power for the subsequent electrochemical reaction; S4 Overpotential Polishing: The power supply voltage is linearly increased to the set value of 400VDC at a rate of 100VDC / s and held for 100s. The high overpotential electrolysis is used to pre-treat the surface of the parts. The strong electrolysis reaction quickly peels off and dissolves the oxide scale, rust, welding slag and other surface impurities on the surface of the parts, completing the removal of loose oxide scale and providing a clean base for uniform oxide scale removal. S5 Conventional Potential Polishing: The voltage is linearly reduced from the overpotential value to 290VDC at a rate of 100VDC / s and held for 450s to maintain stable parameters and electrolyte environment, forming a uniform electrolyte plasma discharge layer on the surface of the part. Utilizing the high-energy effect of the plasma in the micro-area, the micro-protrusions on the surface of the part are selectively dissolved and polished, gradually reducing the surface roughness and achieving mirror-level smoothness and uniform surface morphology. S6 Deionized Water Cleaning: After fine polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and place them in flowing deionized water for thorough rinsing to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S7 Inspection: Conduct quality inspection on the cleaned and dried parts to check for rust, pitting, and over-polishing defects, thus completing the entire processing process.
[0023] The method described in this embodiment is used to remove the oxide scale from GH4169 high-temperature alloy after thermal oxidation, such as... Figure 7 As shown, before removal, the surface of GH4169 high-temperature alloy was yellowish-brown, which was an oxide film formed after thermal oxidation. Figure 8 As shown, after overpotential electrolyte plasma processing, the oxide scale of GH4169 high-temperature alloy is completely removed, and the surface is bright and mirror-like.
[0024] Comparative Example 1: This comparative example demonstrates the polishing effect of conventional plasma electropolishing technology without applied overpotential on GH4169 alloy, specifically including the following steps: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: The prepared 3% (NH4)2SO4 solution is injected into the polishing tank. The tank heating and temperature control system is started to raise the temperature of the electrolyte and maintain it stably at the process set temperature of 85℃. The electrolyte temperature is ensured to be uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power on: Immerse the mounted parts into the electrolyte, confirm that the immersion depth is 120mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode, establish a stable electrolytic electric field, and provide electrical energy for the subsequent electrochemical reaction; S4 conventional potentiometric polishing: The voltage is increased to 310VDC and held for 500s to maintain stable parameters and electrolyte environment, forming a uniform electrolyte plasma discharge layer on the surface of the part. The high energy of the plasma in micro-areas is used to preferentially dissolve and remove surface protrusions, gradually reducing surface roughness. S5 Deionized Water Cleaning: After polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and rinse them thoroughly in flowing deionized water to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S6 Inspection: Conduct quality inspection on the cleaned and dried parts, checking their appearance.
[0025] The above methods are used to remove the oxide scale from GH4169 alloy after hot oxidation, such as... Figure 2 As shown, before removal, the surface of the GH4169 sample was covered with loose oxide scale after thermal oxidation. After conventional plasma electrolytic processing, the surface oxide scale disappeared, but there was still an incomplete oxide film on the sample surface. Since the oxide scale was not completely removed, conventional polishing methods could not be selected.
[0026] Comparative Example 2: This comparative example demonstrates the polishing effect of plasma electropolishing technology, which applies an overpotential exceeding the voltage range of 380VDC~400VDC, on GH907 alloy.
[0027] Specifically, the steps include the following: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: The prepared (NH4)2SO4 solution with a mass concentration of 3.5% is injected into the polishing tank. The tank heating and temperature control system is started to raise the temperature of the electrolyte and maintain it stably within the process set temperature range of 85℃. The electrolyte temperature is ensured to be uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power on: Immerse the mounted parts into the electrolyte, confirm that the immersion depth is 120mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode, establish a stable electrolytic electric field, and provide electrical energy for the subsequent electrochemical reaction; S4 Overpotential Polishing: The power supply voltage is linearly increased to the set value of 410VDC at a rate of 100VDC / s and held for 100s. The high overpotential electrolysis is used to pre-treat the surface of the parts. The strong electrolysis reaction quickly peels off and dissolves the oxide scale, rust, welding slag and other surface impurities on the surface of the parts, so as to achieve the removal of loose oxide scale. S5 Conventional Potential Polishing: The voltage is linearly reduced from the overpotential value to 310VDC at a rate of 100VDC / s and held for 500s to maintain stable parameters and electrolyte environment, forming a uniform electrolyte plasma discharge layer on the surface of the part. The high energy effect of the plasma in the micro-area is used to selectively dissolve and polish the micro protrusions on the surface of the part, gradually reducing the surface roughness. S6 Deionized Water Cleaning: After fine polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and place them in flowing deionized water for thorough rinsing to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S7 Inspection: Conduct quality inspection on the cleaned and dried parts, check their appearance, and complete the entire processing process.
[0028] The above methods are used to remove the oxide scale from GH907 alloy after hot oxidation, such as... Figure 3 As shown, before removal, the surface of the GH907 sample was covered with a black oxide scale from thermal oxidation. Polishing was performed according to the above process parameters, with an overpotential voltage of 410VDC applied, higher than the overpotential range of 380VDC~400VDC. It can be seen that after plasma electrolytic processing, the oxide scale on the sample surface disappeared, but grooves caused by over-polishing were visible on the sample surface, indicating that this processing parameter caused some damage to the substrate; therefore, this parameter should not be selected.
[0029] Comparative Example 3: This comparative example demonstrates the polishing effect of plasma electropolishing technology on GH4169 alloy when an overpotential is applied below the voltage range of 380VDC~400VDC.
[0030] Specifically, the steps include the following: S1 Parts Hanging: Based on the material, size and structural characteristics of the parts to be processed, select appropriate conductive tooling hangers to securely clamp and suspend the parts, ensuring good contact between the parts and the hangers and smooth electrical conduction. At the same time, ensure that the processing surfaces of the parts are unobstructed and do not come into contact with each other, so as to prepare for subsequent immersion in electrolyte and uniform charging. S2 Electrolyte Heating: Inject the prepared (NH4)2SO4 solution with a mass concentration of 3.5% into the polishing tank, start the tank heating and temperature control system, raise the temperature of the electrolyte and maintain it stably within the process set temperature range of 90℃, and ensure the electrolyte temperature is uniform by circulating and stirring to eliminate local temperature differences and meet the temperature conditions for plasma reaction. S3 Power on: Immerse the mounted parts into the electrolyte, confirm that the immersion depth is 120mm, turn on the power of the polishing equipment, connect the parts to the anode and the tank to the cathode, establish a stable electrolytic electric field, and provide electrical energy for the subsequent electrochemical reaction; S4 Overpotential Polishing: The power supply voltage is linearly increased to the set value of 360VDC at a rate of 100VDC / s and held for 100s. The surface of the part is pretreated by high overpotential electrolysis. S5 conventional potential polishing: The voltage is linearly reduced from the overpotential value to 310VDC at a rate of 100VDC / s and held for 450s to maintain stable parameters and electrolyte environment, forming a uniform electrolyte plasma discharge layer on the surface of the part to remove the surface oxide scale. S6 Deionized Water Cleaning: After fine polishing, disconnect the power supply, quickly remove the parts from the electrolyte, and place them in flowing deionized water for thorough rinsing to completely remove residual electrolyte from the surface, gaps, and holes of the parts, preventing residual electrolyte from corroding the workpiece surface and ensuring that the surface is clean and free of dirt. S7 Inspection: Conduct quality inspection on the cleaned and dried parts, checking their appearance.
[0031] The above methods are used to remove the oxide scale from GH4169 alloy after hot oxidation, such as... Figure 4 As shown, before removal, the surface of the GH4169 sample was covered with loose oxide scale after thermal oxidation. Polishing was performed according to the above process parameters, and an overpotential voltage of 360VDC was applied, which is lower than the overpotential range of 380VDC~400VDC. It can be seen that after plasma electrolytic processing, the loose oxide scale on the sample surface disappeared, but oxide scale still existed on the sample surface, indicating that this set of parameters could not completely eliminate the oxide scale generated after thermal oxidation.
Claims
1. A method for removing oxide scale from steel using plasma electrolytic machining based on overpotential, characterized in that, First, apply an overpotential voltage of 380VDC~400VDC to polish the parts, then use a conventional potential voltage of 290VDC~310VDC to finely polish the parts. The process includes parts mounting, electrolyte heating, power connection, overpotential polishing, conventional potential polishing, deionized water cleaning, and inspection.
2. The method for removing steel oxide scale by plasma electrolytic machining based on overpotential according to claim 1, characterized in that, The process flow includes the following steps: S1 Parts Hanging: Select conductive tooling hangers according to the material, size and structural characteristics of the parts to be processed, and securely clamp and suspend the parts to ensure that there is smooth electrical conductivity between the parts and the hangers, and that the processing surfaces of the parts are unobstructed and do not come into contact with each other. S2 Electrolyte Heating: Inject the prepared electrolyte into the polishing tank, start the tank heating and temperature control system to raise the temperature of the electrolyte and maintain it stably within the process set temperature range; S3 Power On: Immerse the assembled parts in the electrolyte, turn on the power to the polishing equipment, connect the parts to the anode and the tank to the cathode to establish an electrolytic electric field; S4 Overpotential Polishing: Linearly increase the power supply voltage to the overpotential range and hold for 100s-150s; S5 Conventional Potential Polishing: The voltage is linearly reduced from the overpotential range to the conventional range and held for 450s-500s; S6 Deionized Water Cleaning: After fine polishing, deionized water is used for cleaning to remove residual electrolyte from the parts; S7 Inspection: Inspect the parts after cleaning and drying.
3. The method for removing steel oxide scale by plasma electrolytic machining based on overpotential according to claim 1, characterized in that, In S2, the electrolyte is a (NH4)2SO4 solution with a mass concentration of 3% to 3.5%, and the process temperature range is set to 80℃ to 95℃.
4. The method for removing steel oxide scale by plasma electrolytic machining based on overpotential according to claim 1, characterized in that, In S3, the depth to which the component is immersed in the electrolyte is 120mm~130mm.
5. The method for removing steel oxide scale by plasma electrolytic machining based on overpotential according to claim 1, characterized in that, In S4, the voltage increases linearly at a rate of 100VDC / s.
6. The method for removing oxide scale from steel using plasma electrolytic machining based on overpotential as described in claim 1, characterized in that, In S5, the voltage decreases linearly at a rate of 100VDC / s.
7. The method for removing steel oxide scale by plasma electrolytic machining based on overpotential according to claim 1, characterized in that, In S6, the deionized water cleaning process is as follows: after polishing, the power is cut off, the parts are removed from the electrolyte, and rinsed in flowing deionized water to thoroughly remove residual electrolyte from the surface, gaps, and holes of the parts, ensuring that the surface is clean and free of dirt.
8. The method for removing steel oxide scale by plasma electrolytic machining based on overpotential according to claim 1, characterized in that, In S7, the inspection process involves inspecting the appearance quality of the cleaned and dried parts to ensure that there is no rust, no pitting, and no over-polishing defects.