Electrochromic devices and their fabrication methods

By controlling the temperature and slowly cooling the electrochromic device, the orange peel texture defect problem was solved, the appearance and optical performance of the device were improved, and the application range was expanded.

CN123113204APending Publication Date: 2026-11-17SHENZHEN GUANGYI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510624613.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing electrochromic devices are prone to surface defects such as orange peel texture after post-processing, which affects the uniformity of appearance and optical flatness.

Method used

In the fabrication process of electrochromic devices, the temperature of the stack is controlled by heating to 15℃-30℃ above the melting temperature of the adhesive layer and slowly cooling to the glass transition temperature range, controlling the cooling rate to be less than or equal to 1.5℃/min, and setting up a heat preservation platform within the stress relaxation temperature range to slow down the cooling rate.

Benefits of technology

It effectively reduces or avoids defects such as orange peel texture, improves the appearance and optical flatness of electrochromic devices, and expands their application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113204A_ABST
    Figure CN123113204A_ABST
Patent Text Reader

Abstract

This application relates to an electrochromic device and its fabrication method. The fabrication method includes: providing an electrochromic film, two glass substrates, and two adhesive layers, forming a stack, wherein the electrochromic film is located between the two glass substrates, and an adhesive layer is disposed between each glass substrate and the electrochromic film; heating the stack to a preset temperature, and cooling the stack to form the electrochromic device. The preset temperature is 15°C-30°C higher than the melting temperature range of the adhesive layers, allowing the adhesive layers to melt sufficiently and reducing the risk of surface unevenness and other defects in the adhesive layers. During the cooling process of the stack, the cooling rate of the stack within the glass transition temperature range of the adhesive layers is less than or equal to 1.5°C / min, which facilitates the slow relaxation of the molecular chain segments of the adhesive layers, reduces shrinkage differences, and improves the surface smoothness of the adhesive layers. The electrochromic device fabricated in this application has excellent appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electro-optic modulation technology, and in particular to an electrochromic device and its fabrication method. Background Technology

[0002] Electro-optic modulation technology alters the physical or chemical properties of a medium by applying an external electric field, thereby changing the intensity and frequency of a light beam emitted through that medium, thus enabling the modulation of the light beam. In recent years, devices utilizing electro-optic modulation technology, such as liquid crystal displays and electrochromic devices, have been increasingly applied in various fields, including electronic devices, wearable devices, transportation, and construction.

[0003] By applying different voltages or currents to an electrochromic device, the electrochromic material within it undergoes a redox reaction, causing it to change color. This alters its color or light transmittance, allowing light beams to pass through completely, partially, or entirely. Typically, electrochromic devices require post-processing during fabrication, such as encapsulation through lamination processes. This protects them from the effects of water and oxygen, preventing failure and enhancing their stability and lifespan.

[0004] However, the electrochromic devices currently in use exhibit surface defects such as orange peel or fish scale textures after post-processing, which significantly reduces the appearance uniformity and optical smoothness of the electrochromic devices. Summary of the Invention

[0005] In view of this, this application provides an electrochromic device and its fabrication method, wherein the temperature of the stack of electrochromic devices is controlled during the lamination process, thereby solving the problem of orange peel texture in electrochromic devices.

[0006] In a first aspect, this application provides a method for fabricating an electrochromic device, comprising:

[0007] An electrochromic film, two glass substrates and two adhesive layers are provided and formed into a stack, wherein the electrochromic film is located between the two glass substrates and an adhesive layer is provided between each glass substrate and the electrochromic film.

[0008] The stack is heated to a preset temperature and then cooled to form the electrochromic device.

[0009] The preset temperature is 15°C-30°C higher than the melting temperature range of the adhesive layer, and the cooling rate of the stack within the glass transition temperature range of the adhesive layer during the cooling process is less than or equal to 1.5°C / min.

[0010] In this embodiment, during the formation of the electrochromic device, the stack undergoes heating and cooling processes sequentially, with the temperatures controlled during both processes. During the heating process, the stack's heating temperature exceeds the adhesive layer's melting temperature by 15°C-30°C, allowing the adhesive layer to fully melt. This improves the adhesive layer's fluidity, reduces the risk of surface defects such as unevenness due to incomplete melting, and enhances the appearance and optical smoothness of the electrochromic device.

[0011] Additionally, during the cooling process, the cooling rate of the stack within the glass transition temperature range of the adhesive layer is slowed down. The adhesive layer is typically composed of polymers, and the glass transition temperature is the critical temperature at which the adhesive layer transitions between a glassy (hard and brittle) and a highly elastic (soft and deformable) state. When the temperature is above the glass transition temperature range, the molecular chain segments in the adhesive layer are actively moving, and the adhesive layer material exhibits a highly elastic state and increased fluidity. Conversely, when the temperature is below the glass transition temperature range, the molecular chain segments in the adhesive layer are frozen, and the adhesive layer material enters the glassy state. If the cooling rate within the glass transition temperature range is too fast—that is, the adhesive layer cools rapidly from a molten state directly to below the glass transition temperature range—the internal thermal stress of the adhesive layer cannot be fully released, easily leading to stress concentration and surface unevenness, affecting the surface smoothness of the adhesive layer, and thus affecting the appearance of the electrochromic device.

[0012] In this embodiment, when the temperature of the stacked body drops to the glass transition temperature range of the adhesive layer, the cooling rate of the stacked body is slowed down, which is conducive to the slow relaxation of the molecular chain segments of the adhesive layer, reducing shrinkage differences and improving the surface flatness of the adhesive layer. This reduces or avoids defects such as orange peel texture in the electrochromic device, and the prepared electrochromic device has a good appearance.

[0013] In one possible implementation, during the cooling of the stack, the stress relaxation temperature range of the adhesive layer includes a first thermal plateau, or the cooling rate of the stack within the stress relaxation temperature range of the adhesive layer is less than or equal to 2°C / min and greater than the cooling rate of the stack within the glass transition temperature range of the adhesive layer; wherein the stress relaxation temperature range of the adhesive layer is 10°C-20°C higher than the glass transition temperature range.

[0014] In one possible implementation, during the heating of the stack to a preset temperature, the heating rate of the stack in the melting temperature range is less than or equal to 2°C / min; or the stack includes a second heat-preserving platform before being heated to the melting temperature range.

[0015] In one possible implementation, before forming the electrochromic device, the method for fabricating the electrochromic device further includes: pressurizing the stack, wherein the pressure applied to the stack before heating it to the preset temperature is less than or equal to 0.3 MPa.

[0016] In one possible implementation, heating the stack to a preset temperature includes: heating the stack to a preset temperature and maintaining the preset temperature for a first preset duration.

[0017] In one possible implementation, the method for fabricating the electrochromic device includes: pressurizing the stack within a first preset time period.

[0018] In one possible implementation, pressurizing the stack during the first preset duration includes: maintaining the preset temperature to a second preset duration, increasing the pressure applied to the stack, and increasing the pressure of the stack to a preset pressure while maintaining the preset temperature to a third preset duration, wherein the second preset duration, the third preset duration, and the first preset duration increase sequentially, and the preset pressure is greater than or equal to 0.8 MPa.

[0019] In one possible implementation, pressurizing the stack during the first preset time period further includes applying a pressure of less than or equal to 0.3 MPa to the stack during the second preset time period.

[0020] In one possible implementation, pressurizing the stack during the first preset time period further includes: the pressurization rate of the stack during the second preset time period is less than 0.01 MPa / min.

[0021] In one possible implementation, pressurizing the stack during the first preset duration further includes: the pressurization rate of the stack during the second preset duration is less than the pressurization rate of the stack during the third preset duration after the second preset duration.

[0022] In one possible implementation, after pressurizing the stack and before forming the electrochromic device, the method for fabricating the electrochromic device further includes: depressurizing the stack, wherein:

[0023] During the cooling of the stack and before the stack cools to the cold flow temperature range of the adhesive layer, the pressure applied to the stack is reduced to less than or equal to 0.15 MPa, and the cold flow temperature range of the adhesive layer is 15°C-25°C lower than the glass transition temperature range.

[0024] In one possible implementation, during the cooling of the stack, the cold flow temperature range of the stack in the adhesive layer includes a third insulation platform, or the cooling rate of the stack in the cold flow temperature range of the adhesive layer is less than or equal to 0.35°C / min.

[0025] Secondly, this application provides an electrochromic device, which is prepared by the method for preparing an electrochromic device as described in any of the preceding claims. Attached Figure Description

[0026] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0027] Figure 1 This is a schematic diagram of an electrochromic device provided in an embodiment of this application.

[0028] Figure 2 This is a cross-sectional schematic diagram of an electrochromic film provided in an embodiment of this application.

[0029] Figure 3 This is a flowchart illustrating the fabrication process of an electrochromic device provided in an embodiment of this application.

[0030] Figure 4 Temperature and pressure control curves for a stack body provided in an embodiment of this application. Detailed Implementation

[0031] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0032] The following explains the terminology that may appear in the embodiments of this application.

[0033] In this application's embodiments, the term "and / or" describes the association relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0034] In the embodiments of this application, "at least one" refers to one or more items, "more than one" refers to two or more items; "at least one of..." or similar expressions refer to any combination of these items, including any combination of a single item or a plurality of items. For example, "at least one selected from a, b or c", or "at least one selected from a, b and c", can both represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, and c can be a single item or multiple items.

[0035] In the embodiments of this application, the terms "first," "second," "third," and similar expressions are used only for descriptive purposes, to distinguish objects, such as substances, from one another, and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. For example, without departing from the scope of the embodiments of this application, "first XX" can also be referred to as "second XX," and similarly, "second XX" can also be referred to as "first XX." Thus, features defined with "first," "second," and "third" may explicitly or implicitly include one or more of that feature.

[0036] In the embodiments of this application, the terms "comprising," "having," and their cognates are intended only to indicate a specific feature, number, step, operation, element, component, or combination of the foregoing, and should not be construed as excluding the existence of one or more other features, numbers, steps, operations, elements, components, or combinations of the foregoing, or adding the possibility of one or more features, numbers, steps, operations, elements, components, or combinations of the foregoing.

[0037] It should be understood that in the various embodiments of this application, the sequence number of each process does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0038] The technical solutions of the embodiments of this application will now be described with reference to the accompanying drawings.

[0039] Please see Figure 1 Please see Figure 1 , Figure 1 This is a schematic diagram of an electrochromic device provided in an embodiment of this application. The electrochromic device includes an electrochromic film 100, two glass substrates, and two adhesive layers. The two glass substrates are a first glass substrate 111 and a second glass substrate 112. The two adhesive layers are a first adhesive layer 121 and a second adhesive layer 122. In the electrochromic device, the first glass substrate 111, the first adhesive layer 121, the electrochromic film 100, the second adhesive layer 122, and the second glass substrate 112 are sequentially stacked.

[0040] The first adhesive layer 121 is used to bond the first glass substrate 111 and the electrochromic film 100, and the second adhesive layer 122 is used to bond the electrochromic film 100 and the second glass substrate 112. For example, the first adhesive layer 121 and the second adhesive layer 122 can be polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), etc.

[0041] The electrochromic film 100 is bonded between the first glass substrate 111 and the second glass substrate 112 through two adhesive layers, which can improve the stability of the electrochromic film 100, protect it from the effects of water and oxygen that could cause the electrochromic device to fail, make the electrochromic device more stable, extend its service life, and make the electrochromic device more robust, so that it can be applied to automotive glass, architectural glass and other scenarios.

[0042] Figure 2 This is a cross-sectional schematic diagram of an electrochromic film 100 provided in an embodiment of this application, as shown below. Figure 1 As shown, the electrochromic film 100 involved in the various embodiments of this application includes a first substrate layer 1, a first conductive layer 2, an electrochromic layer 3, a second conductive layer 4, and a second substrate layer 5 stacked sequentially. The first substrate layer 1 and the second substrate layer 5 are "transparent substrates," which are made of optical-grade transparent materials, specifically flexible substrate materials such as PET (Polyester Film), cyclic olefin copolymers, or cellulose triacetate.

[0043] The first conductive layer 2 and the second conductive layer 4 are "transparent conductive layers". The materials of the transparent conductive layers can be indium-tin oxide (ITO), aluminum zinc oxide (AZO), fluorine-doped tin oxide (FTO), silver nanowires, graphene, carbon nanotubes, metal meshes or silver nanoparticles, etc.

[0044] The electrochromic layer 3 generally comprises an electrochromic material layer 31, an electrolyte layer 32, and an ion storage layer 33, stacked sequentially. The electrochromic material layer 31 contains an electrochromic material, and the ion storage layer 33 contains an ion storage material. The ion storage material stores ions, and the migration of ions from the ion storage material to or from the electrochromic material layer 31 can alter the transmittance of the electrochromic material layer 31. The electrolyte layer 32, also known as the ion transfer layer, serves as the ion transfer channel.

[0045] The first conductive layer 2 is electrically contacted with an external terminal via a first busbar thereon, and the second conductive layer 4 is electrically contacted with another external terminal via a second busbar thereon. Thus, by connecting a power source to the two external terminals, the voltage supplied by the power source is applied between the first conductive layer 2 and the second conductive layer 4, thereby changing the transmittance of the electrochromic device. The voltage causes ions to move between the electrochromic material layer 31 and the ion storage layer 33, and to intercalate / extract or deintercalate / intercalate between them, thereby changing the optical state of the electrochromic material in the electrochromic material layer 31, and consequently changing the transmittance of the electrochromic film 100, allowing the electrochromic film 100 to be adjusted between a colored state, an intermediate state, and a transparent state.

[0046] In the manufacturing process of electrochromic devices, a flexible electrochromic film is bonded to a glass substrate using an adhesive layer under high temperature and pressure. However, when the adhesive layer undergoes a cross-linking reaction due to thermal creep in the autoclave, its fluidity is affected by the temperature gradient, pressure distribution, and material interfacial adhesion, resulting in uneven stress distribution at the microscopic level. This uneven stress easily leads to unevenness in the adhesive layer, affecting its surface smoothness. Ultimately, this results in an orange peel-like or fish-scale-like texture on the surface of the finished electrochromic device, significantly reducing the appearance uniformity and optical smoothness of the device.

[0047] In the traditional lamination process of planar electrochromic devices, the lateral creep direction of the first adhesive layer 121 and the second adhesive layer 122 after thermal expansion is consistent, and the stress distribution is relatively controllable. However, in the manufacturing of curved devices such as automotive electrochromic glass, due to geometric reasons, contact pressure mismatch, and differences in thermal deformation of functional layers, the probability of orange peel texture defects is significantly increased, affecting the application of electrochromic devices on curved glass.

[0048] The electrochromic device prepared by the method provided in this application has no defects such as orange peel texture or stripes on its surface, has a good appearance, and expands the application range of electrochromic devices.

[0049] Please see Figure 3 , Figure 3 This is a flowchart illustrating the fabrication process of an electrochromic device according to an embodiment of this application. The fabrication method of this electrochromic device includes steps S1 and S2, as detailed below:

[0050] Step S1 involves providing an electrochromic film 100, two glass substrates (a first glass substrate 111 and a second glass substrate 112), and two adhesive layers (a first adhesive layer 121 and a second adhesive layer 122), forming a stack. In the stack, the electrochromic film 100 is located between the two glass substrates, and an adhesive layer is provided between each glass substrate and the electrochromic film 100. Specifically, the first glass substrate 111, the first adhesive layer 121, the electrochromic film 100, the second adhesive layer 122, and the second glass substrate 112 are sequentially stacked to form the stack.

[0051] Step S2: Heat the stack to a preset temperature and cool the stack to form the electrochromic device.

[0052] Among them, such as Figure 4 As shown in the temperature curve, the preset temperature is 15℃-30℃ higher than the melting temperature range of the adhesive layer. During the cooling process of the stack, the cooling rate of the stack within the glass transition temperature range of the adhesive layer is less than or equal to 1.5℃ / min.

[0053] The melting temperature range of the adhesive layer refers to the temperature range within which the viscosity of the adhesive layer significantly decreases during heating. For example, the adhesive layer can be PVB, whose melting temperature range is typically 120℃-130℃. Since the preset temperature is 15℃-30℃ higher than the melting temperature range of the adhesive layer, the preset temperature can be 135℃-160℃. To further reduce the risk of localized "cold spots" or "hot spots" in the adhesive layer and ensure complete melting, the preset temperature can be set to greater than or equal to 140℃. Additionally, PVB typically begins thermal decomposition at temperatures above 200℃. To reduce the risk of overheating and decomposition of PVB, the upper limit of the temperature during the heating process is strictly controlled to not exceed 160℃, i.e., the preset temperature is less than or equal to 160℃.

[0054] When the adhesive layer is PVB, the glass transition temperature of PVB is typically in the range of 50℃-70℃. Therefore, during the cooling process of the stack, the cooling rate of the stack within the 50℃-70℃ range is less than or equal to 1.5℃ / min. This can be understood as the instantaneous cooling rate of the stack within the 50℃-70℃ range being less than or equal to 1.5℃ / min, or the average cooling rate of the stack within the 50℃-70℃ range being less than or equal to 1.5℃ / min. Specifically, the cooling rate within the 50℃-70℃ range can be 1.4℃ / min, 1.3℃ / min, 1.2℃ / min, 1.1℃ / min, 1.0℃ / min, 0.9℃ / min, 0.8℃ / min, 0.7℃ / min, 0.6℃ / min, 0.5℃ / min, 0.4℃ / min, 0.3℃ / min, 0.2℃ / min, or 0.1℃ / min. In one embodiment, the stack may further include a heat-insulating platform in the range of 50°C to 70°C, and the cooling rate of the stack on the heat-insulating platform is 0°C / min.

[0055] In this embodiment, during the formation of the electrochromic device, the stacked body undergoes heating and cooling processes sequentially, such that the first glass substrate 111 and the electrochromic film 100 are bonded together by the first adhesive layer 121, and the electrochromic film 100 and the second glass substrate 112 are bonded together by the second adhesive layer 122. Specifically, the stacked body can be placed inside a heating device for heating and cooling. The heating device can be an autoclave.

[0056] In this embodiment, the temperature is controlled during the heating and cooling processes. During the heating process, the heating temperature of the stack is 15°C-30°C higher than the melting temperature of the adhesive layer, which allows the adhesive layer to melt fully, improves the fluidity of the adhesive layer, reduces the risk of unevenness and other defects on the surface of the adhesive layer due to incomplete melting in some areas, and improves the appearance and optical flatness of the electrochromic device.

[0057] Additionally, during the cooling process, the cooling rate of the stack within the glass transition temperature range of the adhesive layer is slowed down. The adhesive layer is typically composed of polymers, and the glass transition temperature is the critical temperature at which the adhesive layer transitions between a glassy (hard and brittle) and a highly elastic (soft and deformable) state. When the temperature is above the glass transition temperature range, the molecular chain segments in the adhesive layer are actively moving, and the adhesive layer material exhibits a highly elastic state and increased fluidity. Conversely, when the temperature is below the glass transition temperature range, the molecular chain segments in the adhesive layer are frozen, and the adhesive layer material enters the glassy state. If the cooling rate within the glass transition temperature range is too fast—that is, the adhesive layer cools rapidly from a molten state directly to below the glass transition temperature range—the internal thermal stress of the adhesive layer cannot be fully released, easily leading to stress concentration and surface unevenness, affecting the surface smoothness of the adhesive layer, and thus affecting the appearance of the electrochromic device.

[0058] In this embodiment, when the temperature of the stacked body drops to the glass transition temperature range of the adhesive layer, the cooling rate of the stacked body is slowed down, which is conducive to the slow relaxation of the molecular chain segments of the adhesive layer, reducing shrinkage differences and improving the surface flatness of the adhesive layer. This reduces or avoids defects such as orange peel texture in the electrochromic device, and the prepared electrochromic device has a good appearance.

[0059] In one embodiment, after step S1 and before step S2, the method for fabricating the electrochromic device further includes removing air from the stack. That is, removing the air between the first glass substrate 111, the first adhesive layer 121, the electrochromic film 100, the second adhesive layer 122, and the second glass substrate 112, so that each layer is tightly bonded.

[0060] In one embodiment, removing air from the stack body includes: providing a vacuum bag, placing the stack body inside the vacuum bag, and evacuating the vacuum bag to remove air from the stack body.

[0061] In one embodiment, removing air from the stack body includes: providing a collar, bonding the collar to the edge of the stack body such that the collar and the stack body together form a vacuum bag structure, and evacuating the vacuum bag structure to remove air from the stack body.

[0062] like Figure 4 As shown in the temperature curve, in one embodiment, during step S2, the stress relaxation temperature range of the adhesive layer of the stack includes the first insulation plateau. The stress relaxation temperature range of the adhesive layer is 10°C-20°C higher than the glass transition temperature range.

[0063] When the adhesive layer is PVB, if the glass transition temperature of PVB is in the range of 50℃-70℃, then the stress relaxation temperature range of the adhesive layer is 60℃-90℃.

[0064] During the cooling process of the stack, a first thermal plateau is set within the stress relaxation temperature range of the adhesive layer. That is, when the temperature of the stack drops to a specific temperature within the stress relaxation temperature range, the stack stops cooling down and instead maintains that specific temperature for a period of time (e.g., 20-30 minutes) before continuing to cool down. For example, when the stack cools down to 80°C, it is maintained at 80°C for 25 minutes before continuing to cool down.

[0065] The optimal temperature range for the molecular chain segments of the adhesive layer to release residual stress through thermal motion is usually within the stress relaxation temperature range. In this embodiment, a heat preservation platform is set in a temperature range slightly higher than the glass transition temperature range of the adhesive layer during the cooling process. This allows the adhesive layer to fully release residual stress, and the molecular chain segments of the adhesive layer to relax slowly. This helps to reduce the shrinkage difference of the adhesive layer during the cooling process, improve the surface smoothness of the adhesive layer, thereby reducing or avoiding defects such as orange peel texture in the electrochromic device. The prepared electrochromic device has a good appearance.

[0066] In one embodiment, during step S2, the cooling rate of the stack within the stress relaxation temperature range of the adhesive layer is less than or equal to 2°C / min during the cooling process of the stack. In this embodiment, slowing down the cooling rate of the stack within the stress relaxation temperature range allows the adhesive layer to fully release residual stress, and the molecular chain segments of the adhesive layer relax slowly. This helps reduce the shrinkage differences of the adhesive layer during cooling, improves the surface smoothness of the adhesive layer, and thus reduces or avoids defects such as orange peel texture in the electrochromic device, resulting in an electrochromic device with a good appearance.

[0067] In one embodiment, in step S2, during the cooling of the stack, the cooling rate of the stack within the stress relaxation temperature range of the adhesive layer is greater than the cooling rate within the glass transition temperature range of the adhesive layer. In this embodiment, the stack passes through both the stress relaxation temperature range and the glass transition temperature range sequentially, thus reducing the cooling rate of the stack. Compared to the glass transition temperature range, the cooling rate within the stress relaxation temperature range is faster, which helps to shorten the overall cooling time of the stack. Maintaining a low cooling rate in both the stress relaxation temperature range and the glass transition temperature range, and an even lower cooling rate within the glass transition temperature range, allows the adhesive layer to fully release residual stress, which helps to reduce the shrinkage difference of the adhesive layer during cooling and improve the surface smoothness of the adhesive layer.

[0068] In one embodiment, during the heating of the stack to a preset temperature, the heating rate of the stack within the melting temperature range is less than or equal to 2°C / min. In this embodiment, during the heating process, the heating rate is reduced in the melting stage to ensure uniform temperature coverage of the viscous flow region. This reduces the risk of unevenness and other defects on the adhesive layer surface due to localized unmelted or degraded areas, thereby improving the appearance and optical smoothness of the electrochromic device.

[0069] like Figure 4 As shown in the temperature curve, in one embodiment, the stack includes a second heat-preserving platform before being heated to the melting temperature range. During the heating of the stack, a first heat-preserving platform is provided before the melting temperature range of the adhesive layer. That is, when the temperature of the stack rises to a specific temperature before the melting temperature range, the heating temperature of the stack is not increased further, but rather maintained at that specific temperature for a period of time (e.g., 20-30 minutes) before further heating. For example, when the stack is heated to 80°C, it is held at 80°C for 25 minutes before the temperature is further increased.

[0070] In this embodiment, the stack is kept at a certain temperature for a period of time before melting to ensure a more uniform temperature distribution of the adhesive layer. During the melting stage, to avoid uneven melting of different parts of the adhesive layer due to temperature variations, the different parts of the adhesive layer in this application can melt simultaneously, which helps improve the flatness of the adhesive layer in the electrochromic device.

[0071] In one embodiment, heating the stack to a preset temperature includes: heating the stack to the preset temperature and maintaining the preset temperature for a first preset duration. In this embodiment, maintaining the stack at the preset temperature for a first preset duration is beneficial for the adhesive layer to fully melt.

[0072] In one embodiment, before forming the electrochromic device, the fabrication method further includes pressurizing the stack, wherein the pressure applied to the stack before heating it to a preset temperature is less than or equal to 0.3 MPa. In this embodiment, by not directly applying a large pressure before the stack reaches its maximum temperature, it is possible to ensure uniform stress on the stack. Subsequent annealing and aging of the stack can improve the pressure resistance of the electrochromic device.

[0073] In one embodiment, the stack can be pressurized after heating but before reaching a preset temperature. Specifically, after heating the stack begins, a small pressure (e.g., less than or equal to 0.3 MPa) is applied to the stack initially, and the pressure is increased once the temperature of the stack rises to the preset temperature.

[0074] like Figure 4As shown in the temperature and pressure curves, in one embodiment, the method for fabricating an electrochromic device includes: pressurizing the stacked body for a first preset time period. In this embodiment, the stacked body is also subjected to pressurization during a preheating stage at a preset temperature. The pressurization process can remove air bubbles between the layers of the stacked body and ensure good bonding between the adhesive layer and the glass substrate, and between the adhesive layer and the electrochromic film.

[0075] like Figure 4 As shown in the temperature and pressure curves, in one embodiment, the stack is pressurized within a first preset time period, including: maintaining a preset temperature to a second preset time period, increasing the pressure applied to the stack, and maintaining the preset temperature to a third preset time period while increasing the pressure of the stack to a preset pressure. The second, third, and first preset time periods increase sequentially. Those skilled in the art can set specific values ​​for each preset time period according to actual conditions. For example, the second preset time period is 10-25 minutes (specifically, 15 minutes, 17 minutes, etc.), the third preset time period is 30-40 minutes (specifically, 35 minutes, 37 minutes, etc.), and the first preset time period is 60-75 minutes (specifically, 65 minutes, 67 minutes, etc.).

[0076] The preset pressure is greater than or equal to 0.8 MPa. In one embodiment, the preset pressure can be 0.9 MPa, 1 MPa, 1.1 MPa, or 1.2 MPa.

[0077] The stack comprises a first stage, a second stage, and a third stage sequentially within a first preset duration. The duration of the first stage is the second preset duration, and the total duration of the first and second stages is the third preset duration. During the second stage, the pressure applied to the stack is increased, and after the second stage ends and the third stage begins, the stack is pressurized to the preset pressure.

[0078] In one embodiment, pressurizing the stack during a first preset time period further includes: applying a pressure to the stack of less than or equal to 0.3 MPa during a second preset time period. That is, a relatively low pressure is applied to the stack of less than or equal to 0.3 MPa during the first stage. Exemplarily, the average pressure applied to the stack of less than or equal to 0.3 MPa during the first stage, or a preset low pressure is applied to the stack of less than or equal to 0.3 MPa during the first stage, i.e., a pressure-holding plateau exists.

[0079] In one embodiment, pressurizing the stack during a first preset time period further includes: a pressurization rate of less than 0.01 MPa / min during a second preset time period. That is, during the first stage, the stack has a relatively small pressurization rate, such as... Figure 4As shown, during the first stage, the pressure ramp rate of the stack is 0 MPa / min. In one embodiment, prior to the first stage, the pressure ramp rate of the stack is less than or equal to 5 kPa / min.

[0080] In one embodiment, pressurizing the stack within a first preset time period further includes: the pressurization rate of the stack within a second preset time period is less than the pressurization rate of the stack within a third preset time period after the second preset time period. That is, the pressurization rate of the stack in the first stage is less than the pressurization rate in the second stage.

[0081] In one embodiment, the stack is maintained at a preset pressure in the third stage. Applying a preset pressure to the stack and maintaining it for a period of time helps to remove air bubbles between the stack layers and ensures good bonding between the adhesive layer and the glass substrate, and between the adhesive layer and the electrochromic film.

[0082] In this embodiment, the stack may be heated unevenly during the heating process. In the first stage of heating the stack to the preset temperature, a small pressure is applied to the stack or the pressure increase rate of the stack is slowed down. After the first stage of heat preservation, the overall temperature distribution of the stack is more uniform. At this time (in the second stage), the pressure applied to the stack is increased again to ensure that the stack is subjected to uniform force, and the resulting electrochromic device has a better appearance.

[0083] In one embodiment, after pressurizing the stack and before forming the electrochromic device, the method for fabricating the electrochromic device further includes: depressurizing the stack. During the depressurization process, the pressure applied to the stack is reduced from a preset pressure to 0, meaning the stack is at atmospheric pressure after the depressurization process.

[0084] In one embodiment, the depressurization process and cooling of the stack are initiated simultaneously. That is, the stack is simultaneously cooled and depressurized while at a preset temperature and preset pressure.

[0085] If the temperature is lowered before the pressure is reduced, the adhesive layer will solidify under high pressure. In reality, the pressure in the adhesive layer is unstable, which can easily lead to uneven stress and thus aggravate the orange peel texture.

[0086] If the pressure is reduced before the temperature is lowered, the following problems may occur: First, at high temperatures, the adhesive layer has good fluidity. If the pressure is reduced first, the adhesive layer may not be able to evenly fill the gaps between the glass panes due to the reduced fluidity, resulting in uneven interlayer thickness and affecting the transparency and strength of the glass. Furthermore, the glass substrate has a high coefficient of thermal expansion at high temperatures; if the pressure is reduced first, the glass substrate may crack during the cooling process due to uneven internal stress.

[0087] Secondly, a decrease in pressure can cause gas to become trapped between the adhesive layer and the glass substrate, forming bubbles or voids. This not only affects the appearance of the electrochromic device but may also reduce its durability and safety. Furthermore, it can lead to inadequate sealing between the glass substrate and the adhesive layer, and between the adhesive layer and the electrochromic film, affecting the waterproof and soundproofing performance of the electrochromic device.

[0088] In addition, the molecular chains of the adhesive layer are relatively loose at high temperatures. If the pressure is reduced first and then the temperature is reduced, the molecular chains of the adhesive layer may not be able to rearrange well, resulting in a decrease in bonding performance and affecting the overall strength and durability of the electrochromic device.

[0089] Therefore, in this embodiment, the stack is gradually depressurized during the cooling process to ensure good bonding between the adhesive layer and the glass substrate and the electrochromic film, thereby ensuring the quality, performance and good appearance of the electrochromic device.

[0090] During the cooling process of the stack and before the stack cools to the cold flow temperature range of the adhesive layer, the pressure applied to the stack is reduced to less than or equal to 0.15 MPa, and the cold flow temperature range of the adhesive layer is 15°C-25°C lower than the glass transition temperature range. For example, when the glass transition temperature range of the adhesive layer is in the range of 50°C-70°C, the cold flow temperature range of the adhesive layer is 25°C-55°C; in one embodiment, the cold flow temperature range of the adhesive layer is 30°C-50°C.

[0091] If the external pressure is not fully released when the stack cools to the cold flow temperature, the adhesive layer may undergo local deformation (such as "creep") due to viscoelastic flow, resulting in surface wrinkles. In the embodiments of this application, the stack is gradually depressurized before cooling to the cold flow temperature, which can reduce the risk of secondary flow caused by residual pressure and is beneficial to improving the surface smoothness of the adhesive layer in the electrochromic device.

[0092] In one embodiment, during the cooling process of the stack, the cold flow temperature range of the stack in the adhesive layer includes a third thermal plateau. The third thermal plateau refers to a point where, after the temperature of the stack cools to a certain temperature, the temperature is not further reduced, but rather maintained at that specific temperature for a period of time (e.g., 10-20 minutes) before further cooling. For example, when the stack cools to 50°C, it is maintained at 50°C for a period of time (e.g., 15 minutes).

[0093] In one embodiment, during the cooling of the stack, the cooling rate of the stack within the cold flow temperature range of the adhesive layer is less than or equal to 0.35°C / min.

[0094] In this embodiment, during the cooling stage, a heat-insulating platform is set up within the cold flow temperature range to release stress or reduce the cooling rate, ensuring uniform temperature and improving the smoothness of the adhesive layer.

[0095] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application.

Claims

1. A method for preparing an electrochromic device, characterized in that, include: An electrochromic film, two glass substrates and two adhesive layers are provided and formed into a stack, wherein the electrochromic film is located between the two glass substrates and an adhesive layer is provided between each glass substrate and the electrochromic film. The stack is heated to a preset temperature and then cooled to form the electrochromic device. The preset temperature is 15°C-30°C higher than the melting temperature range of the adhesive layer, and the cooling rate of the stack within the glass transition temperature range of the adhesive layer during the cooling process is less than or equal to 1.5°C / min.

2. The method for preparing the electrochromic device according to claim 1, characterized in that, During the cooling process of the stack, the stress relaxation temperature range of the adhesive layer includes the first insulation plateau, or the cooling rate of the stack within the stress relaxation temperature range of the adhesive layer is less than or equal to 2°C / min and greater than the cooling rate of the stack within the glass transition temperature range of the adhesive layer; wherein the stress relaxation temperature range of the adhesive layer is 10°C-20°C higher than the glass transition temperature range.

3. The method for preparing the electrochromic device according to claim 1, characterized in that, During the heating of the stack to a preset temperature, the heating rate of the stack within the melting temperature range is less than or equal to 2°C / min; or the stack includes a second heat-preserving platform before being heated to the melting temperature range.

4. The method for preparing the electrochromic device according to claim 1, characterized in that, Before forming the electrochromic device, the method for preparing the electrochromic device further includes: pressurizing the stack, wherein the pressure applied to the stack before heating it to the preset temperature is less than or equal to 0.3 MPa.

5. The method for preparing the electrochromic device according to claim 4, characterized in that, Heating the stack to a preset temperature includes: heating the stack to a preset temperature and maintaining the preset temperature for a first preset duration; Within the first preset time period, the stack is pressurized.

6. The method for preparing the electrochromic device according to claim 5, characterized in that, Within the first preset duration, the stack is pressurized, including: maintaining the preset temperature to the second preset duration, increasing the pressure applied to the stack, and maintaining the preset temperature to the third preset duration while the stack is pressurized to the preset pressure, wherein the second preset duration, the third preset duration and the first preset duration increase sequentially, and the preset pressure is greater than or equal to 0.8 MPa.

7. The method for preparing the electrochromic device according to claim 6, characterized in that, Within the first preset time period, pressurizing the stack further includes: within the second preset time period, applying a pressure to the stack that is less than or equal to 0.3 MPa, and / or Within the second preset time period, the pressure increase rate of the stack is less than 0.01 MPa / min, and / or The rate of increase of the stack within the second preset time period is less than the rate of increase of the stack within the third preset time period after the second preset time period.

8. The method for preparing the electrochromic device according to claim 4, characterized in that, After pressurizing the stacked body and before forming the electrochromic device, the method for fabricating the electrochromic device further includes: depressurizing the stacked body, wherein: During the cooling of the stack and before the stack cools to the cold flow temperature range of the adhesive layer, the pressure applied to the stack is reduced to less than or equal to 0.15 MPa, and the cold flow temperature range of the adhesive layer is 15°C-25°C lower than the glass transition temperature range.

9. The method for preparing the electrochromic device according to claim 8, characterized in that, During the cooling process of the stack, the cold flow temperature range of the stack in the adhesive layer includes a third insulation platform, or the cooling rate of the stack in the cold flow temperature range of the adhesive layer is less than or equal to 0.35°C / min.

10. An electrochromic device, characterized in that, The electrochromic device is prepared using the method for preparing an electrochromic device as described in any one of claims 1-9.