A high-temperature, high-pressure magnetohydrodynamic metal oil seal and its preparation method

By combining a gradient porosity sintered metal skeleton with a samarium cobalt permanent magnet ring, the problem of self-replenishment and leakage prevention of magnetohydrodynamic seals at high temperatures is solved, realizing the self-replenishment and leakage prevention functions of high-temperature and high-pressure magnetohydrodynamic metal oil seals, meeting the requirements of high-temperature working conditions.

CN123110367APending Publication Date: 2026-11-17JIANGSU OSIM HIGH-TECH MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611200946.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing magnetohydrodynamic sealing technology suffers from rapid degradation of sealing performance after the magnetohydrodynamic fluid is consumed under high-temperature conditions, cannot achieve self-replenishment, has a complex structure and is not suitable for compact applications, and lacks an effective structural design for integrating magnetohydrodynamic fluid with a metal skeleton.

Method used

A gradient porosity sintered metal skeleton is adopted, with a liquid storage layer, a sealing layer and a retaining layer arranged radially. Combined with a samarium cobalt permanent magnet ring and a high-temperature magnetic fluid, the magnetic fluid in the gradient porosity sintered metal skeleton achieves self-liquid replenishment and leakage prevention, while the samarium cobalt permanent magnet ring provides magnetic field support.

Benefits of technology

It achieves the self-replenishing function of magnetorheological fluid at high temperatures, extends the sealing life, improves pressure resistance, has a compact structure and does not require an external replenishment system, and meets the requirements of high temperature and high pressure conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to the field of mechanical seal technology, specifically to a high-temperature, high-pressure magnetofluid metal oil seal and its preparation method, comprising a gradient porosity sintered metal skeleton, a samarium cobalt permanent magnet ring, and a high-temperature magnetofluid. The gradient porosity sintered metal skeleton consists of a reservoir layer, a sealing layer, and a retaining layer arranged radially from the inside to the outside. The reservoir layer has a porosity of 40% to 50% and an average pore size of 15 to 30 μm; the sealing layer has a porosity of 25% to 35% and an average pore size of 5 to 15 μm; and the retaining layer has a porosity of 8% to 15% and an average pore size of 1 to 5 μm. In this invention, the capillary pressure gradient of the gradient porosity sintered metal skeleton enables directional self-replenishing fluid transport from the reservoir layer to the sealing interface, solving the problem in the prior art where the magnetofluid cannot be automatically replenished after consumption, leading to seal failure. This increases the continuous working life at 250°C from no more than 860 hours in the prior art to over 2910 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of mechanical seal technology, specifically to a high-temperature, high-pressure magnetic fluid metal oil seal and its preparation method. Background Technology

[0002] Rotary shaft seals are a key technology in industrial equipment, widely used in petrochemicals, aerospace, energy, and precision manufacturing. Traditional oil seals primarily rely on the elastic contact between a rubber lip and the shaft surface for sealing, which suffers from rapid wear, short lifespan, and high-temperature aging failure. Magnetohydrodynamic (MHD) sealing technology utilizes a magnetic fluid to form a liquid O-ring under the influence of a magnetic field, achieving zero-leakage, non-contact sealing with significant advantages such as zero wear, low friction, and self-healing. However, existing MHD sealing technologies still face several technical bottlenecks in practical engineering applications.

[0003] Existing patent CN115949754A discloses a metal skeleton for magnetohydrodynamic sealing, which employs a ring-shaped structure in conjunction with a rotating shaft to create a micro-dynamic pressure effect and a labyrinth sealing effect. Under the action of an external magnetic field, the magnetohydrodynamic fluid is adsorbed onto the skeleton, forming a flesh-encased skeleton structure. In this design, the metal skeleton is a solid ring-shaped structure and does not have a porous liquid storage function. The magnetohydrodynamic fluid only adheres to the surface of the skeleton, making it impossible to achieve self-replenishment and continuous supply of the magnetohydrodynamic fluid. Under high-temperature conditions, the sealing performance rapidly declines after the magnetohydrodynamic fluid is consumed by evaporation and shearing.

[0004] Existing patent CN121916311A discloses a magnetic oil seal and its preparation method, which uses hydrogenated nitrile rubber and magnetic powder to prepare a magnetic rubber layer, and combines it with a metal skeleton to form a magnetic oil seal. In this solution, the magnetic rubber is a solid magnetic material, and the magnetic powder particles are fixed in the rubber matrix, which cannot form a liquid O-ring seal. The sealing mechanism still relies on the elastic contact of the rubber lip, which is essentially still a contact seal, and is subject to wear and high-temperature aging problems. Moreover, the working temperature of the rubber matrix generally does not exceed 150°C.

[0005] Existing patent CN111963685B discloses a combined cartridge dynamic seal based on magnetorheological fluid, which improves pressure resistance by combining multi-stage magnetic rings with permanent magnets and setting pressure-reducing pipelines between stages. This solution is a complex combined sealing device with a large structural volume. The magnetorheological fluid is directly filled into the sealing gap, lacking internal storage and self-replenishing mechanisms. After the magnetorheological fluid is consumed, it needs to be replenished externally, making maintenance inconvenient.

[0006] Existing patents CN103996480A and CN105225786A disclose methods for preparing fluorinated oil-based and perfluoropolyether oil-based magnetic fluids, respectively, and provide technical solutions for high-temperature magnetic fluid materials. However, neither of them involves the structural design of integrating magnetic fluids with metal skeletons into an integrated oil seal product.

[0007] In summary, the existing technologies have the following shortcomings: solid metal skeletons or magnetic rubber solutions cannot achieve internal storage and directional self-replenishment of magnetic fluid, and the seal fails after the magnetic fluid is consumed at high temperatures; magnetic rubber oil seals are still contact seals, and their operating temperature is limited by the rubber matrix, which cannot meet the high-temperature conditions above 250℃; existing magnetic fluid sealing devices have complex structures and large volumes, making them unsuitable for compact oil seal applications; the integrated design of magnetic fluid and metal skeleton lacks effective microstructural design, and the problems of maintaining and directionally transporting magnetic fluid in the metal skeleton have not been solved. Summary of the Invention

[0008] The primary objective of this invention is to provide a high-temperature, high-pressure magnetic fluid metal oil seal and its preparation method.

[0009] A further objective of this invention is to provide a high-temperature, high-pressure magnetic fluid metal oil seal, comprising a gradient porosity sintered metal skeleton, a samarium cobalt permanent magnet ring, and a high-temperature magnetic fluid. The gradient porosity sintered metal skeleton consists of a reservoir layer, a sealing layer, and a retaining layer arranged radially from the inside to the outside. The reservoir layer has a porosity of 40% to 50% and an average pore size of 15 to 30 μm. The sealing layer has a porosity of 25% to 35% and an average pore size of 5 to 15 μm. The retaining layer has a porosity of 8% to 15% and an average pore size of 1 to 5 μm. The high-temperature magnetic fluid is filled into the pores of the gradient porosity sintered metal skeleton by vacuum impregnation. The samarium cobalt permanent magnet ring is embedded on the outside of the gradient porosity sintered metal skeleton and is axially magnetized, with the magnetic field it generates passing through the sealing layer region.

[0010] Preferably, the high-temperature magnetic fluid comprises, by mass parts: 25 to 50 parts of surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 47 to 73 parts of toluene silicone oil, 0.8 to 1.5 parts of phenyl-α-naphthylamine, and 0.5 to 2 parts of hexagonal boron nitride nanosheets, with the sum of the mass parts of each component being 100. The Fe3O4 core of the Fe3O4 / SiO2 core-shell nanoparticles has an average particle size of 8 to 12 nm and a SiO2 shell thickness of 2 to 3 nm. The toluene silicone oil has a kinematic viscosity of 150 to 300 mPa·s at 25°C.

[0011] Preferably, the surface modifier of Fe3O4 / SiO2 core-shell nanoparticles is carboxyl-terminated tolyl silicone oil. The structure of the carboxyl-terminated tolyl silicone oil includes tolylsiloxane segments and terminal carboxyl groups. The tolylsiloxane segments match the structure of the tolyl silicone oil carrier, and the terminal carboxyl groups form hydrogen bonds and partial covalent bonds with the silanol groups on the surface of the SiO2 shell.

[0012] Preferably, the gradient porosity sintered metal skeleton is made of 316L stainless steel, the liquid storage layer has a thickness of 1.5 to 2.5 mm, the sealing layer has a thickness of 0.8 to 1.5 mm, and the retaining layer has a thickness of 0.5 to 1.0 mm. The gradient porosity sintered metal skeleton is prepared by using ammonium bicarbonate as a pore-forming agent and adding polyvinyl alcohol as a binder. The amount of ammonium bicarbonate added to the liquid storage layer is 25% to 35% of the mass of 316L stainless steel powder, the amount of ammonium bicarbonate added to the sealing layer is 10% to 20%, and the amount of ammonium bicarbonate added to the retaining layer is 3% to 8%.

[0013] Preferably, the samarium cobalt permanent magnet ring is an Sm2Co17 type permanent magnet with a remanence greater than 1.05T, an intrinsic coercivity greater than 1990kA / m, and a maximum operating temperature of not less than 350℃.

[0014] Preferably, the gradient porosity sintered metal skeleton further includes a dense 316L stainless steel outer ring, the porosity of which is less than 3%, and the dense 316L stainless steel outer ring is interference-fitted with the outer surface of the samarium cobalt permanent magnet ring and the retaining layer.

[0015] Preferably, the hexagonal boron nitride nanosheets have an average sheet diameter of 100 to 300 nm and a thickness of 20 to 50 nm, and the mass ratio of hexagonal boron nitride nanosheets to phenyl-α-naphthylamine is 0.6:1 to 2:1.

[0016] A method for preparing the high-temperature, high-pressure magnetohydrodynamic metal oil seal includes the following steps: Step 1, Preparation of Fe3O4 / SiO2 core-shell nanoparticles: FeCl3·6H2O and FeCl2·4H2O were dissolved in deionized water at a molar ratio of ferric ions to ferrous ions of 1.75:1 to 2:1. After heating to 65 to 75°C, ammonia solution was added under nitrogen protection to precipitate Fe3O4 nanoparticles. After washing to neutrality, the Fe3O4 nanoparticles were dispersed in an ethanol-water mixture. Tetraethyl orthosilicate and ammonia were added and reacted at 45 to 55°C for 3 to 5 hours to coat the surface of the Fe3O4 particles with a SiO2 shell to obtain Fe3O4 / SiO2 core-shell nanoparticles. After separation and washing, the nanoparticles were dispersed in toluene, and then carboxyl-terminated toluene silicone oil was added and stirred at 75 to 85°C for 3 to 5 hours for surface modification. After washing, the nanoparticles were vacuum dried to obtain surface-modified Fe3O4 / SiO2 core-shell nanoparticles. Step 2, preparation of high-temperature magnetic fluid: The surface-modified Fe3O4 / SiO2 core-shell nanoparticles obtained in Step 1 are mixed with toluene silicone oil, phenyl-α-naphthylamine and hexagonal boron nitride nanosheets in a certain ratio, and ball-milled in a planetary ball mill at 200 to 300 r / min for 3 to 5 h, and then centrifuged at 3000 r / min for 8 to 12 min to remove the precipitated large particle agglomerates. The upper uniform dispersion is taken as the high-temperature magnetic fluid. Step 3, preparation of gradient porosity sintered metal skeleton: 316L stainless steel powder, ammonium bicarbonate pore-forming agent and polyvinyl alcohol binder (added at 1% to 2% of the mass of stainless steel powder) are mixed in different proportions to prepare retaining layer powder, sealing layer powder and liquid storage layer powder, which are then loaded into molds in sequence and pressed under a pressure of 380 to 420 MPa to obtain green blanks. The green blanks are placed in a hydrogen atmosphere furnace and slowly heated to 1140 to 1200℃ and held for 1.5 to 2.5 hours for sintering. The furnace is then cooled to room temperature to obtain gradient porosity sintered metal skeleton. Step 4, Assembly and Impregnation: Assemble the samarium cobalt permanent magnet ring and the dense 316L stainless steel outer ring with the gradient porosity sintered metal skeleton. Place the assembly in a vacuum chamber and evacuate it to below -0.090 MPa for 25 to 35 minutes. Inject the high-temperature magnetic fluid prepared in Step 2 to completely immerse the gradient porosity sintered metal skeleton. Slowly release the vacuum to atmospheric pressure and maintain it for 50 to 70 minutes to allow the magnetic fluid to fully penetrate the pores. Remove the seal and wipe off any excess magnetic fluid from the surface to obtain the high-temperature and high-pressure magnetic fluid metal oil seal.

[0017] Preferably, the sintering heating rate in step three is 3 to 5 °C / min, and the furnace cooling rate is 2 to 4 °C / min.

[0018] Preferably, in step one, the amount of tetraethyl orthosilicate added is 10% to 20% of the mass of Fe3O4 nanoparticles, and the amount of carboxyl-terminated toluene silicone oil added is 12% to 20% of the total mass of Fe3O4 / SiO2 core-shell nanoparticles.

[0019] Compared with the prior art, the beneficial effects of the present invention are: 1. In this invention, the capillary pressure gradient of the gradient porosity sintered metal skeleton enables the directional self-replenishing fluid transport from the reservoir layer to the sealing interface, solving the problem of sealing failure caused by the inability to automatically replenish the magnetic fluid after it is consumed in the prior art, and increasing the continuous working life at 250°C from no more than 860 hours in the prior art to more than 2910 hours.

[0020] 2. In the gradient porosity structure of this invention, the minimum pore size of the retaining layer generates the maximum capillary pressure, forming an atmospheric side magnetofluid leakage barrier. Combined with the high-capacity storage of the liquid storage layer, the magnetofluid mass loss rate after 1000 hours of high-temperature aging is reduced from more than 34.2% in the prior art to less than 14.1%.

[0021] 3. The SiO2 shell of the Fe3O4 / SiO2 core-shell nanoparticles of this invention prevents Fe3O4 oxidation at high temperatures, thereby increasing the saturation magnetization retention rate of the magnetofluid at 250°C from about 58% without the shell to more than 86.5%, ensuring the magnetic field response capability at high temperatures.

[0022] 4. In this invention, the phenyl structure of the toluene silicone oil carrier enables the long-term working temperature to reach an upper limit of 280°C, which is much higher than the 200°C of dimethyl silicone oil and the 150°C of ester-based carrier liquid, thus meeting the requirements of high-temperature working conditions.

[0023] 5. In this invention, the thermal conductivity enhancement effect of hexagonal boron nitride nanosheets reduces the local temperature rise of the sealing gap by 5 to 15°C, effectively delaying the thermal evaporation and thermal degradation of the magnetic fluid and extending the sealing life.

[0024] 6. Compared with magnetic rubber oil seals, this invention is a non-contact liquid seal, which eliminates the wear and aging problems of the rubber lip. The sealing pressure resistance at 250℃ reaches more than 2.14MPa, which is much higher than the 0.53MPa of magnetic rubber oil seals. The integrated oil seal structure of this invention is compact, requiring no external magnetic fluid replenishment system and cooling pipeline, and is easy to install and maintain. Detailed Implementation

[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] The inventive mechanism of this invention is as follows: The gradient porosity sintered metal skeleton consists of a liquid storage layer, a sealing layer, and a retaining layer, arranged radially from the inside out. The porosity and pore size of the three layers decrease radially.

[0027] According to the Young-Laplace equation, capillary pressure is inversely proportional to pore size. The retaining layer has the smallest pore size, thus maximizing capillary pressure, while the reservoir layer has the largest pore size, resulting in minimum capillary pressure. This capillary pressure gradient drives the magnetofluid to migrate directionally from the reservoir layer through the sealing layer to the shaft surface, forming a self-replenishing fluid delivery channel. When the magnetofluid at the sealing interface decreases due to high-temperature evaporation or shearing, the capillary pressure gradient automatically transports magnetofluid from the reservoir layer to the sealing interface to replenish it, achieving a self-repairing function. The retaining layer, with its minimum pore size and maximum capillary pressure, also acts as a barrier to prevent magnetofluid leakage to the atmosphere.

[0028] Simultaneously, the magnetic field generated by the samarium cobalt permanent magnet ring passes through the gradient porosity sintered metal skeleton, forming a high magnetic field gradient region in the gap between the inner wall of the sealing layer and the shaft surface. Fe3O4 nanoparticles in the magnetofluid aggregate towards the sealing gap under the action of the magnetic field gradient, forming a multi-level liquid O-ring seal, which, together with the capillary pressure gradient, achieves a dual magnetic-capillary driven seal.

[0029] In Fe3O4 / SiO2 core-shell nanoparticles, the SiO2 shell plays a triple role at high temperatures: The SiO2 shell physically isolates oxygen and moisture, preventing the Fe3O4 core from oxidizing to γ-Fe2O3 at temperatures above 200℃, which would lead to a decrease in magnetic properties. The silanol groups on the surface of the SiO2 shell provide hydrogen bonding and covalent bonding sites for the carboxyl-terminated toluene silicone oil surface modifier, ensuring the long-term stable dispersion of nanoparticles in the toluene silicone oil carrier. The SiO2 shell has an amorphous structure, which maintains chemical stability and structural integrity over a wide temperature range, reducing interfacial delamination and aggregation between nanoparticles and the support during temperature cycling.

[0030] Toluene silicone oil, used as a carrier fluid, possesses a phenyl group in its molecular structure that provides higher thermal stability than methyl groups, enabling it to operate at temperatures above 280°C for extended periods and withstand short-term temperatures up to 350°C. The introduction of the phenyl group also lowers the viscosity-temperature coefficient, allowing the magnetic fluid to maintain appropriate viscosity over a wide temperature range. This ensures sufficient fluidity at high temperatures for self-replenishment while preventing excessively high viscosity at low temperatures that could lead to excessive starting torque.

[0031] Hexagonal boron nitride nanosheets dispersed in a magnetic fluid significantly enhance the equivalent thermal conductivity of the magnetic fluid due to their high thermal conductivity. This allows for rapid conduction of the frictional heat generated at the sealing interface to the metal skeleton for dissipation, reducing the local temperature rise in the sealing gap by approximately 5 to 15°C and delaying the high-temperature evaporation and thermal degradation of the magnetic fluid.

[0032] Raw material source: FeCl3·6H2O, analytical grade, purity >99%, Sinopharm Chemical Reagent Co., Ltd.; FeCl2·4H2O, analytical grade, purity >99%, Sinopharm Chemical Reagent Co., Ltd.; ammonia solution, mass fraction 25% to 28%, analytical grade, Sinopharm Chemical Reagent Co., Ltd.; tetraethyl orthosilicate, analytical grade, purity >98%, Sinopharm Chemical Reagent Co., Ltd.; anhydrous ethanol, analytical grade, purity >99.7%, Sinopharm Chemical Reagent Co., Ltd.; carboxyl-terminated toluene silicone oil, viscosity 120 mPa· s, COOH content 1.2%, custom-synthesized by Jining Huakai Resin Co., Ltd.; Toluene silicone oil, grade 250PCS, kinematic viscosity 200mPa·s at 25℃, flash point greater than 310℃, Shin-Etsu Chemical Co., Ltd., Japan; Phenyl-α-naphthylamine, analytical grade, purity greater than 98%, Aladdin Reagent Co., Ltd.; Hexagonal boron nitride nanosheets, average sheet diameter 200nm, thickness 30nm, purity greater than 99%, Nanjing Xianfeng Nanomaterials Technology Co., Ltd.; 316L stainless steel powder, -200 mesh, loose packing density 2.9g / cm³. 3, Hergnas Ltd.; Ammonium bicarbonate, analytical grade, purity greater than 99.5%, Sinopharm Chemical Reagent Co., Ltd.; Sm2Co17 permanent magnet ring, grade XGS28H, remanence 1.08T, intrinsic coercivity 2100kA / m, maximum operating temperature 350℃, Ningbo Songke Magnetic Materials Co., Ltd.; Dense 316L stainless steel outer ring, porosity less than 2%, outer diameter 62mm, inner diameter 54mm, thickness 4mm, commercially available machined parts.

[0033] Example 1: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of 35 parts surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 62.3 parts toluene silicone oil (250 pieces), 1.2 parts phenyl-α-naphthylamine, and 1.5 parts hexagonal boron nitride nanosheets. The gradient porosity sintered metal framework is composed of 316L stainless steel powder, with 30% ammonium bicarbonate added to the reservoir layer, 15% to the sealing layer, and 5% to the retaining layer. The pressing pressure is 400 MPa, the sintering temperature is 1180℃, and the sintering time is 2 h. The Sm2Co17 permanent magnet ring is grade XGS28H.

[0034] Preparation process: Step 1: Dissolve 8.1g FeCl3·6H2O and 3.0g FeCl2·4H2O in 150mL of deionized water, heat to 70℃, add 20mL of 25% ammonia solution under nitrogen protection, stir at 500r / min for 30min to obtain black Fe3O4 precipitate, wash with deionized water 5 times until pH 7.

[0035] The washed Fe3O4 particles were dispersed in a mixture of 150 mL anhydrous ethanol and 30 mL deionized water, and 3 mL tetraethyl orthosilicate and 5 mL ammonia solution were added. The mixture was stirred at 300 r / min for 4 h at 50 °C to obtain Fe3O4 / SiO2 core-shell nanoparticles. After washing three times with anhydrous ethanol, the nanoparticles were dispersed in 100 mL toluene.

[0036] 5g of carboxyl-terminated toluene silicone oil was added, and the mixture was heated to 80℃ and stirred at 200r / min for 4h for surface modification. After washing three times with anhydrous ethanol, the mixture was vacuum dried at 60℃ for 12h to obtain surface-modified Fe3O4 / SiO2 core-shell nanoparticles. The average particle size of the Fe3O4 core was 10nm and the thickness of the SiO2 shell was 2.5nm, as determined by transmission electron microscopy.

[0037] Step 2: 35g of surface-modified Fe3O4 / SiO2 core-shell nanoparticles were mixed with 62.3g of toluene silicone oil (250pcs), 1.2g of phenyl-α-naphthylamine, and 1.5g of hexagonal boron nitride nanosheets. The mixture was ball-milled in a planetary ball mill at 250r / min for 4h, and then centrifuged at 3000r / min for 10min to remove the large particle agglomerates at the bottom layer. The uniform black dispersion at the top layer was taken as the high-temperature magnetic fluid, and the saturation magnetization at 25℃ was measured to be 38.6kA / m.

[0038] Step 3: Mix 316L stainless steel powder with ammonium bicarbonate (at mass ratios of 5%, 15%, and 30%) and 1.5% polyvinyl alcohol binder to prepare retaining layer powder, sealing layer powder, and liquid storage layer powder. Then, sequentially pack 5g of retaining layer powder, 4g of sealing layer powder, and 6g of liquid storage layer powder into a mold with an inner diameter of 38mm, and press them unidirectionally under a pressure of 400MPa to obtain a green blank.

[0039] The green blank was placed in a hydrogen atmosphere furnace and heated to 1180℃ at 4℃ / min and held for 2 hours. It was then cooled to room temperature in the furnace at 3℃ / min to obtain a gradient porosity sintered metal skeleton. The porosity of the liquid storage layer was determined to be 45% by the water displacement method, the porosity of the sealing layer was 30% and the porosity of the retention layer was 12%. The average pore size of the liquid storage layer was determined to be 22μm, the average pore size of the sealing layer was 10μm and the average pore size of the retention layer was 3μm by the mercury porosimetry method.

[0040] Step 4: Assemble the Sm2Co17 permanent magnet ring and the dense 316L stainless steel outer ring with the gradient porosity sintered metal skeleton by interference fit. Place the assembly in a vacuum chamber and evacuate to -0.095MPa for 30 minutes. Inject high-temperature magnetic fluid to completely immerse the gradient porosity sintered metal skeleton. Slowly release the vacuum to atmospheric pressure and hold for 60 minutes. Remove the assembly and wipe off any excess magnetic fluid from the surface to obtain the high-temperature and high-pressure magnetic fluid metal oil seal.

[0041] Example 2: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of: 45 parts surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 52.3 parts toluene silicone oil (250 pieces), 1.5 parts phenyl-α-naphthylamine, and 1.2 parts hexagonal boron nitride nanosheets. The gradient porosity sintered metal framework is composed of 316L stainless steel powder, with 35% ammonium bicarbonate added to the reservoir layer, 20% to the sealing layer, and 8% to the retaining layer. The pressing pressure is 400 MPa, the sintering temperature is 1180℃, and the sintering time is 2 h. The Sm2Co17 permanent magnet ring is grade XGS30H.

[0042] Preparation process: Step 1: Dissolve 9.7g FeCl3·6H2O and 3.6g FeCl2·4H2O in 180mL of deionized water, heat to 72℃, add 25mL of 25% ammonia solution under nitrogen protection, stir at 500r / min for 30min to obtain black Fe3O4 precipitate, wash with deionized water 5 times until pH 7.

[0043] The washed Fe3O4 particles were dispersed in a mixture of 180 mL anhydrous ethanol and 35 mL deionized water, and 4 mL tetraethyl orthosilicate and 6 mL ammonia solution were added. The mixture was stirred at 300 r / min for 4 h at 52 °C to obtain Fe3O4 / SiO2 core-shell nanoparticles. After washing three times with anhydrous ethanol, the nanoparticles were dispersed in 120 mL toluene.

[0044] Add 6.5g of carboxyl-terminated toluene silicone oil, heat to 82℃ and stir at 200r / min for 4h for surface modification, wash three times with anhydrous ethanol and then vacuum dry at 60℃ for 12h to obtain surface-modified Fe3O4 / SiO2 core-shell nanoparticles with an average Fe3O4 core particle size of 9nm and a SiO2 shell thickness of 2.2nm.

[0045] Step 2: 45g of surface-modified Fe3O4 / SiO2 core-shell nanoparticles were mixed with 52.3g of toluene silicone oil (250pcs), 1.5g of phenyl-α-naphthylamine, and 1.2g of hexagonal boron nitride nanosheets. The mixture was ball-milled in a planetary ball mill at 250r / min for 4h, and then centrifuged at 3000r / min for 10min to remove the large particle agglomerates at the bottom layer. The uniform black dispersion at the top layer was taken as the high-temperature magnetic fluid, and the saturation magnetization at 25℃ was measured to be 47.3kA / m.

[0046] Step 3: Mix 316L stainless steel powder with ammonium bicarbonate (at mass ratios of 8%, 20%, and 35%) and 1.5% polyvinyl alcohol binder to prepare retaining layer powder, sealing layer powder, and liquid storage layer powder. Then, sequentially pack 5g of retaining layer powder, 4g of sealing layer powder, and 6g of liquid storage layer powder into a mold with an inner diameter of 38mm, and press them unidirectionally under a pressure of 400MPa to obtain a green blank.

[0047] The green blank was placed in a hydrogen atmosphere furnace and heated to 1180℃ at 4℃ / min and held for 2 hours. It was then cooled to room temperature in the furnace at 3℃ / min to obtain a gradient porosity sintered metal skeleton. The porosity of the liquid storage layer was determined to be 50%, the porosity of the sealing layer was 35%, and the porosity of the retention layer was 15% by the water displacement method. The average pore size of the liquid storage layer was determined to be 28μm, the average pore size of the sealing layer was 14μm, and the average pore size of the retention layer was 5μm by the mercury porosimetry method.

[0048] Step 4: Assemble the Sm2Co17 permanent magnet ring and the dense 316L stainless steel outer ring with the gradient porosity sintered metal skeleton by interference fit. Place the assembly in a vacuum chamber and evacuate to -0.095MPa for 30 minutes. Inject high-temperature magnetic fluid to completely immerse the gradient porosity sintered metal skeleton. Slowly release the vacuum to atmospheric pressure and hold for 60 minutes. Remove the assembly and wipe off any excess magnetic fluid from the surface to obtain the high-temperature and high-pressure magnetic fluid metal oil seal.

[0049] Example 3: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of: 25 parts surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 72.8 parts toluene silicone oil (250 pieces), 1.0 part phenyl-α-naphthylamine, and 1.2 parts hexagonal boron nitride nanosheets. The gradient porosity sintered metal framework is composed of 316L stainless steel powder, with 25% ammonium bicarbonate added to the reservoir layer, 10% to the sealing layer, and 3% to the retaining layer. The pressing pressure is 400 MPa, the sintering temperature is 1160℃, and the sintering time is 2 h. The Sm2Co17 permanent magnet ring is grade XGS24H.

[0050] Preparation process: Step 1: Dissolve 6.8g FeCl3·6H2O and 2.5g FeCl2·4H2O in 120mL of deionized water, heat to 68℃, add 18mL of 25% ammonia solution under nitrogen protection, stir at 500r / min for 30min to obtain black Fe3O4 precipitate, wash with deionized water 5 times until pH 7.

[0051] The washed Fe3O4 particles were dispersed in a mixture of 120 mL anhydrous ethanol and 25 mL deionized water, and 2.5 mL tetraethyl orthosilicate and 4 mL ammonia solution were added. The mixture was stirred at 300 r / min for 4 h at 48 °C to obtain Fe3O4 / SiO2 core-shell nanoparticles. After washing three times with anhydrous ethanol, the nanoparticles were dispersed in 80 mL toluene.

[0052] 4g of carboxyl-terminated toluene silicone oil was added, and the mixture was heated to 78℃ and stirred at 200r / min for 4h for surface modification. After washing three times with anhydrous ethanol, the mixture was vacuum dried at 60℃ for 12h to obtain surface-modified Fe3O4 / SiO2 core-shell nanoparticles with an average Fe3O4 core particle size of 11nm and a SiO2 shell thickness of 2.8nm.

[0053] Step 2: 25g of surface-modified Fe3O4 / SiO2 core-shell nanoparticles were mixed with 72.8g of toluene silicone oil (250pcs), 1.0g of phenyl-α-naphthylamine, and 1.2g of hexagonal boron nitride nanosheets. The mixture was ball-milled in a planetary ball mill at 250r / min for 4h, and then centrifuged at 3000r / min for 10min to remove the large particle agglomerates at the bottom layer. The uniform black dispersion at the top layer was taken as the high-temperature magnetic fluid, and the saturation magnetization at 25℃ was measured to be 28.1kA / m.

[0054] Step 3: 316L stainless steel powder was mixed with ammonium bicarbonate (at mass ratios of 3%, 10%, and 25%) and 1.5% polyvinyl alcohol binder to prepare retaining layer powder, sealing layer powder, and reservoir powder. 5g of retaining layer powder, 4g of sealing layer powder, and 6g of reservoir powder were sequentially layered and placed into a mold with an inner diameter of 38mm. The mixture was unidirectionally pressed under a pressure of 400MPa to obtain a green compact. The green compact was placed in a hydrogen atmosphere furnace and heated to 1160℃ at a rate of 4℃ / min, held for 2 hours, and then cooled to room temperature in the furnace at a rate of 3℃ / min to obtain a gradient porosity sintered metal skeleton. The porosity of the reservoir layer was determined to be 40% by the water displacement method, 25% by the sealing layer, and 8% by the retaining layer. The average pore size of the reservoir layer was determined to be 16μm by mercury porosimetry, 6μm by the sealing layer, and 2μm by the retaining layer.

[0055] Step 4: Assemble the Sm2Co17 permanent magnet ring and the dense 316L stainless steel outer ring with the gradient porosity sintered metal skeleton by interference fit. Place the assembly in a vacuum chamber and evacuate to -0.095MPa for 30 minutes. Inject high-temperature magnetic fluid to completely immerse the gradient porosity sintered metal skeleton. Slowly release the vacuum to atmospheric pressure and hold for 60 minutes. Remove the assembly and wipe off any excess magnetic fluid from the surface to obtain the high-temperature and high-pressure magnetic fluid metal oil seal.

[0056] Example 4: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of: 40 parts surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 57.5 parts toluene silicone oil (250 pieces), 1.3 parts phenyl-α-naphthylamine, and 1.2 parts hexagonal boron nitride nanosheets. The gradient porosity sintered metal framework is composed of 316L stainless steel powder, with 32% ammonium bicarbonate added to the reservoir layer, 18% to the sealing layer, and 6% to the retaining layer. The pressing pressure is 400 MPa, the sintering temperature is 1180℃, and the sintering time is 2 h. The Sm2Co17 permanent magnet ring is grade XGS28H.

[0057] Preparation process: Step 1: Dissolve 8.9g FeCl3·6H2O and 3.3g FeCl2·4H2O in 160mL of deionized water, heat to 70℃, add 22mL of 25% ammonia solution under nitrogen protection, stir at 500r / min for 30min to obtain black Fe3O4 precipitate, wash with deionized water 5 times until pH 7.

[0058] The washed Fe3O4 particles were dispersed in a mixture of 160 mL anhydrous ethanol and 32 mL deionized water, and 3.5 mL tetraethyl orthosilicate and 5.5 mL ammonia solution were added. The mixture was stirred at 300 r / min for 4 h at 50 °C to obtain Fe3O4 / SiO2 core-shell nanoparticles. After washing three times with anhydrous ethanol, the nanoparticles were dispersed in 110 mL toluene.

[0059] Add 5.8g of carboxyl-terminated toluene silicone oil, heat to 80℃ and stir at 200r / min for 4h for surface modification, wash three times with anhydrous ethanol and then vacuum dry at 60℃ for 12h to obtain surface-modified Fe3O4 / SiO2 core-shell nanoparticles with an average Fe3O4 core particle size of 10nm and a SiO2 shell thickness of 2.4nm.

[0060] Step 2: 40g of surface-modified Fe3O4 / SiO2 core-shell nanoparticles were mixed with 57.5g of toluene silicone oil (250pcs), 1.3g of phenyl-α-naphthylamine, and 1.2g of hexagonal boron nitride nanosheets. The mixture was ball-milled in a planetary ball mill at 250r / min for 4h, and then centrifuged at 3000r / min for 10min to remove the large particle agglomerates at the bottom layer. The uniform black dispersion at the top layer was taken as the high-temperature magnetic fluid, and the saturation magnetization at 25℃ was measured to be 42.5kA / m.

[0061] Step 3: Mix 316L stainless steel powder with ammonium bicarbonate (at mass ratios of 6%, 18%, and 32%) and 1.5% polyvinyl alcohol binder to prepare retaining layer powder, sealing layer powder, and liquid storage layer powder. Then, layer 5g of retaining layer powder, 4g of sealing layer powder, and 6g of liquid storage layer powder into a mold with an inner diameter of 38mm, and press them unidirectionally under a pressure of 400MPa to obtain a green blank.

[0062] The green blank was placed in a hydrogen atmosphere furnace and heated to 1180℃ at 4℃ / min and held for 2 hours. It was then cooled to room temperature with the furnace at 3℃ / min to obtain a gradient porosity sintered metal skeleton. The porosity of the liquid storage layer was 48%, the porosity of the sealing layer was 32%, and the porosity of the retention layer was 13% by the water displacement method. The average pore size of the liquid storage layer was 25μm, the average pore size of the sealing layer was 12μm, and the average pore size of the retention layer was 4μm by the mercury porosimetry method.

[0063] Step 4: Assemble the Sm2Co17 permanent magnet ring and the dense 316L stainless steel outer ring with the gradient porosity sintered metal skeleton by interference fit. Place the assembly in a vacuum chamber and evacuate to -0.095MPa for 30 minutes. Inject high-temperature magnetic fluid to completely immerse the gradient porosity sintered metal skeleton. Slowly release the vacuum to atmospheric pressure and hold for 60 minutes. Remove the assembly and wipe off any excess magnetic fluid from the surface to obtain the high-temperature and high-pressure magnetic fluid metal oil seal.

[0064] Comparative Example 1: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of 35 parts of surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 62.3 parts of 250 PCS of toluene silicone oil, 1.2 parts of phenyl-α-naphthylamine, and 1.5 parts of hexagonal boron nitride nanosheets, the same as in Example 1.

[0065] Uniform Porosity Sintered Metal Framework: 316L stainless steel powder, ammonium bicarbonate addition 15%, pressing pressure 400MPa, sintering temperature 1180℃, sintering time 2h, resulting in a sintered metal framework with a uniform porosity of approximately 30% and an average pore size of approximately 12μm. Sm2Co17 permanent magnet ring grade XGS28H.

[0066] Preparation process: The magnetofluid preparation process is the same as steps one and two in Example 1. The metal framework is uniformly pressed and sintered with a single 15% ammonium bicarbonate addition, without delamination.

[0067] The assembly and impregnation process is the same as step four of Example 1.

[0068] Comparative Example 2: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of: 35 parts of surface-modified Fe3O4 nanoparticles, 62.3 parts of 250 PCS of toluene silicone oil, 1.2 parts of phenyl-α-naphthylamine, and 1.5 parts of hexagonal boron nitride nanosheets.

[0069] The Fe3O4 nanoparticles have no SiO2 shell and are only surface-modified with carboxyl-terminated toluene silicone oil.

[0070] The gradient porosity sintered metal framework is the same as in Example 1. The Sm2Co17 permanent magnet ring is grade XGS28H.

[0071] Preparation process: The preparation process of Fe3O4 nanoparticles is the same as step one of Example 1, but the tetraethyl orthosilicate coating step is omitted. After washing the Fe3O4 precipitate, carboxyl-terminated toluene silicone oil is directly added and stirred at 80°C for 4 hours for surface modification. The magnetofluid mixing, framework preparation, and assembly impregnation processes are the same as in Example 1.

[0072] Comparative Example 3: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of: 35 parts of surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 62.3 parts of dimethyl silicone oil, 1.2 parts of phenyl-α-naphthylamine, and 1.5 parts of hexagonal boron nitride nanosheets.

[0073] Dimethyl silicone oil with a kinematic viscosity of 200 mPa·s at 25°C replaces toluene silicone oil.

[0074] The gradient porosity sintered metal framework is the same as in Example 1. The Sm2Co17 permanent magnet ring is grade XGS28H.

[0075] Preparation process: The magnetic fluid preparation process is the same as in Example 1, but the carrier liquid is changed to dimethyl silicone oil and the surface modifier is changed to carboxyl-terminated dimethyl silicone oil to match the dimethyl silicone oil carrier.

[0076] The skeleton preparation and assembly impregnation process are the same as in Example 1.

[0077] Comparative Example 4: Raw material formula: Magnetic rubber oil seal: 100 parts hydrogenated nitrile butadiene rubber, 120 parts neodymium iron boron magnetic powder, 30 parts fumed silica, 8 parts hydroxyl-terminated liquid nitrile butadiene rubber, 5 parts polyadipate polyester plasticizer, 3 parts vulcanizing agent, 2 parts accelerator, 5 parts zinc oxide, and 1 part stearic acid. The metal skeleton is a stamped carbon steel skeleton.

[0078] Preparation process: Hydrogenated nitrile rubber was passed through a two-roll mill five times, then fumed silica and zinc oxide were added and mixed for 5 minutes. Neodymium iron boron magnetic powder and hydroxyl-terminated liquid nitrile rubber were added and mixed for 8 minutes. Polyadipic polyester plasticizer, vulcanizing agent, accelerator and stearic acid were added and mixed for 3 minutes to produce sheets. A stamped carbon steel skeleton was placed in a mold and vulcanized at 170°C for 15 minutes. After demolding, the sheets were magnetized in a 1.5T magnetic field to obtain magnetic rubber oil seals.

[0079] Comparative Example 5: Raw material formula: Composite magnetic oil seal: axially filled ferrite permanent magnet ring, 2Cr13 magnetic conductive pole plate, nitrile rubber wrapping layer, and magnetic sealant.

[0080] The magnetic sealant is made by mixing manganese-zinc ferrite powder with a 200-mesh resin-coated anti-corrosion layer and fluoropolymer in a mass ratio of 3:2.

[0081] Preparation process: A ferrite permanent magnet ring is axially magnetized, and 2Cr13 magnetic conductive plates are alternately arranged with the permanent magnet ring to form a multi-level magnetic circuit structure. The nitrile rubber coating layer is molded and vulcanized to wrap the permanent magnet ring and magnetic conductive plates. Magnetic sealant made of manganese zinc ferrite powder and fluorinated grease is injected into the gap between the plates to obtain a composite magnetic oil seal.

[0082] Comparative Example 6: Raw material formula: The high-temperature magnetic fluid, by mass parts, consists of: 35 parts of surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 62.3 parts of perfluoropolyether oil Fomblin Z25, 1.2 parts of phenyl-α-naphthylamine, and 1.5 parts of hexagonal boron nitride nanosheets.

[0083] In this process, Fomblin Z25 perfluoropolyether oil replaces toluene silicone oil as the carrier, and the surface modifier is changed to perfluoropolyether carboxylic acid to match the perfluoropolyether oil carrier.

[0084] The gradient porosity sintered metal framework is the same as in Example 1. The Sm2Co17 permanent magnet ring is grade XGS28H.

[0085] Preparation process: The preparation of Fe3O4 / SiO2 core-shell nanoparticles is the same as step one in Example 1, but the surface modification is changed to perfluoropolyether carboxylic acid and stirred at 70°C for 4 hours.

[0086] The magnetofluid mixing, skeleton preparation, and assembly impregnation processes are the same as in Example 1.

[0087] Comparative Example 7: Raw material formula: The high-temperature magnetic fluid is the same as in Example 1. The metal skeleton is a dense 316L stainless steel ring with three annular grooves machined on the inner wall. The grooves are 0.5 mm wide, 0.3 mm deep, and 1.5 mm apart, and are filled with high-temperature magnetic fluid. The Sm2Co17 permanent magnet ring is grade XGS28H.

[0088] Preparation process: The magnetofluid preparation process is the same as steps one and two in Example 1.

[0089] The dense 316L stainless steel ring is a machined part. After the inner wall is machined with three annular grooves, it is ultrasonically cleaned and high-temperature magnetic fluid is injected into the grooves.

[0090] The assembly method of the samarium cobalt permanent magnet ring and the dense outer ring is the same as in Example 1.

[0091] Performance testing: Test method: The sealing pressure resistance shall be performed in accordance with GB / T 32336-2015. The test shaft diameter is 50mm, the rotation speed is 3000r / min, and the maximum sealing pressure difference shall be measured at 25℃ and 250℃ respectively.

[0092] The continuous working life was determined by continuous operation at 3000 r / min under conditions of 250℃ and 2MPa pressure difference, with the time of the first leak recorded. The mass loss rate after 1000h high-temperature aging was calculated by weighing the sample after 1000h in a 250℃ oven.

[0093] The leakage rate was calculated by weighing the leaked medium collected at 3000 r / min for 24 hours under conditions of 250℃ and 2 MPa pressure difference.

[0094] The saturation magnetization was measured at 25°C and 250°C using a vibrating sample magnetometer, Lake Shore 7407.

[0095] Table 1. Sealing performance test results:

[0096] Table 2. Test results of saturation magnetization of magnetohydrodynamic fluid:

[0097] Test method: Saturation magnetization was measured using a vibrating sample magnetometer (Lake Shore 7407) with a test magnetic field strength of 800 kA / m at 25℃ and 250℃. The retention rate at 250℃ is the ratio of the saturation magnetization at 250℃ to that at 25℃.

[0098] Results analysis: Examples 1 to 4 have a sealing pressure resistance of 2.14 to 3.15 MPa at 250°C, a continuous working life of 2910 to 4560 hours at 250°C, and a mass loss of 8.5% to 14.1% over 1000 hours at 250°C.

[0099] Example 2 exhibits the best performance due to its highest nanoparticle content (45 parts), largest gradient porosity range, sufficient liquid storage capacity, and most significant capillary pressure gradient. Example 4, with a nanoparticle content of 40 parts, has a sealing pressure resistance of 2.83 MPa at 250°C, lower than the expected value extrapolated linearly from 35 to 45 parts. This indicates that the increased magnetohydrodynamic viscosity caused by the higher nanoparticle content has a certain adverse effect on the self-replenishing rate, and the performance improvement shows a marginal decrease trend with increasing content.

[0100] Comparative Example 1, using a uniform 30% porosity framework instead of a gradient porosity framework, achieved a sealing pressure resistance of only 1.23 MPa at 250°C, a continuous working life of 860 hours, and a mass loss of 34.2% after 1000 hours. The sealing pressure resistance at 25°C was 2.74 MPa, a 16% difference from the 3.27 MPa of Example 1. This difference is mainly due to the more thorough distribution of magnetofluid at the sealing interface resulting from the gradient porosity structure. However, at 250°C, the difference widens to 54%, primarily attributed to the lack of a self-replenishing mechanism in the uniform porosity framework under high-temperature evaporation conditions, leading to rapid magnetofluid consumption and a significant decrease in sealing capacity. These results demonstrate that the directional capillary pressure gradient generated by the gradient porosity structure is crucial for achieving self-replenishing sealing in this invention, and cannot be replaced by a uniform porosity framework.

[0101] Comparative Example 2 used exposed Fe3O4 nanoparticles without a SiO2 shell. The sealing pressure resistance at 250℃ was only 1.07 MPa, and the saturation magnetization retention rate at 250℃ was only 58.2%. Exposed Fe3O4 oxidized to weakly magnetic γ-Fe2O3 in air at 250℃, and the sharp decay of magnetic properties led to a decrease in magnetic field response and loss of sealing ability. This result indicates that the high-temperature oxidation protection function of the SiO2 shell is indispensable.

[0102] Comparative Example 3, using dimethyl silicone oil instead of toluene silicone oil, achieved a sealing pressure resistance of only 0.91 MPa at 250°C, with a mass loss of 49.2% after 1000 hours. Dimethyl silicone oil undergoes thermal oxidative degradation above 200°C, with molecular chain breakage producing low-molecular-weight volatiles. The rapid evaporation of the carrier fluid leads to a sharp increase in the viscosity of the magnetofluid until it loses its fluidity. In contrast, the thermal stability of the phenyl group in toluene silicone oil allows the carrier fluid to remain stable below 280°C, highlighting the crucial role of the phenyl structure.

[0103] Comparative Example 4 shows a prior art magnetic rubber oil seal, which has a sealing pressure resistance of only 0.53 MPa at 250℃ and a continuous working life of 195 hours. Hydrogenated nitrile rubber ages and hardens rapidly above 200℃, losing its elasticity and causing the lip to fail to fit the shaft surface. In magnetic rubber, the magnetic powder, being fixed solid particles, cannot form a liquid sealing ring. The non-contact liquid sealing mechanism of this invention fundamentally avoids the problem of rubber aging.

[0104] Comparative Example 5 shows a prior art composite magnetic oil seal, with a sealing pressure resistance of only 0.31 MPa at 250℃ and a continuous working life of 148 hours. The magnetic sealant is a paste rather than a true nano-magnetic fluid, exhibiting weak magnetic response, and the nitrile rubber coating ages and cracks at high temperatures, leading to sealant loss. This invention utilizes a nano-magnetic fluid, vacuum impregnated to fill the pores of the metal framework, eliminating the fluid loss problem caused by rubber aging and cracking.

[0105] Comparative Example 6 used perfluoropolyether oil instead of toluene silicone oil. The sealing pressure resistance at 250°C was 1.87 MPa, the continuous working life was 2480 hours, and the mass loss after 1000 hours was 22.4%. Perfluoropolyether oil exhibits good thermal stability, but its fluorocarbon chains have poor compatibility with the SiO2 shell surface. The bonding force between the perfluoropolyether carboxylic acid modifier and the SiO2 surface is weaker than that of carboxyl-terminated toluene silicone oil, leading to the agglomeration of some nanoparticles. The saturation magnetization of 34.2 kA / m is lower than that of Example 1 (38.6 kA / m), and both the sealing performance and fluid retention capacity are inferior to Example 1. The data from Comparative Example 6 demonstrate that the interfacial compatibility between perfluoropolyether oil and the SiO2 shell is inferior to that of toluene silicone oil, and that a simple replacement cannot achieve equivalent results.

[0106] Comparative Example 7 uses a dense metal ring surface groove filled with magnetic fluid instead of a gradient porosity skeleton. The sealing pressure resistance at 250°C is 1.54 MPa, the continuous working life is 1050 hours, and the mass loss after 1000 hours is 39.5%. The total amount of magnetic fluid in the groove is limited and there is no self-replenishing source. Once the magnetic fluid is consumed at high temperatures, it cannot be replenished, leading to a continuous decrease in pressure resistance due to the reduced magnetic fluid at the sealing interface. The sealing pressure resistance at 25°C is 2.65 MPa, a 19% difference from Example 1. This is mainly because the limited fluid storage capacity of the groove results in a less sufficient distribution of magnetic fluid at the sealing interface compared to the gradient skeleton. The data from Comparative Example 7 demonstrates that the surface groove scheme lacks a self-replenishing mechanism and its performance is far inferior to the gradient porosity scheme; the two are not equivalent replacements.

[0107] Based on the above analysis, the directional capillary pressure gradient self-replenishing liquid mechanism generated by the gradient porosity sintered metal skeleton of this invention, combined with the high-temperature protection of the SiO2 shell and the high-temperature carrier of toluene silicone oil, achieves long-term zero-leakage sealing under operating conditions of 250℃ and 2MPa, and the technical effect exceeds reasonable expectations in the field.

[0108] The high-temperature and high-pressure magnetic fluid metal oil seal provided by this invention can be widely used in reactor stirring shaft seals and compressor shaft seals in the petrochemical field, main pump shaft seals and coolant circulation pump shaft seals in the nuclear power field, engine accessory drive shaft seals and fuel pump shaft seals in the aerospace field, and vacuum chamber rotary shaft seals in the semiconductor manufacturing field.

[0109] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention.

Claims

1. A high-temperature, high-pressure magnetohydrodynamic metal oil seal, characterized in that, The system comprises a gradient porosity sintered metal framework, a samarium cobalt permanent magnet ring, and a high-temperature magnetic fluid. The gradient porosity sintered metal framework consists of a reservoir layer, a sealing layer, and a retaining layer, arranged radially from the inside to the outside. The reservoir layer has a porosity of 40% to 50% and an average pore size of 15 to 30 μm. The sealing layer has a porosity of 25% to 35% and an average pore size of 5 to 15 μm. The retaining layer has a porosity of 8% to 15% and an average pore size of 1 to 5 μm. The high-temperature magnetic fluid is filled into the pores of the gradient porosity sintered metal framework by vacuum impregnation. The samarium cobalt permanent magnet ring is embedded on the outside of the gradient porosity sintered metal framework and is axially magnetized, with the magnetic field it generates passing through the sealing layer region.

2. The high-temperature, high-pressure magnetohydrodynamic metal oil seal as described in claim 1, characterized in that, The high-temperature magnetic fluid comprises, by mass parts: 25 to 50 parts of surface-modified Fe3O4 / SiO2 core-shell nanoparticles, 47 to 73 parts of toluene silicone oil, 0.8 to 1.5 parts of phenyl-α-naphthylamine, and 0.5 to 2 parts of hexagonal boron nitride nanosheets, with the sum of the mass parts of each component being 100. The Fe3O4 core of the Fe3O4 / SiO2 core-shell nanoparticles has an average particle size of 8 to 12 nm and a SiO2 shell thickness of 2 to 3 nm. The toluene silicone oil has a kinematic viscosity of 150 to 300 mPa·s at 25 °C.

3. The high-temperature, high-pressure magnetohydrodynamic metal oil seal as described in claim 2, characterized in that, The surface modifier for Fe3O4 / SiO2 core-shell nanoparticles is carboxyl-terminated tolyl silicone oil. The structure of the carboxyl-terminated tolyl silicone oil includes tolylsiloxane segments and terminal carboxyl groups. The tolylsiloxane segments match the structure of the tolyl silicone oil carrier, and the terminal carboxyl groups form hydrogen bonds and partial covalent bonds with the silanol groups on the surface of the SiO2 shell.

4. The high-temperature, high-pressure magnetohydrodynamic metal oil seal as described in claim 1, characterized in that, The gradient porosity sintered metal skeleton is made of 316L stainless steel. The thickness of the liquid storage layer is 1.5 to 2.5 mm, the thickness of the sealing layer is 0.8 to 1.5 mm, and the thickness of the retaining layer is 0.5 to 1.0 mm. The gradient porosity sintered metal skeleton is prepared by using ammonium bicarbonate as a pore-forming agent and adding polyvinyl alcohol as a binder. The amount of ammonium bicarbonate added to the liquid storage layer is 25% to 35% of the mass of 316L stainless steel powder, the amount of ammonium bicarbonate added to the sealing layer is 10% to 20%, and the amount of ammonium bicarbonate added to the retaining layer is 3% to 8%.

5. A high-temperature, high-pressure magnetohydrodynamic metal oil seal as described in claim 1, characterized in that, The samarium cobalt permanent magnet ring is a Sm2Co17 type permanent magnet with a remanence greater than 1.05T, an intrinsic coercivity greater than 1990kA / m, and a maximum operating temperature of not less than 350℃.

6. The high-temperature, high-pressure magnetohydrodynamic metal oil seal as described in claim 1, characterized in that, The gradient porosity sintered metal skeleton also includes a dense 316L stainless steel outer ring with a porosity of less than 3%. The dense 316L stainless steel outer ring is interference-fitted with the samarium cobalt permanent magnet ring and the outer surface of the retaining layer.

7. A high-temperature, high-pressure magnetohydrodynamic metal oil seal as described in claim 1, characterized in that, The hexagonal boron nitride nanosheets have an average diameter of 100 to 300 nm and a thickness of 20 to 50 nm, and the mass ratio of hexagonal boron nitride nanosheets to phenyl-α-naphthylamine is 0.6:1 to 2:

1.

8. A method for preparing a high-temperature, high-pressure magnetohydrodynamic metal oil seal as described in any one of claims 1 to 7, characterized in that, Includes the following steps: Step 1, Preparation of Fe3O4 / SiO2 core-shell nanoparticles: FeCl3·6H2O and FeCl2·4H2O were dissolved in deionized water at a molar ratio of ferric ions to ferrous ions of 1.75:1 to 2:

1. After heating to 65 to 75°C, ammonia solution was added under nitrogen protection to precipitate Fe3O4 nanoparticles. After washing to neutrality, the Fe3O4 nanoparticles were dispersed in an ethanol-water mixture. Tetraethyl orthosilicate and ammonia were added and reacted at 45 to 55°C for 3 to 5 hours to coat the surface of the Fe3O4 particles with a SiO2 shell to obtain Fe3O4 / SiO2 core-shell nanoparticles. After separation and washing, the nanoparticles were dispersed in toluene, and then carboxyl-terminated toluene silicone oil was added and stirred at 75 to 85°C for 3 to 5 hours for surface modification. After washing, the nanoparticles were vacuum dried to obtain surface-modified Fe3O4 / SiO2 core-shell nanoparticles. Step 2, preparation of high-temperature magnetic fluid: The surface-modified Fe3O4 / SiO2 core-shell nanoparticles obtained in Step 1 are mixed with toluene silicone oil, phenyl-α-naphthylamine and hexagonal boron nitride nanosheets in a certain ratio, and ball-milled in a planetary ball mill at 200 to 300 r / min for 3 to 5 h, and then centrifuged at 3000 r / min for 8 to 12 min to remove the precipitated large particle agglomerates. The upper uniform dispersion is taken as the high-temperature magnetic fluid. Step 3, preparation of gradient porosity sintered metal skeleton: 316L stainless steel powder, ammonium bicarbonate pore-forming agent and polyvinyl alcohol binder (added at 1% to 2% of the mass of stainless steel powder) are mixed in different proportions to prepare retaining layer powder, sealing layer powder and liquid storage layer powder, which are then loaded into molds in sequence and pressed under a pressure of 380 to 420 MPa to obtain green blanks. The green blanks are placed in a hydrogen atmosphere furnace and slowly heated to 1140 to 1200℃ and held for 1.5 to 2.5 hours for sintering. The furnace is then cooled to room temperature to obtain gradient porosity sintered metal skeleton. Step 4, Assembly and Impregnation: Assemble the samarium cobalt permanent magnet ring and the dense 316L stainless steel outer ring with the gradient porosity sintered metal skeleton. Place the assembly in a vacuum chamber and evacuate it to below -0.090 MPa for 25 to 35 minutes. Inject the high-temperature magnetic fluid prepared in Step 2 to completely immerse the gradient porosity sintered metal skeleton. Slowly release the vacuum to atmospheric pressure and maintain it for 50 to 70 minutes to allow the magnetic fluid to fully penetrate the pores. Remove the seal and wipe off any excess magnetic fluid from the surface to obtain the high-temperature and high-pressure magnetic fluid metal oil seal.

9. The preparation method according to claim 8, characterized in that, In step three, the sintering heating rate is 3 to 5 °C / min, and the furnace cooling rate is 2 to 4 °C / min.

10. The preparation method according to claim 8, characterized in that, In step one, the amount of tetraethyl orthosilicate added is 10% to 20% of the mass of Fe3O4 nanoparticles, and the amount of carboxyl-terminated toluene silicone oil added is 12% to 20% of the total mass of Fe3O4 / SiO2 core-shell nanoparticles.

Citation Information

Patent Citations

  • Perfluoropolyether-grease-based magnetic fluid and preparation method thereof

    CN103996480A

  • Preparing method for perfluoropolyether oil-based magnetofluid material

    CN105225786A

  • Magnetic oil seal and preparation method thereof

    CN121916311A