A flexible cross-linked silicone-embedded integral molding process for melamine decals
By using slow-release inhibitors, silane activating solutions, and gradient temperature control modification processes, the problems of delamination, bleeding, and tearing in the integrated molding of melamine paper and silicone were solved, achieving high-strength interfacial bonding and smooth finished product appearance, which is suitable for mass production of inlaid printed silicone products.
Patent Information
- Application Number
- CN202611292393.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
The existing melamine transfer paper and silicone one-piece molding process cannot simultaneously ensure construction stability, interface adhesion and finished product appearance smoothness, resulting in problems such as delamination, ink bleeding and transfer paper tearing.
By employing a sustained-release inhibitor inclusion system, a silane-activated interface bridging modification liquid, a gradient temperature-controlled modification process, and a paper cutting allowance compensation scheme, a flexible cross-linked transition layer is constructed through steps such as modification liquid preparation, paper pretreatment, and co-vulcanization molding, thereby achieving molecular-level fusion between the paper and silicone.
It achieves seamless, non-delaminating, non-bulging, and non-tearing embedding of melamine decals and silicone, improving interface adhesion strength and finished product smoothness. It is suitable for mass production and reduces raw material costs and production cycle.
Smart Images

Figure REF-OBJ-1787536050578-000001 
Figure REF-OBJ-1787536050578-000002
Abstract
Description
Technical Field
[0001] This invention relates to the field of heterogeneous material composite molding technology, specifically to a flexible cross-linked silicone-embedded integral molding process for melamine decals. Background Technology
[0002] Current silicone inlay printing methods mostly use expensive PET transfer films and special release films to transfer patterns, resulting in high raw material procurement costs and long customization cycles for printing decals. If melamine printing decals are directly placed into a mold and co-cured with liquid silicone, ink bleeding and paper carbonization problems will occur during the high-temperature molding stage. Furthermore, there is no chemical bond between the melamine printing decal and the silicone interface, making it extremely easy for the entire delaminated material to peel off after curing. The industry commonly uses ordinary silicone oil to single-sided impregnate the printing decal, which only forms a physical isolation film without intermolecular cross-linking. After curing, 100% interface peeling occurs, and the printing adhesion does not meet mass production standards at all.
[0003] Conventional hydrosilicone modified systems, when directly mixed, lack inhibitors, leading to rapid hydrosilylation at room temperature and premature gelation and structuring of the system. This results in an extremely short coating application window, hindering continuous mass production. Furthermore, existing modified formulations significantly increase crosslinking density, resulting in a hard and brittle modified layer after curing. Melamine transfer paper fibers become brittle due to heat-induced dehydration, and while silicone vulcanization exhibits approximately 1.03% shrinkage, transfer paper shows almost no shrinkage. This difference in shrinkage creates significant internal stress, leading to common defects after molding, such as transfer paper tearing, surface bulging and unevenness, and overall warping. Traditional modification baking often employs a single high-temperature baking process, causing rapid dehydration and carbonization of the paper surface, further exacerbating the paper's brittleness. Moreover, the crosslinking groups are completely deactivated after curing, lacking stress buffering capacity and making it impossible to compensate for the shrinkage difference through hot pressing, rendering the defects unrepairable.
[0004] Therefore, developing a flexible cross-linking embedding process that enables seamless, non-delaminating, non-bulging, and tear-free integral molding of melamine decals and silicone is a technical challenge that urgently needs to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to provide a flexible cross-linked silicone-embedded integral molding process for melamine decals, solving the following technical problems: The existing flexible cross-linking embedding process that integrates melamine decals with silicone still cannot simultaneously address the issues of construction stability, interfacial bonding strength, and the smoothness of the finished product.
[0006] The objective of this invention can be achieved through the following technical solutions: A flexible cross-linked silicone-embedded integral molding process for melamine decals includes the following steps: S1: Cut the melamine decal paper according to the finished size, leaving a fixed positive allowance of 1.0%-1.1%. Then clean it with anhydrous ethanol, pre-bake it at 55℃ for 5 minutes, and cool it to obtain the pre-treated melamine decal paper. S2: Immerse the pretreated melamine decal completely in the modification solution for 5-8 seconds, then remove it at a uniform speed of 1-2 mm / s, or evenly coat both sides of the pretreated melamine decal with a modification solution of 15-20 μm thickness, then drain the liquid vertically and blow away the accumulated liquid with low pressure, then let it stand at room temperature of 15-35℃ for 2-3 minutes, and finally treat it at 75℃ for 10-12 minutes. After cooling, the modified melamine decal is obtained. S3: The modified melamine decal is flattened and pre-placed in the cavity of a silicone mold without an external release agent. Liquid addition-type silicone is injected into the mold and co-cured at 165-170℃ in one step to obtain silicone with embedded melamine printing. The modified liquid is prepared from vinyl-terminated silicone oil, silane activating liquid, sustained-release inhibitor, isopropanol, hydrogen-containing silicone oil, and platinum catalyst.
[0007] Preferably, the modified liquid is prepared as follows: Add silane activating solution and slow-release inhibitor to the stirred vinyl silicone oil and stir for 3-5 min. Then add isopropanol 1 and vacuum extract for 10-15 min at 35-40℃ and -0.06--0.07MPa. Then add isopropanol 2 and stir for 2 min. After cooling to 15-20℃, add hydrogen-containing silicone oil and stir for 3 min. Before use, add platinum catalyst and stir for 4 min. Finally, let stand for 5-7 min to degas and obtain the modified solution.
[0008] Preferably, the mass ratio of the terminal vinyl silicone oil, silane activating liquid, sustained-release inhibitor, isopropanol 1, isopropanol 2, and hydrogen-containing silicone oil is 100:12:12:20:35-45:3.8-4.2.
[0009] Preferably, the effective platinum content in the embedded melamine printing silicone is 10-15 ppm by total mass.
[0010] Preferably, the method for preparing the sustained-release inhibitor is as follows: A1: Add β-cyclodextrin to deionized water and stir at 60°C for 20-30 min. Then add acetylenecyclohexanol dropwise and stir at 60°C for 3 h. Then cool to 4°C and let stand at 4°C for 12 h. Then filter, wash the filter cake, dry and grind to obtain the inclusion complex powder. A2: Add deionized water to isopropanol and sonicate for 10 min. Then add silane coupling agent KH-560 and adjust the pH to 4.3-4.7. Stir at 50-55℃ for 40-50 min, cool to 30℃ and add compound powder and sonicate for 10 min. Then stir at 45℃ for 3 h to obtain sustained-release inhibitor.
[0011] Preferably, the mass ratio of deionized water, β-cyclodextrin, and acetylenecyclohexanol in A1 is 100-120: 11.35-13.62g: 1.24-1.49.
[0012] Preferably, the mass ratio of isopropanol, deionized water, silane coupling agent KH-560, and compound powder in A2 is 8-9:0.3:0.5:2.2.
[0013] Preferably, the preparation method of the silane activation solution is as follows: Add silane coupling agent KH-560 and deionized water to isopropanol and adjust the pH to 4.5-5.0. Then, stir and hydrolyze at 25°C for 30-40 minutes to obtain silane activated solution.
[0014] Preferably, the ratio of isopropanol, silane coupling agent KH-560, and deionized water is 10-12:1.8:0.3-0.5.
[0015] The beneficial effects of this invention are: This invention provides a flexible cross-linking and silicone-embedded integral molding process for melamine transfer paper. Through the synergistic combination of a slow-release inhibitor inclusion system, a silane-activated interface bridging modifier, a gradient temperature-controlled modification process, and a transfer paper cutting allowance compensation scheme, it specifically addresses industry pain points of traditional printing processes, such as easy delamination and peeling, ink bleeding, transfer paper tearing, product bulging and warping, rapid gelation of the modifier at room temperature, and short application window. This achieves seamless, delamination-free, bulging-free, and tear-free integral molding of melamine transfer paper and silicone, while also ensuring mass production stability, high-strength interface adhesion, and a smooth finished product appearance. Specific beneficial effects are as follows: (I) This invention employs a sustained-release inhibitor system constructed by encapsulating acetylenic cyclohexanol with β-cyclodextrin, replacing the direct addition of free acetylenic alcohol inhibitors. The cyclodextrin cavity enables controlled sustained release of acetylenic cyclohexanol, stably complexing the platinum catalyst at room temperature, inhibiting premature initiation of hydrosilylation, significantly extending the coating application window of the modified liquid, and meeting the requirements of continuous mass production. During the high-temperature co-sulfurization stage, the inclusion complex dissociates, the inhibitor release effect disappears, and the hydrosilylation reaction proceeds normally and fully. Compared to directly adding free acetylenic cyclohexanol, this avoids incomplete cross-linking caused by excessively high instantaneous inhibitor concentration, while also eliminating interfacial cross-linking differences caused by uneven local inhibition, ensuring the formation of a continuous, flexible cross-linking transition layer in the modified coating, eliminating interfacial gaps between the silicone matrix and melamine transfer paper, and avoiding interfacial peeling defects from the reaction source.
[0016] (II) The present invention utilizes a compound silane activating liquid and a modified liquid system, relying on the silane coupling agent KH-560 to act as a molecular bridge. Silane hydrolysis generates silanol groups, which condense with the hydroxyl groups on the surface of melamine transfer paper fibers to form covalent bonds. The epoxy groups at the other end participate in a hydrosilylation reaction, forming chemical bonds with liquid silicone. This completely overcomes the technical bottleneck of traditional silicone oils, which rely solely on physical isolation, lack molecular cross-linking, and require 100% peeling after vulcanization. It achieves molecular-level fusion of the transfer paper, transitional modified layer, and silicone matrix. After molding, the interfacial peel strength is significantly improved. After prolonged boiling at 100℃ and thousands of repeated bending fatigue tests, there is no printing peeling, whitening, or ink bleeding, greatly extending the service life of inlaid printed silicone products.
[0017] (III) This invention establishes a gradient temperature-controlled modification process, employing a segmented treatment mode of low-temperature pre-baking, room-temperature static leveling, and moderate curing at 75°C, abandoning the traditional single high-temperature baking process. The gentle heating curve avoids rapid dehydration and carbonization of melamine transfer paper fibers and paper embrittlement; the modified coating retains some active vinyl groups, forming a flexible and elastic transition layer with stress buffering capacity. When the silicone vulcanization produces approximately 1.03% curing shrinkage, the flexible transition layer can buffer the internal stress between the silicone and the non-shrink transfer paper, alleviate interface stress concentration, and effectively suppress appearance defects such as transfer paper tearing, product bulging, and uneven warping during the molding process.
[0018] (iv) This invention sets a 1.0%-1.1% positive fixed allowance for the cutting of melamine decals, precisely matching the shrinkage difference during silicone vulcanization, and compensating for the tensile stress caused by molding shrinkage at the dimensional level. Combined with a standardized coating process of modified liquid immersion coating / thin brushing, uniform speed lifting, and low-pressure purging of accumulated liquid, it ensures uniform modified film thickness on the decal surface, avoiding uneven local coating thickness that causes differences in crosslinking degree and unbalanced stress distribution; the modified decal with the coated side facing the silicone feed side is pre-positioned, allowing for more thorough melt wetting during high-temperature vulcanization, further improving the uniformity of interface bonding, and eliminating the risk of local delamination throughout the entire area.
[0019] (V) The modified liquid adopts a staged addition of isopropanol combined with a vacuum gradient extraction process to achieve precise control of the solvent system. In the early stage, vacuum extraction removes excess low-boiling-point solvent from the system, preventing rapid solvent evaporation during the wet film stage that could cause pinholes and craters in the coating. Subsequent addition of isopropanol adjusts the viscosity of the modified liquid, ensuring the fluidity and uniformity of the film layer during dip coating and brush coating. The entire process eliminates the need for expensive PET transfer film and special release film, saving on the decal transfer process, resulting in lower raw material costs. Decals do not require customized transfer versions, shortening the delivery cycle. The process is compatible with conventional liquid silicone molding production lines, requiring no equipment modification and allowing for direct large-scale implementation. It is widely applicable to the production of various embedded printed silicone daily necessities, gifts, and kitchenware products.
[0020] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Detailed Implementation
[0021] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. The embodiments described below are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0022] Example 1: A flexible cross-linked silicone-embedded integral molding process for melamine decals is as follows: S1: Add 11.35g of β-cyclodextrin to 100mL of deionized water and stir at 60℃ for 20min. Then add 1.24g of ethynylcyclohexanol and stir at 60℃ for 3h to encapsulate the mixture. Then cool to 4℃ and let stand at 4℃ for 12h. Then filter and wash the filter cake with 10mL of deionized water at 1℃. Finally, vacuum dry at 45℃ for 18h and grind to obtain the inclusion compound powder. S2: Add 0.3g of deionized water to 9g of isopropanol and sonicate for 10min. Then add 0.5g of silane coupling agent KH-560 and adjust the pH to 4.3 with food-grade glacial acetic acid. Stir at 50℃ for 40min, cool to 30℃ and add 2.2g of compound powder and sonicate for 10min. Then stir at 45℃ for 3h and cool to obtain the sustained-release inhibitor. S3: Add 1.8g of silane coupling agent KH-560 and 0.3g of deionized water to 10g of isopropanol, and adjust the pH to 4.5 with food-grade glacial acetic acid. Then stir and hydrolyze at 25℃ for 30-40 minutes to obtain silane activated solution. S4: Add 12g of silane activating solution and 12g of slow-release inhibitor to 100g of vinyl-terminated silicone oil (viscosity 500-1000mPa·s, vinyl content 0.8wt%-1.2wt%) stirred at 300r / min and stir for 3min. Then add 20g of isopropanol and vacuum extract at 35℃ and -0.06MPa for 10min. Then add 35g of isopropanol and stir for 2min. After cooling to 15℃, add 3.8g of hydrogen-containing silicone oil and stir at 200r / min for 3min. Before use, add platinum catalyst (the effective platinum content in the final embedded melamine printing silicone system is 10ppm) and stir for 4min. Finally, let stand for 5min to degas and obtain the modified solution. S5: For the melamine decal paper, reserve a fixed positive allowance of 1.0% according to the finished size, then spray and clean it with anhydrous ethanol on both sides to remove dust, grease and demolding residue from the paper. Then, pre-bake it at 55℃ for 5 minutes and cool it to room temperature to obtain the pretreated melamine decal paper. S6: Immerse the pretreated melamine decal completely in the modification solution for 5 seconds, then remove it at a uniform speed of 1 mm / s (or evenly coat both sides of the pretreated melamine decal with a 15 μm thick modification solution, resulting in a dry film thickness of 5 μm), then drain vertically for 30 seconds, and use a dust-free air gun to blow away any accumulated liquid from the edges and textures to ensure a uniform film layer without floating oil. Then, let it stand in a dust-free environment at 15°C for 2 minutes, and finally treat it at 75°C for 10 minutes. After naturally cooling to room temperature, the modified melamine decal is obtained. S7: The modified melamine decal is flattened and pre-placed in the cavity of a silicone mold without an external release agent. Liquid addition-type silicone is injected into the mold and co-cured at 165°C in one step. The uncrosslinked coating is used to melt and wet the silicone matrix at high temperature, and platinum addition co-crosslinking occurs simultaneously to achieve "molecular-level fusion" and obtain the embedded melamine printing silicone.
[0023] Example 2: A flexible cross-linked silicone-embedded integral molding process for melamine decals is as follows: S1: Add 12.48g of β-cyclodextrin to 110mL of deionized water and stir at 60℃ for 25min. Then add 1.36g of ethynylcyclohexanol and stir at 60℃ for 3h to encapsulate the mixture. Then cool to 4℃ and let stand at 4℃ for 12h. Then filter and wash the filter cake with 11mL of deionized water at 3℃. Finally, vacuum dry at 45℃ for 19h and grind to obtain the inclusion compound powder. S2: Add 0.3g of deionized water to 8.5g of isopropanol and sonicate for 10min. Then add 0.5g of silane coupling agent KH-560 and adjust the pH to 4.5 with food-grade glacial acetic acid. Stir at 53℃ for 45min, cool to 30℃ and add 2.2g of compound powder and sonicate for 10min. Then stir at 45℃ for 3h and cool to obtain the sustained-release inhibitor. S3: Add 1.8g of silane coupling agent KH-560 and 0.4g of deionized water to 11g of isopropanol, and adjust the pH to 4.7 with food-grade glacial acetic acid. Then, stir and hydrolyze at 25℃ for 35min to obtain silane activated solution. S4: Add 12g of silane activating solution and 11.5g of slow-release inhibitor to 100g of vinyl-terminated silicone oil (viscosity 500-1000mPa·s, vinyl content 0.8wt%-1.2wt%) stirred at 300r / min and stir for 4min. Then add 20g of isopropanol and vacuum extract at 38℃ and -0.065MPa for 13min. Then add 40g of isopropanol and stir for 2min. After cooling to 18℃, add 4g of hydrogen-containing silicone oil and stir at 200r / min for 3min. Before use, add platinum catalyst (the effective platinum content in the final embedded melamine printing silicone system is 12ppm) and stir for 4min. Finally, let stand for 6min to degas and obtain the modified solution. S5: For the melamine decal paper, reserve a fixed positive allowance of 1.05% according to the finished size. Then, spray and clean it with anhydrous ethanol on both sides to remove dust, grease and demolding residue from the paper. Then, pre-bake it at 55℃ for 5 minutes and cool it to room temperature to obtain the pretreated melamine decal paper. S6: Immerse the pretreated melamine decal completely in the modification solution for 7 seconds, then remove it at a uniform speed of 1.5 mm / s (or evenly coat both sides of the pretreated melamine decal with a 17 μm thick modification solution, resulting in a dry film thickness of 7 μm), then drain vertically for 30 seconds, and use a dust-free air gun to blow away any accumulated liquid from the edges and textures to ensure a uniform film layer without floating oil. Then, let it stand in a dust-free environment at 25°C for 2.5 minutes, and finally treat it at 75°C for 11 minutes. After naturally cooling to room temperature, the modified melamine decal is obtained. S7: The modified melamine decal is flattened and pre-placed in the cavity of a silicone mold without an external release agent. Liquid addition-type silicone is injected into the mold and co-cured at 168°C in one step. The uncrosslinked coating is used to melt and wet the silicone matrix at high temperature, and platinum addition co-crosslinking occurs simultaneously to achieve "molecular-level fusion" and obtain melamine-embedded printing silicone.
[0024] Example 3: A flexible cross-linked silicone-embedded integral molding process for melamine decals is as follows: S1: Add 13.62g of β-cyclodextrin to 120mL of deionized water and stir at 60℃ for 30min. Then add 1.49g of ethynylcyclohexanol and stir at 60℃ for 3h to encapsulate the mixture. Then cool to 4℃ and let stand at 4℃ for 12h. Then filter and wash the filter cake with 12mL of deionized water at 5℃. Finally, vacuum dry at 45℃ for 20h and grind to obtain the inclusion complex powder. S2: Add 0.3g of deionized water to 8g of isopropanol and sonicate for 10min. Then add 0.5g of silane coupling agent KH-560 and adjust the pH to 4.7 with food-grade glacial acetic acid. Stir at 55℃ for 50min, cool to 30℃ and add 2.2g of compound powder and sonicate for 10min. Then stir at 45℃ for 3h. After cooling, add isopropanol to a total of 12g to obtain the sustained-release inhibitor. S3: Add 1.8g of silane coupling agent KH-560 and 0.5g of deionized water to 12g of isopropanol, and adjust the pH to 5.0 with food-grade glacial acetic acid. Then, stir and hydrolyze at 25℃ for 40min to obtain silane activated solution. S4: Add 12g of silane activating solution and 11g of slow-release inhibitor to 100g of vinyl-terminated silicone oil (viscosity 500-1000mPa·s, vinyl content 0.8wt%-1.2wt%) stirred at 300r / min and stir for 5min. Then add 20g of isopropanol and vacuum extract at 40℃ and -0.07MPa for 15min. Then add 45g of isopropanol and stir for 2min. After cooling to 20℃, add 4.2g of hydrogen-containing silicone oil and stir at 200r / min for 3min. Before use, add platinum catalyst (the effective platinum content in the final embedded melamine printing silicone system is 15ppm) and stir for 4min. Finally, let stand for 7min to degas and obtain the modified solution. S5: For the melamine decal paper, reserve a fixed positive allowance of 1.1% according to the finished size, then spray and clean it with anhydrous ethanol on both sides to remove dust, grease and demolding residue from the paper. Then, pre-bake it at 55℃ for 5 minutes and cool it to room temperature to obtain the pretreated melamine decal paper. S6: Immerse the pretreated melamine decal completely in the modification solution for 8 seconds, then remove it at a uniform speed of 2 mm / s (or evenly coat both sides of the pretreated melamine decal with a 20 μm thick modification solution, resulting in a dry film thickness of 8 μm), then drain vertically for 30 seconds, and use a dust-free air gun to blow away any accumulated liquid from the edges and textures to ensure a uniform film layer without floating oil. Then, let it stand in a dust-free environment at 35°C for 3 minutes, and finally treat it at 75°C for 12 minutes. After naturally cooling to room temperature, the modified melamine decal is obtained. S7: The modified melamine decal is flattened and pre-placed in the cavity of a silicone mold without an external release agent. Liquid addition-type silicone is injected into the mold and co-cured at 170°C in one step. The uncrosslinked coating is used to melt and wet the silicone matrix at high temperature, and platinum addition co-crosslinking occurs simultaneously to achieve "molecular-level fusion" and obtain the embedded melamine printing silicone.
[0025] Comparative Example 1: Compared with Example 1, this comparative example only replaces the "2.2g inclusion compound powder" added in the S2 preparation process with "2.2g acetylenecyclohexanol". All other steps and parameters are the same, and will not be repeated in this comparative example. Finally, the silicone for melamine printing is obtained.
[0026] Comparative Example 2: Compared with Example 2, this comparative example only did not add "12g silane activating liquid" in the S4 preparation process. All other steps and parameters were the same, and will not be repeated here. Finally, the silicone for melamine printing was obtained.
[0027] Comparative Example 3: Compared with Example 1, this comparative example only did not add "0.5g silane coupling agent KH-560" in the S2 preparation process. All other steps and parameters were the same, and will not be repeated here. The final product was silicone for melamine printing.
[0028] Comparative Example 4: Compared with Example 1, this comparative example only replaces "leaving a 1.0% fixed positive allowance for the melamine decal according to the finished size" in the S5 preparation process with "cutting the melamine decal directly according to the finished size without leaving a positive shrinkage allowance". All other steps and parameters are the same, and will not be repeated in this comparative example. Finally, the embedded melamine printing silicone is obtained.
[0029] Comparative Example 5: Compared with Example 1, this comparative example only replaces the step in the S4 preparation process of "then add 20g of isopropanol and vacuum extract at 35°C and -0.06MPa for 10 min, then add 35g of isopropanol and stir for 2 min" with "then add 55g of isopropanol and stir at 35°C for 2 min". All other steps and parameters are the same, and will not be repeated in this comparative example. Finally, the silicone for melamine printing is obtained.
[0030] Comparative Example 6: Compared with Example 1, this comparative example only replaces "add platinum catalyst (final effective platinum content 10 ppm) and stir for 4 min before use" in the S4 preparation process with "add platinum catalyst (final effective platinum content 20 ppm) and stir for 4 min before use". All other steps and parameters are the same, and will not be repeated in this comparative example. Finally, the silicone for melamine printing is obtained.
[0031] Performance testing: Inspection of appearance and structure: A flat cross-section was prepared by cryogenic freezing and brittle fracture. The layered structure of the cross-section was observed under a metallographic microscope at 100x magnification, and the presence of gaps between the three layers (silicone matrix, flexible cross-linked transition layer, and melamine transfer paper) was recorded. The embedded melamine transfer silicone was then placed freely on a grade 0 standard marble platform, and a full-area inspection was performed under natural light at a 45° oblique angle and a 10x magnifying glass. The presence of bulges and dents was recorded, and the front and back sides and the cross-section of the transfer paper were observed for cracks and tears. The test results are shown in Table 1.
[0032] Determination of interfacial adhesion: In accordance with GB / T 7122-2025 standard, a standard strip specimen embedded in the mold was prepared, and a local peeling start point was pre-made along the thickness direction. Then, the floating roller method was used for 180° peeling, with a tensile speed of 50 mm / min. The average peeling force at the interface (kN / m) was recorded. The test results are shown in Table 2.
[0033] Determination of water boiling resistance: The silicone embedded in melamine printing was immersed in 100℃ deionized water for 120 minutes, then removed and dried at room temperature for 30 minutes. The appearance was then observed to see if there was peeling, whitening, or bleeding. The test results are shown in Table 2.
[0034] Determination of bending fatigue resistance: A rubber bending fatigue testing machine was used. The sample width was 25 mm and the bending radius was 2 mm. The sample was bent 1000 times at a bending frequency of 60 times / min. After 1000 times, the appearance was observed to see if there was any peeling or tearing. The test results are shown in Table 2.
[0035] Table 1: Appearance and structural inspection results of Examples 1-3 and Comparative Examples 1-6
[0036] Table 2: Performance test results of Examples 1-3 and Comparative Examples 1-6
[0037] Data Analysis: As can be seen from the performance test data in Tables 1 and 2, the embedded melamine printing silicone prepared in this embodiment of the invention has no gaps at the three-layer interface, and the finished product has no bulging, dents, or tearing of the printing paper; the interfacial peel strength can reach 5.5-6.0 kN / m; after boiling in water for 120 minutes, there was no peeling, whitening, or bleeding; the printing remained intact after 1000 bending fatigue tests, simultaneously achieving excellent interfacial bonding strength, appearance smoothness, and long-term use stability, with all indicators being superior to all comparative examples. Each comparative example, which only changed the core components, auxiliary agent system, or key process parameters, all produced varying degrees of defects and deterioration, as detailed below: In Comparative Example 1, the sustained-release inhibitor inclusion complex powder was replaced with free acetylenecyclohexanol. Compared with Example 1, local micro-gaps appeared at the interface, the finished product showed slight bulging, and the decal paper cracked. The peel strength decreased to 3.3 kN / m, and the paper turned slightly white after boiling. After bending fatigue, local peeling and tearing occurred. This may be because free acetylenecyclohexanol has no sustained-release regulation ability, the inhibitor in the modified liquid is unevenly distributed, the cross-linking reaction in some areas is hindered, and the continuity of the flexible transition layer is destroyed. Insufficient local cross-linking density leads to a decrease in stress buffering capacity, and the internal stress of vulcanization directly acts on the decal paper interface, inducing micro-gaps and paper cracks. The number of chemical bonds at the interface is reduced, and water vapor can easily penetrate the interface, resulting in a significant decrease in water resistance and bending resistance.
[0038] Comparative Example 2 differed from Example 1 only in that "12g of silane activating solution" was not added during the preparation of the modified solution; all other steps and parameters remained the same. Compared to Example 1, local micro-gaps appeared in the sample cross-section, the finished product showed slight bulging and indentation, and a small number of micro-cracks appeared in the decal. The interfacial peel strength decreased to 4.1 kN / m, the water-resistant test sample showed slight whitening with local slight bleeding, and the bending fatigue test showed localized printing peeling and micro-tear defects. This may be because the silane activating solution contains fully hydrolyzed and activated silanol groups, which act as an interfacial bridging medium. One end can condense with the hydroxyl groups of the melamine decal fibers, while the other end participates in hydrosilylation and crosslinking with the silica matrix, constructing a continuous chemically bonded transition layer. After removing the silane activating solution, there was no effective covalent bond between the modified coating and the melamine decal; they were only physically bonded by intermolecular forces, resulting in a significant reduction in interfacial bonding strength. When silicone vulcanization generates shrinkage stress, the stress concentrates in the interface area, inducing micro-gap. The continuous accumulation of stress causes slight bulging defects. In boiling water, water vapor seeps in along the micro-gap at the interface, damaging the interface and penetrating the printing ink layer, resulting in whitening and bleeding. Under repeated bending loads, the micro-defects at the interface continue to expand, eventually causing failure problems such as localized peeling of the print and micro-tears in the printing paper.
[0039] Comparative Example 3 differed from Example 1 only in that "silane coupling agent KH-560" was not added during the preparation of the sustained-release inhibitor; all other steps and parameters were the same. Compared to Example 1, the peel strength decreased to 4.0 kN / m, and while water boiling resistance was improved, whitening and ink bleeding occurred, and localized detachment occurred during bending fatigue. This may be because, lacking silane molecular bridging, the modified coating and melamine transfer paper only rely on physical adsorption to bond, failing to form stable chemical bonds; under high-temperature water boiling conditions, continuous water vapor intrusion into the interface disrupted the interfacial bonding, and water vapor penetration into the transfer paper ink layer caused bleeding, making the interface highly susceptible to detachment under external bending forces.
[0040] Comparative Example 4: The decals were cut without any positive allowance and directly to the finished size. Compared to Example 1, the sample showed obvious bulging and indentation, and the decals had cracks; the interfacial peel strength was significantly reduced to 1.6 kN / m, and it severely whitened and peeled off after boiling in water. Large-area tearing occurred during the bending test. This may be because the silicone vulcanization shrinkage caused dimensional reduction, and without allowance compensation, the decals were continuously subjected to uniaxial tensile stress, which exceeded the paper fiber's bearing capacity, directly causing breakage; continuous stretching caused the modified transition layer to be continuously stretched, resulting in micro-cracks, destruction of interfacial integrity, rapid moisture penetration, and significant deterioration of various durability properties.
[0041] Comparative Example 5 simplified the solvent process by eliminating the segmented addition and vacuum extraction of isopropanol, adding all isopropanol at once. Compared to Example 1, local micro-gaps were observed in the cross-section, the sample showed slight bulging, paper cracking, a peel strength of 3.4 kN / m, and slight peeling and color bleeding occurred during boiling. This may be due to the lack of vacuum extraction for impurity removal and gradient solvent control, resulting in residual low-boiling-point solvent in the modified solution. During the curing process, solvent escaped and formed micro-voids at the interface; the wet film evaporation rate was uncontrollable, the modified coating thickness was uneven, the continuity of the flexible transition layer was damaged, and the stress buffering capacity decreased, ultimately leading to interface defects and paper cracking.
[0042] Comparative Example 6 increased the platinum catalyst dosage to 20 ppm. Compared with Example 1, the finished product showed slight bulging and indentation, the peel strength decreased to 4.9 kN / m, and micro-detachment and whitening occurred during boiling in water, with localized detachment after bending. This may be due to the excessively high platinum catalyst concentration, the excessively fast crosslinking reaction rate of the modified system, the high crosslinking density of the coating, the decreased flexibility, and the weakened elastic buffering capacity; the inability to effectively dissipate the shrinkage stress between the silicone and the decal during the vulcanization stage, which easily leads to interfacial micro-defects; and the increased rigidity of the dense, highly crosslinked structure, which is more prone to interfacial micro-cracks when subjected to thermal cycling and bending forces.
[0043] Comprehensive test results confirm that this invention utilizes a synergistic approach involving multiple technologies: sustained-release inclusion inhibitors, a hydrolyzed and activated silane bridging system, gradient temperature-controlled modification, shrinkage allowance compensation for transfer paper, and segmented solvent regulation. All process parameters are precisely matched and indispensable. This allows for the construction of a continuous, flexible cross-linked transition layer during compression molding and co-curing, effectively mitigating the internal stress caused by the shrinkage of dissimilar materials and establishing a strong chemical bond between the transfer paper and silicone. It completely solves the problems of delamination, color bleeding, transfer paper tearing, and product bulging and warping inherent in traditional processes. Furthermore, it combines the stability of the modified liquid during application, the quality of the finished product's appearance, and long-term durability, demonstrating significant value for industrial application.
[0044] The foregoing has provided a detailed description of one embodiment of the present invention, but this description is merely a preferred embodiment and should not be construed as limiting the scope of the invention. All equivalent variations and modifications made within the scope of the claims of this invention should still fall within the patent coverage of this invention.
Claims
1. A flexible cross-linked silicone-embedded integral molding process for melamine decals, characterized in that, Includes the following steps: S1: Cut the melamine decal paper according to the finished size, leaving a fixed positive allowance of 1.0%-1.1%. Then clean, pre-dry, and cool to obtain the pre-treated melamine decal paper. S2: Immerse the pretreated melamine decal completely in the modification solution and remove it after 5-8 seconds, or evenly coat both sides of the pretreated melamine decal with the modification solution, then drain the liquid vertically and blow away the accumulated liquid with low pressure, then let it stand at 15-35℃ for 2-3 minutes, and finally treat it at 75℃ for 10-12 minutes. After cooling, the modified melamine decal is obtained. S3: The modified melamine decal is flattened and pre-placed in the cavity of the silicone mold. Liquid addition-curing silicone is injected into the mold and co-cured at 165-170℃ to obtain the melamine-embedded printing silicone. The modified liquid is prepared from vinyl-terminated silicone oil, silane activating liquid, sustained-release inhibitor, isopropanol, hydrogen-containing silicone oil, and platinum catalyst.
2. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 1, characterized in that, The modified liquid is prepared as follows: Add silane activating solution and slow-release inhibitor to the stirred vinyl silicone oil and stir for 3-5 min. Then add isopropanol 1 and vacuum extract for 10-15 min at 35-40℃ and -0.06--0.07MPa. Then add isopropanol 2 and stir for 2 min. After cooling to 15-20℃, add hydrogen-containing silicone oil and stir for 3 min. Before use, add platinum catalyst and stir for 4 min. Finally, let stand for 5-7 min to degas and obtain the modified solution.
3. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 2, characterized in that, The mass ratio of the terminal vinyl silicone oil, silane activating liquid, sustained-release inhibitor, isopropanol 1, isopropanol 2, and hydrogen-containing silicone oil is 100:12:12:20:35-45:3.8-4.
2.
4. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 1, characterized in that, The embedded melamine printing silicone contains 10-15 ppm of effective platinum by total mass.
5. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 1, characterized in that, The preparation method of the sustained-release inhibitor is as follows: A1: Add β-cyclodextrin to deionized water and stir at 60°C for 20-30 min. Then add acetylenecyclohexanol dropwise and stir at 60°C for 3 h. Then cool to 4°C and let stand at 4°C for 12 h. Then filter, wash the filter cake, dry and grind to obtain the inclusion complex powder. A2: Add deionized water to isopropanol and sonicate for 10 min. Then add silane coupling agent KH-560 and adjust the pH to 4.3-4.
7. Stir at 50-55℃ for 40-50 min, cool to 30℃ and add compound powder and sonicate for 10 min. Then stir at 45℃ for 3 h to obtain sustained-release inhibitor.
6. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 5, characterized in that, The mass ratio of deionized water, β-cyclodextrin, and acetylenol in A1 is 100-120: 11.35-13.62 g: 1.24-1.
49.
7. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 5, characterized in that, The mass ratio of isopropanol, deionized water, silane coupling agent KH-560, and compound powder in A2 is 8-9:0.3:0.5:2.
2.
8. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 1, characterized in that, The preparation method of the silane activation solution is as follows: Add silane coupling agent KH-560 and deionized water to isopropanol and adjust the pH to 4.5-5.
0. Then, stir and hydrolyze at 25°C for 30-40 minutes to obtain silane activated solution.
9. The melamine decal flexible cross-linked embedded silicone integral molding process according to claim 8, characterized in that, The ratio of isopropanol, silane coupling agent KH-560, and deionized water is 10-12. 1.8:0.3-0.5。